A difficult-to-form composite liquid-absorbing core and its preparation method

By using electron beam selective melting technology to control melting or sintering in different regions, the manufacturing challenge of combined wicking elements under extreme aerodynamic thermal environments has been solved, enabling high-precision integrated forming of difficult-to-form alloy ultra-high temperature heat pipes and improving the heat transfer performance and fatigue resistance of the heat pipes.

CN117680707BActive Publication Date: 2026-11-17BEIJING HANGXING MACHINERY MFG CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311802984.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2026-11-17
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

Existing processing techniques are insufficient for efficiently manufacturing complex composite liquid wicks under extreme aerodynamic heating conditions, and difficult-to-form alloys are prone to cracking during laser additive manufacturing, failing to meet the forming requirements of ultra-high temperature heat pipes.

Method used

Electron beam selective melting (EBSM) technology is used to control process parameters and scanning strategies to melt or sinter in different regions, thereby achieving the integrated forming of groove structures and porous powder material layers and preparing difficult-to-form alloy composite liquid wicking cores.

Benefits of technology

It achieves high-precision integrated molding of complex structure combination liquid wicks, avoids the airtightness problem caused by welding, is suitable for ultra-high temperature heat pipe manufacturing, provides large capillary force and small backflow resistance, and improves the heat transfer performance of heat pipes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117680707B_ABST
    Figure CN117680707B_ABST
Patent Text Reader

Abstract

This invention relates to a method for fabricating difficult-to-form composite wicking cores using electron beam additive manufacturing, belonging to the field of additive manufacturing technology for heat pipe components. It solves the problems of low processing accuracy, slow efficiency, or unsuitability for extreme aerodynamic and thermal environments in existing processing techniques. The method includes the following steps: S1, equipment and raw material preparation; S2, model design; S3, EBSM additive manufacturing; S4, heat treatment and machining. This method enables the integrated forming and on-demand construction of complex geometric shapes and ultra-high temperature composite wicking cores.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of additive manufacturing technology for heat pipe components, and in particular to a method for preparing a difficult-to-form composite liquid wick using electron beam additive manufacturing and the difficult-to-form composite liquid wick. Background Technology

[0002] High-speed aircraft generate extremely high temperatures due to air stagnation and surface friction, with windward temperatures exceeding 2000°C. This extreme aerodynamic thermal environment poses a significant challenge to the safe operation of high-speed aircraft. Heat pipe protection, with its advantages of high thermal protection capability and reusability, has become one of the most promising thermal protection technologies for next-generation aircraft. In the severely heated area, heat is absorbed by the heat pipe and vaporized into a working fluid. Under the influence of internal pressure difference, the working fluid flows to the cold end, condenses, and releases heat. The condensed working fluid then returns to the severely heated area along the pipe wall under the capillary action of the wick, forming a cycle of flow and heat transfer.

[0003] The wick is a crucial component of a heat pipe, typically composed of porous materials with a capillary structure, and determines the heat transfer performance of the heat pipe. To ensure the heat pipe functions properly under various service environments, the wick must provide sufficiently high capillary pull and sufficiently low flow resistance to overcome the effects of gravity and reduce the flow resistance of the working fluid within the heat pipe. Simultaneously, the wick must reduce the radial thermal resistance of the heat pipe, improve its temperature uniformity, and increase its maximum tolerable heat flux density, thereby enhancing the heat transfer performance. Depending on the structural type, wicks are mainly classified into single-structure wicks such as powder sintered, fiber sintered, wire mesh, and grooved wicks. However, these single-structure wicks generally struggle to simultaneously meet the requirements of small capillary pore size, high porosity, and enhanced heat transfer. Therefore, composite wicks have become a research focus in this field in recent years, addressing the challenge of simultaneously achieving high capillary pull and low flow resistance. Related studies have shown that heat pipes using composite wicks exhibit significantly better heat transfer performance than heat pipes with single-structure wicks.

[0004] Compared to single-structure liquid-absorbing cores, composite liquid-absorbing cores have a more complex internal structure, resulting in an exceptionally cumbersome manufacturing process that often involves multiple processing techniques. This significantly increases the process risk of tandem manufacturing techniques. Furthermore, aircraft windward components typically have complex and irregular geometric shapes, making tandem manufacturing processes unsuitable for the on-demand construction of such complex windward components.

[0005] As aircraft speeds continue to increase, the demand for ultra-high temperature materials for their windward components is becoming increasingly urgent. Refractory metals (such as tungsten and molybdenum), high-temperature high-entropy alloys, and cast high-temperature alloys have become candidate materials for the main structure of windward components in next-generation high-speed aircraft. However, due to their unique physical properties, difficult-to-form alloys are prone to cracking during laser additive manufacturing. Furthermore, ultra-high temperature heat pipes operate in a high-vacuum environment, therefore current laser additive manufacturing methods cannot meet the forming requirements of difficult-to-form alloy heat pipes.

[0006] To overcome the above problems and improve the ultra-high temperature thermal protection capability of the next generation of aircraft, it is urgent to propose a new electron beam additive manufacturing method for difficult-to-form alloy composite liquid absorber cores with high forming accuracy and degree of freedom and excellent performance. This method can not only realize the integrated forming of composite liquid absorber cores and overcome the technical and process difficulties brought about by serial processes, but also fill the gap in ultra-high temperature materials for ultra-high temperature heat pipe protection. Summary of the Invention

[0007] Based on the above analysis, the present invention aims to provide an electron beam additive manufacturing method for difficult-to-form composite liquid wicking cores, in order to solve the problems of low processing accuracy, slow efficiency or unsuitability for extreme aerodynamic and thermal environments in existing processing technologies, while enabling the on-demand construction of composite liquid wicking cores with complex geometries.

[0008] On one hand, embodiments of the present invention provide a method for electron beam additive manufacturing of a difficult-to-form composite liquid-absorbing core, comprising the following steps:

[0009] S1. Equipment and raw material preparation;

[0010] S2. Model Design: Use modeling software to design a combined liquid absorption core model, including a groove structure and a layer of porous powder material;

[0011] S3. Additive manufacturing: Based on the combined liquid suction core model determined in step S2, the combined liquid suction core additive blank is integrally formed by controlling process parameters and scanning strategy.

[0012] S4. Heat treatment and machining: The combined liquid-absorbing core additive blank obtained in step S3 is processed sequentially to obtain the combined liquid-absorbing core sample.

[0013] Furthermore, the additive manufacturing described in step S3 employs the EBSM process, specifically including the following steps:

[0014] S301. Based on the structural characteristics of the combined absorbent core model, the model is split into two parts: a groove structure and a powder porous material layer. The groove structure and the powder porous material layer are sliced ​​to form a combined absorbent core additive model.

[0015] S302. Spread a layer of powder raw material evenly on the substrate. Set different process parameters and scanning strategies according to the two regions divided in step S301. Melt or sinter the powder according to the region to achieve the densification of the trench structure and the sintering of the surface powder material.

[0016] S303. After the first layer of powder is formed, powder is spread on the basis of the first layer, and the process of step S302 is repeated until a combined liquid-absorbing core additive blank that meets the design of the combined liquid-absorbing core model in step S2 is obtained.

[0017] Further, step S1 includes: firstly, vacuum low-temperature drying treatment of the difficult-to-form alloy powder, then loading the treated powder raw material into an electron beam selective melting equipment, selecting a metal plate suitable for the powder raw material as the forming substrate, debugging the EBSM equipment, and completing the preparation of additive manufacturing equipment and raw materials.

[0018] For example, the difficult-to-form alloy mentioned in step S1 is one of the following: refractory metals W and Mo, casting high-temperature alloy Mar-M247, easily cracked titanium alloy Ta15, high-temperature high-entropy alloy, or pure copper.

[0019] Specifically, the particle size of the difficult-to-form alloy powder is 53μm to 105μm.

[0020] On the other hand, embodiments of the present invention provide a difficult-to-form composite liquid-absorbing core, which is prepared by the electron beam additive manufacturing method for the difficult-to-form composite liquid-absorbing core.

[0021] Specifically, the combined liquid-absorbing core comprises two parts: a groove structure and a layer of porous powder material.

[0022] Furthermore, the groove structure includes a substrate and fins disposed thereon, with grooves formed between the fins. The fin thickness is 0.2-0.3 mm, the fin spacing is 0.1-0.2 mm, and the groove depth is 0.3-0.8 mm.

[0023] Furthermore, the porous powder material layer is formed above the trench structure;

[0024] Specifically, the porous powder material layer has a pore size of 0.04-0.1 mm and a thickness of 1-3 mm.

[0025] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0026] 1. The method for preparing the combined liquid wick provided by the present invention utilizes the process characteristics of high-temperature sintering and selective melting of EBSM technology, which is suitable for the engineering manufacturing of ultra-high temperature components with complex structures, meets the requirements of integrated forming of the combined liquid wick, and effectively avoids the airtightness problem caused by preparing the combined liquid wick through welding and other processes, that is, the oxidation or leakage of the cooling medium.

[0027] 2. The preheating temperature during the forming process of the combined wicking core EBSM of the present invention can reach up to 1100℃. It is used to manufacture refractory metals such as W and Mo, casting high-temperature alloys such as Mar-M247, easily cracked titanium alloys such as TA15, high-temperature high-entropy alloys and pure copper combined wicking cores and their heat pipes. It realizes low-stress forming of difficult-to-form alloys and solves the problem of defect-free manufacturing of ultra-high temperature heat pipe body materials.

[0028] In addition, this invention can prepare ultra-high temperature components of difficult-to-form alloys with combined liquid-absorbing cores. With the high melting point and high hardness of difficult-to-form alloys, they have become one of the best solutions for extreme thermal protection of the windward surface components of the next generation of high-speed aircraft.

[0029] 3. The electron beam additive manufacturing method for difficult-to-form composite liquid-absorbing cores provided by the present invention can realize the metallurgical bond between the difficult-to-form alloy grooves and the powder sintering structure through an integrated molding method, and has better high-temperature mechanical properties and fatigue resistance.

[0030] 4. The combined wicking core of the present invention is formed by EBSM. Different process parameters and scanning strategies are set for different regions according to the two parts: the groove structure and the porous powder material layer. The powder is melted or sintered according to the region to achieve the densification of the groove structure and the sintering of the surface powder material. This achieves the integral molding of the combined wicking core, which takes into account both large capillary force and small backflow resistance, and is conducive to reducing the radial thermal resistance of the heat pipe and improving the overall heat transfer performance of the heat pipe.

[0031] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description

[0032] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.

[0033] Figure 1 This is a schematic diagram of the overall structure and working principle of an ultra-high temperature heat pipe;

[0034] Figure 2Flowchart of electron beam additive manufacturing process for combined liquid suction core;

[0035] Figure 3 This is a schematic diagram of the combined suction core structure;

[0036] Figure 4 This is a picture of the assembled absorbent core.

[0037] Figure label:

[0038] 1-Powder sintered layer; 2-Groove; 3-Inner wall of combined liquid suction core; 4-Coolant reflux; 5-Combined liquid suction core; 6-Evaporation end; 7-Condensation end. Detailed Implementation

[0039] Preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which form part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.

[0040] In one specific embodiment of the present invention, a method for fabricating a difficult-to-form composite liquid-absorbing core using electron beam additive manufacturing is disclosed, comprising the following steps:

[0041] S1. Equipment and raw material preparation: First, the difficult-to-form alloy powder is vacuum-dried at low temperature, and the processed powder raw material is loaded into the electron beam selective melting equipment. A metal plate suitable for the powder raw material is selected as the forming substrate. The EBSM equipment is debugged to complete the preparation of additive manufacturing equipment and raw materials.

[0042] S2. Model Design: Design a composite absorbent core model using commercial modeling software, including a groove structure and a layer of porous powder material on top of it.

[0043] S3. Additive manufacturing: Based on the combined liquid suction core model determined in step S2, the combined liquid suction core additive blank is integrally formed by controlling process parameters and scanning strategy.

[0044] S4. Heat treatment and machining: The composite liquid-absorbing core additive blank obtained in step S3 is sequentially subjected to powder cleaning, stress-relieving annealing, wire cutting and heat treatment processes to obtain the composite liquid-absorbing core sample.

[0045] S5. Quality Inspection: Non-destructive testing and performance testing are performed on the liquid absorption core sample to determine the groove and porous material structure, surface quality and capillary properties, and to obtain the combined liquid absorption core component.

[0046] In one possible design, step S1 involves using a vacuum drying device to perform low-temperature vacuum drying on the difficult-to-form alloy powder, with a vacuum degree of 5–10 × 10⁻⁶. -1Torr, keep at a low temperature of 120-150℃ for 1-2 hours to dry; improve powder flowability, which is beneficial to improve the quality of additive products.

[0047] Furthermore, in step S1, the EBSM device is debugged to maintain a vacuum level of 10. -1 Pa.

[0048] In one possible design, the vacuum low-temperature drying process in step S1 is performed at 5–10 °C. -1 Under Torr vacuum, heat to 120-150℃ and maintain for 1-2 hours.

[0049] For example, the difficult-to-form alloy mentioned in step S1 is one of the following: refractory metals W, Mo, casting high-temperature alloy Mar-M247, easily cracked titanium alloy Ta15, high-temperature high-entropy alloy or pure copper.

[0050] It is worth noting that the aforementioned difficult-to-form alloys are suitable for ultra-high temperature heat pipes or ultra-high temperature components, but these metals are unsuitable for laser powder bed additive manufacturing due to the susceptibility to defects such as cracks during laser additive manufacturing. In contrast, the high preheating temperature of electron beam selective additive manufacturing helps suppress crack formation, making it particularly suitable for additive manufacturing of such difficult-to-form alloys. However, electron beam selective additive manufacturing involves numerous process control parameters, including substrate preheating, powder bed preheating, filling, sintering, and scanning processes. Problems in any of these stages can lead to additive components failing to meet production requirements. Furthermore, electron beam selective additive manufacturing equipment requires a high vacuum environment, placing higher demands on the operating environment and maintenance. These two factors limit the application of electron beam selective additive manufacturing for complex structures made of difficult-to-form alloys.

[0051] Specifically, the particle size of the difficult-to-form alloy powder is 53μm to 105μm.

[0052] In one possible design, in step S2, the groove structure includes a substrate and fins disposed thereon, with grooves formed between the fins. The fin thickness is 0.2-0.3 mm, the fin spacing is 0.1-0.2 mm, and the groove depth is 0.3-0.8 mm. The porous powder material layer has a pore size of 0.04-0.1 mm and a coating thickness of 1-3 mm.

[0053] Furthermore, the additive manufacturing described in step S3 employs the EBSM process, specifically including the following steps:

[0054] S301. Based on the structural characteristics of the combined absorbent core model, the model is divided into two parts, a groove structure and a powder porous material layer, using MAGICS software. The groove structure and the powder porous material layer are sliced ​​to form a combined absorbent core additive model.

[0055] S302. A layer of powder raw material is evenly spread on the substrate. According to the trench structure and porous powder material layer divided in step S301, the corresponding process parameters and scanning strategies are set respectively. The powder in the two regions is selectively melted or sintered to achieve the densification of the trench structure and the sintering of the surface powder material.

[0056] S303. After the first layer of powder is formed, powder is spread on the basis of the first layer, and the process of step S302 is repeated until a combined liquid-absorbing core additive blank that meets the design of the combined liquid-absorbing core model in step S2 is obtained.

[0057] It should be noted that the substrate is preheated before spreading the powder raw materials in steps S302 and S303. This is to ensure the heat storage capacity of the powder bed and improve the temperature field stability of the initial layer. After the powder is spread, the powder is preheated by electron beam defocusing heating to achieve slight sintering of the powder, so that the powder has better thermal conductivity, electrical conductivity and mechanical stability, which helps to prevent preparation failure caused by powder scattering. The thickness of each layer of the powder raw materials is 40-50 μm.

[0058] The powder is melted or sintered by region, and then connected by high-temperature solid-state diffusion sintering with electron beam preheating, resulting in high metallurgical strength and giving the combined liquid absorbing core good high-temperature mechanical properties and fatigue resistance. The trench structure is made by selective electron beam melting, which can obtain dense material. The porous powder material layer is made by selective electron beam sintering, which sintersects the powder material into shape to form a porous powder material layer. The selective melting and selective sintering processes are achieved by controlling parameters such as electron beam focusing or defocusing, beam energy, and scanning speed after the substrate and powder material reach the preheating temperature. The specific process parameters are obtained through experiments based on different materials. Steps S302 and S303 are continuous operations to achieve the integral forming of the trench structure and the porous material layer.

[0059] In one possible design, for pure tungsten material, the substrate is preheated before spreading the powder raw material in step S302. The preheating temperature is 1100℃, and the preheating time is approximately 20-30 minutes. After powder spreading, the powder is preheated using electron beam defocusing heating at a temperature of 900-1100℃. The process parameters for electron beam defocusing heating are: beam current 25-35mA, scanning speed 18-21m / s, powder thickness 50μm, and high-speed reciprocating scanning. The process parameters for selective electron beam melting of the trench structure are: beam current 15-20mA, scanning speed 0.5-1.0m / s, powder thickness 50μm, and slow reciprocating scanning. The process parameters for electron beam sintering of the porous material layer are: beam current 25-35mA, scanning speed 5-10m / s, powder thickness 50μm, and high-speed reciprocating scanning.

[0060] In one possible design, for the M247 nickel-based superalloy, the substrate is preheated before spreading the powder raw material in step S302. The preheating temperature is 1100℃, and the preheating time is approximately 20-30 minutes. After powder spreading, the powder is preheated using electron beam defocusing heating at a temperature of 900-1100℃. The process parameters for electron beam defocusing heating to achieve this preheating temperature are: beam current 17-33mA, scanning speed 18-21m / s, powder thickness 50μm, and high-speed reciprocating scanning strategy. The process parameters for selective electron beam melting of the trench structure are: beam current 1-10mA, scanning speed 0.4-5.0m / s, powder thickness 50μm, and slow reciprocating scanning strategy. The process parameters for electron beam sintering of the porous material layer are: beam current 17-33mA, scanning speed 10-15m / s, powder thickness 50μm, and high-speed reciprocating scanning strategy.

[0061] In one possible design, for TA15 titanium alloy, the substrate is preheated before spreading the powder raw material in step S302. The preheating temperature is 600℃, and the preheating time is approximately 20-30 minutes. After powder spreading, the powder is preheated using electron beam defocusing heating at a temperature of 500-600℃. The process parameters for electron beam defocusing heating are: beam current 25-30mA, scanning speed 27-55m / s, powder thickness 40μm, and high-speed reciprocating scanning. The process parameters for selective electron beam melting of the trench structure are: beam current 6-20mA, scanning speed 0.7-2.4m / s, powder thickness 40μm, and slow reciprocating scanning. The process parameters for electron beam sintering of the porous material layer are: beam current 25-30mA, scanning speed 15-30m / s, powder thickness 40μm, and high-speed reciprocating scanning.

[0062] Furthermore, the powder cleaning in step S4 involves using a powder cleaning device and high-pressure gas to remove excess metal powder from the grooves of the combined liquid suction core blank.

[0063] Optionally, stress-relief annealing can be used to eliminate internal stress during additive manufacturing and prevent deformation of components after wire cutting.

[0064] The combined liquid-absorbing core component is separated from the substrate by wire cutting after annealing.

[0065] Optionally, the performance of the combined liquid-absorbing core component can be controlled through a heat treatment process.

[0066] In one possible design, for pure tungsten material, after powder cleaning in step S4, stress-relief annealing is performed. Process parameters include: vacuum heat treatment furnace, vacuum environment (5~10×10⁻⁶). -1Torr), 1200℃, held for 3 hours; the combined liquid-absorbing core component is obtained by separating it from the substrate through wire cutting process.

[0067] In one possible design, for M247 nickel-based superalloy, after cleaning the powder in step S4, the alloy is separated from the substrate by wire cutting. After separation, it undergoes heat treatment with the following process parameters: solution treatment at 1150-1200℃ for 4 hours, air cooling, aging treatment at 900-1000℃ for 4 hours, and air cooling; thus obtaining the combined liquid wick component.

[0068] In one possible design, for TA15 titanium alloy, after powder cleaning in step S4, stress-relief annealing is performed, with the following process parameters: vacuum heat treatment furnace, vacuum environment (5~10×10). -1 Torr), 500℃, hold for 2 hours; separate from the substrate by wire cutting process; after separation, perform heat treatment with the following process parameters: heat to 850℃, hold for 2-4 hours, and then air cool.

[0069] Furthermore, the combined liquid-absorbing core sample obtained in step S4 is subjected to non-destructive testing using X-rays or three-dimensional scanning; and after capillary force testing, it meets the usage requirements.

[0070] Furthermore, the combined wicking core component is used in hard-to-form alloy ultra-high temperature heat pipes or ultra-high temperature components; the combined wicking core provides greater capillary force through a sintered powder porous material layer, and has smaller backflow resistance when combined with the groove structure; it can enable the working medium in the ultra-high temperature heat pipe or ultra-high temperature component to achieve anti-gravity transport.

[0071] On the other hand, embodiments of the present invention provide a difficult-to-form composite liquid-absorbing core, which is prepared by the electron beam additive manufacturing method for the difficult-to-form composite liquid-absorbing core.

[0072] Specifically, the combined liquid-absorbing core comprises two parts: a groove structure and a layer of porous powder material.

[0073] Furthermore, the groove structure includes a substrate and fins disposed thereon, with grooves formed between the fins. The fin thickness is 0.2-0.3 mm, the fin spacing is 0.1-0.2 mm, and the groove depth is 0.3-0.8 mm.

[0074] Furthermore, the sintered powder porous material layer is formed above the trench structure;

[0075] Specifically, the sintered powder porous material layer has a pore size of 0.04-0.1 mm and a thickness of 1-3 mm.

[0076] The following specific embodiments illustrate the application of the electron beam additive manufacturing method for difficult-to-form composite liquid-absorbing cores of the present invention in ultra-high temperature heat pipes.

[0077] Example 1

[0078] This invention utilizes the electron beam selective melting (EBSM) technique to prepare a new generation of pure tungsten composite wicking core for thermal protection of ultra-high temperature heat pipes, such as... Figure 1 As shown, it is suitable for ultra-high temperature environments above 1500℃.

[0079] This composite absorbent core is made of pure tungsten powder. The tungsten powder has a D10 of 45–50 μm, a D50 of 72–78 μm, a D90 of 100–105 μm, a flowability (Hall flow rate) ≤6.5 s / 50 g, and a loose packing density ≥10.5 g / cm³. 3 .

[0080] like Figure 2 As shown, the preparation process of electron beam selective melting of pure tungsten composite liquid wick is as follows:

[0081] Step 1, Raw material preparation: First, the required pure tungsten powder material is subjected to vacuum low-temperature drying treatment (5-10 minutes). - 1 Torr (120-150℃, 1-2 hours) to improve powder flowability; load the treated powder raw material into the EBSM equipment, using a tungsten plate as the molding substrate, and adjust the EBSM equipment to maintain a vacuum level of 10. -1 Pa, ready for 3D printing;

[0082] Step 2, Model Design: Use commercial modeling software to design a combined aspiration core model, such as... Figure 3 As shown, it includes a trench structure and a layer of porous powder material;

[0083] Step 3, EBSM additive manufacturing:

[0084] (1) Based on the structural characteristics of the combined liquid-absorbing core model, the model was split into two parts, a groove structure and a powder porous material layer, using MAGICS software. The groove structure and the powder porous material layer were sliced ​​to form a combined liquid-absorbing core additive model.

[0085] (2) Preheat the substrate of the EBSM equipment to 1100℃;

[0086] (3) Pure tungsten powder is spread on the preheated substrate and the powder is preheated by electron beam defocusing heating to achieve slight sintering; the target temperature is set at 1100℃, and the process parameters are: beam current 25-35mA, scanning speed 18-21m / s, powder thickness 50μm, and high-speed reciprocating scanning strategy; so that the powder can obtain better thermal conductivity, electrical conductivity and mechanical stability.

[0087] (4) The combined liquid absorption core groove structure powder is melted according to the model design in step 2 to form a dense groove structure; the melting process parameters are: beam current 15-20mA, scanning speed 0.5-1.0m / s, overlap spacing 80-100μm, powder thickness 50μm, and scanning strategy is slow reciprocating scanning.

[0088] (5) According to the model design in step 2, the powder sintering area is sintered at high temperature to form a porous material layer of powder sintering; sintering process parameters: beam current 25-35mA, scanning speed 5-10m / s, powder thickness 50μm, scanning strategy is high-speed reciprocating scanning.

[0089] (6) Repeat the above steps on the surface of the formed layer until the combined liquid-absorbing core additive blank designed in step 2 is completed.

[0090] Step 4, Heat treatment and machining: Use a powder cleaning device and high-pressure gas to remove excess metal powder from the grooves of the combined liquid absorbing core blank, and perform stress-relief annealing. Process parameters: vacuum environment, 1200℃, 3 hours, furnace cooling; polishing; obtain the combined liquid absorbing core sample.

[0091] The mechanical and fatigue properties of the combined liquid-absorbing core are shown in Table 1.

[0092] Example 2

[0093] A new generation of M247 nickel-based high-temperature alloy composite wicking core for thermal protection of ultra-high temperature heat pipes is prepared using the electron beam selective melting (EBSM) technology proposed in this invention, such as... Figure 1 As shown, it is suitable for ultra-high temperature environments above 1500℃.

[0094] The material of this combined liquid-absorbing core is M247 nickel-based high-temperature alloy.

[0095] like Figure 2 As shown, the preparation process of the M247 nickel-based superalloy combined wicking core electron beam selective melting is as follows:

[0096] Step 1, Raw Material Preparation: First, the required M247 nickel-based high-temperature alloy powder material is subjected to vacuum low-temperature drying treatment (5-10 minutes). -1 Torr (120-150℃, 1-2 hours) to improve powder flowability; load the treated powder raw material into the EBSM equipment, using an M247 nickel-based high-temperature alloy plate as the forming substrate, and adjust the EBSM equipment to maintain a vacuum level of 10. -1 Pa, ready for 3D printing;

[0097] Step 2, Model Design: Use commercial modeling software to design a combined aspiration core model, such as... Figure 3As shown, it includes a trench structure and a layer of porous powder material;

[0098] Step 3, EBSM additive manufacturing:

[0099] (1) Based on the structural characteristics of the combined liquid-absorbing core model, the model was split into two parts, a groove structure and a powder porous material layer, using MAGICS software. The groove structure and the powder porous material layer were sliced ​​to form a combined liquid-absorbing core additive model.

[0100] (2) Preheat the substrate of the EBSM equipment to 1100℃;

[0101] (3) M247 nickel-based high-temperature alloy powder was spread on the preheated substrate, and the powder was preheated by electron beam defocusing heating to achieve slight sintering; the target temperature was set at 1100℃, and the process parameters were: beam current 17-33mA, scanning speed 21m / s, powder thickness 50μm, and high-speed reciprocating scanning strategy; so that the powder could obtain better thermal conductivity, electrical conductivity and mechanical stability.

[0102] (4) Melt the trench structure powder according to the model design in step 2 to form a dense trench structure; melting process parameters: beam current 1-10mA, scanning speed 0.4-5m / s, powder thickness 50μm, scanning strategy is slow reciprocating scanning.

[0103] (5) According to the model design in step 2, the powder sintering area is sintered at high temperature to form a porous material layer of powder sintering; sintering process parameters: beam current 17-33mA, scanning speed 10-15m / s, powder thickness 50μm, scanning strategy is high-speed reciprocating scanning.

[0104] (6) Repeat the above steps on the surface of the formed layer until the combined liquid-absorbing core additive blank designed in step 2 is completed.

[0105] Step 4, Heat treatment and machining: Use a powder cleaning device and high-pressure gas to remove excess metal powder from the grooves of the combined liquid suction core blank;

[0106] Heat treatment: solution treatment at 1150-1200℃ for 4 hours, followed by air cooling; aging at 900-1000℃ for 4 hours, followed by air cooling.

[0107] Polishing; to obtain a combined liquid-absorbing core sample.

[0108] The mechanical and fatigue properties of the combined liquid-absorbing core are shown in Table 1.

[0109] Example 3

[0110] A composite liquid wick made of TA15 titanium alloy for thermal protection of high-temperature heat pipes is prepared using the electron beam selective melting (EBSM) technology proposed in this invention. Figure 1 As shown.

[0111] like Figure 2 As shown, the preparation process of electron beam selective melting of the TA15 titanium alloy composite wick is as follows:

[0112] Step 1, Raw Material Preparation: First, the required TA15 titanium alloy powder material is subjected to vacuum low-temperature drying treatment (5-10 minutes). -1 Torr (120-150℃, 1-2 hours) to improve powder flowability; load the treated powder raw material into the EBSM equipment, using TA15 titanium alloy plate as the molding substrate, and adjust the EBSM equipment to maintain a vacuum degree of 10. -1 Pa, ready for 3D printing;

[0113] Step 2, Model Design: Use commercial modeling software to design a combined aspiration core model, such as... Figure 3 As shown, it includes a trench structure and a layer of porous powder material;

[0114] Step 3, EBSM additive manufacturing:

[0115] (1) Based on the structural characteristics of the combined liquid-absorbing core model, the model was split into two parts, a groove structure and a powder porous material layer, using MAGICS software. The groove structure and the powder porous material layer were sliced ​​to form a combined liquid-absorbing core additive model.

[0116] (2) Preheat the substrate of the EBSM equipment to 600°C;

[0117] (3) TA15 titanium alloy powder is spread on the preheated substrate, and the powder is preheated by electron beam defocusing heating to achieve slight sintering; the target temperature is set to 600℃, and the process parameters are: beam current 25-30mA, scanning speed 27-55m / s, powder layer thickness 40μm, and scanning strategy is high-speed reciprocating scanning; so that the powder can obtain better thermal conductivity, electrical conductivity and mechanical stability.

[0118] (4) Melt the groove structure powder according to the model design in step 2 to form a dense groove structure; melting process parameters: beam current 6-20mA, scanning speed 0.7-2.4m / s, powder layer thickness 40μm, scanning strategy is slow reciprocating scanning;

[0119] (5) According to the model design in step 2, the powder sintering area is sintered at high temperature to form a porous material layer of powder sintering; sintering process parameters: beam current 25-30mA, scanning speed 15-30m / s, powder layer thickness 40μm, scanning strategy is high-speed reciprocating scanning.

[0120] (6) Repeat the above steps on the surface of the formed layer until the combined liquid-absorbing core additive blank designed in step 2 is completed.

[0121] Step 4, Heat Treatment and Machining: Use a powder cleaning device and high-pressure gas to remove excess metal powder from the grooves of the combined liquid absorbing core blank, and perform stress-relief annealing. Process parameters: vacuum environment, 500℃, 2h, furnace cooling; performance-controlled heat treatment temperature: 850℃, 2-4 hours, air cooling; polishing; obtain the combined liquid absorbing core sample.

[0122] The mechanical and fatigue properties of the combined liquid-absorbing core are shown in Table 1.

[0123] Comparative Example 1

[0124] A combined pure tungsten wicking core for ultra-high temperature heat pipes was prepared using a series process: groove machining + powder sintering. The raw materials for this combined wicking core are pure tungsten plates and pure tungsten powder. The tungsten powder has a D10 of 45–50 μm, a D50 of 72–78 μm, a D90 of 100–105 μm, a flowability (Hall flow rate) ≤6.5 s / 50 g, and a bulk density ≥10.5 g / cm³. 3 .

[0125] The preparation process is as follows:

[0126] Step 1, Raw material preparation: First, the surface of the tungsten plate is alkaline washed to remove surface oil, impurities and oxide layer;

[0127] Step 2, Tungsten Plate Fixing: Fix the tungsten plate on the processing platform to ensure that the tungsten plate will not move during the microgroove processing;

[0128] Step 3, Parameter Settings: Set all operating parameters of the laser processing equipment: laser wavelength 1064nm, energy density 50-60J / cm². 2 The pulse width is 100ns, the repetition frequency is 40kHz, the scanning speed is 180-220mm / s, and the scanning interval is 0.2mm.

[0129] Step 4, Groove processing: Use laser processing equipment to process at a fixed position on the surface of the tungsten plate to obtain microgrooves on the surface of the tungsten plate, ensuring that the laser beam is perpendicular to the surface of the component processing position;

[0130] Step 5, Grinding and Polishing: Grinding and polishing the tungsten plate after laser processing to remove the recast layer and "flanging" problem caused by laser processing on the workpiece surface;

[0131] Step 6, Cleaning: Use mechanical methods to clean the grooves on the surface of the tungsten plate to ensure the wettability of the groove walls and the flow performance of the cooling medium; after cleaning, perform drying.

[0132] Step 7, Powder Spreading: Powder is spread on the surface of the grooved tungsten plate, and a powder layer of uniform thickness is obtained by vibration treatment. Then, the tungsten plate covered with powder is placed in a vacuum heat treatment furnace.

[0133] Step 8, Sintering: Set the parameters of the vacuum heat treatment furnace, evacuate, heat up, sinter, cool down, and remove the parts to complete the powder sintering and forming; the vacuum sintering process parameters are: sintering temperature 1500-1700℃, holding time 1-3 hours.

[0134] Step 9, Powder Cleaning: Clean the sintered combined liquid absorbing core to remove unsintered residual powder and obtain a combined liquid absorbing core blank.

[0135] Step 10, Inspection: Finally, non-destructive testing and performance testing are carried out on the combined liquid suction core blank. After passing the test, a combined liquid suction core with groove structure and powder sintering structure is obtained.

[0136] The mechanical and fatigue properties of the combined liquid-absorbing core are shown in Table 1.

[0137] Comparative Example 2

[0138] The composite wicking core was prepared using the same preparation method as in Example 1, with the difference being the different process parameters for electron beam selective melting and sintering. The specific parameters are as follows:

[0139] Melting process parameters: beam current 6-20mA, scanning speed 0.7-2.4m / s, powder thickness 50μm, scanning strategy is slow reciprocating scanning;

[0140] Sintering process parameters: beam current 25-30mA, scanning speed 15-30m / s, powder thickness 50μm, scanning strategy is high-speed reciprocating scanning;

[0141] As a result, printing could not be completed under the above process parameters.

[0142] Table 1 Mechanical and fatigue properties of the combined liquid-absorbing core

[0143]

[0144]

[0145] Comparative analysis of Examples 1-3 and Comparative Example 1 shows that the production efficiency of Example 1 is improved by more than 50%, and the forming accuracy and process controllability are significantly better than the latter.

[0146] As can be seen from Table 1, the combined liquid-absorbing core prepared in Example 1 has significantly improved high-temperature compression performance compared with Comparative Example 1, mainly reflected in the improvement of compressive strength at high temperature.

[0147] Meanwhile, the method of the present invention achieves integrated forming of heat pipe components, eliminating the need for welding to complete component assembly. As can be seen from Table 1, the fatigue performance of the combined liquid wick prepared by the method of the present invention is much higher than that of the combined liquid wick prepared by the prior art.

[0148] As can be seen from Example 1 and Comparative Example 2, the various process parameters of electron beam selective melting and sintering in the method of the present invention need to be strictly controlled in order to achieve additive manufacturing and complete the printing of the target component.

[0149] This invention utilizes the advantages of EBSM technology, such as high preheating temperature, good forming accuracy, and high degree of freedom in decoking sintering and focused melting. By controlling the EBSM melting and sintering process, it solves the problem of on-demand construction and integrated manufacturing of difficult-to-form alloy composite liquid absorber cores. It is suitable for the engineering manufacturing of ultra-high temperature components with complex structures on the windward side, laying a technical foundation for the manufacturing and processing of heat pipe protection components for next-generation high-speed aircraft.

[0150] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for electron beam additive manufacturing of a difficult-to-form composite liquid-absorbing core, characterized in that, Includes the following steps: S1. Equipment and raw material preparation; wherein, the raw materials are selected from one of the following difficult-to-form alloys: refractory metals W and Mo, casting high-temperature alloy Mar-M247, easily cracked titanium alloy Ta15, high-temperature high-entropy alloy, or pure copper. S2. Model Design: Use modeling software to design a combined liquid absorption core model, including a groove structure and a layer of porous powder material on it; S3, EBSM additive manufacturing: Based on the combined liquid suction core model determined in step S2, the combined liquid suction core additive blank is integrally formed by controlling process parameters and scanning strategy; S4. Heat treatment and machining: The combined liquid-absorbing core additive blank obtained in step S3 is subjected to post-processing in sequence to obtain the combined liquid-absorbing core sample. The additive manufacturing process described in step S3 uses the EBSM process and specifically includes the following steps: S301. Based on the structural characteristics of the combined absorbent core model, the model is divided into two parts: a groove structure and a powder porous material layer. The groove structure and the powder porous material layer are sliced ​​to form a combined absorbent core additive model. S302. Spread a layer of powder raw material evenly on the substrate. Set different process parameters and scanning strategies according to the two regions divided in step S301. Melt or sinter the powder according to the region to achieve the densification of the trench structure and the sintering of the surface powder material. S303. After the first layer of powder is formed, powder is spread on the basis of the first layer. Repeat step S302 until a combined liquid-absorbing core additive blank that meets the design of the combined liquid-absorbing core model in step S2 is obtained. In steps S302 and S303, the substrate is preheated before spreading the powder raw material. After the powder is spread, the powder is preheated by electron beam defocusing heating to achieve slight sintering of the powder. In steps S302 and S303, the trench structure is melted by electron beam selective melting, and the porous powder material layer is sintered by electron beam selective melting. Steps S302 and S303 are continuous operations, which realize the integral forming of the trench structure and the porous material layer.

2. The electron beam additive manufacturing method for difficult-to-form composite liquid-absorbing cores according to claim 1, characterized in that, Step S1 includes: first, vacuum low-temperature drying treatment of the difficult-to-form alloy powder, then loading the treated powder raw material into an electron beam selective melting (EBSM) device, selecting a metal plate suitable for the powder raw material as the forming substrate, debugging the EBSM device, and completing the preparation of additive manufacturing equipment and raw materials.

3. The electron beam additive manufacturing method for difficult-to-form composite liquid-absorbing cores according to claim 1, characterized in that, The particle size of the difficult-to-form alloy powder is 53μm~105μm.

4. A difficult-to-form composite liquid-absorbing core, characterized in that, It is prepared by the electron beam additive manufacturing method for difficult-to-form composite liquid-absorbing cores as described in any one of claims 1-3.

5. The difficult-to-form composite liquid-absorbing core according to claim 4, characterized in that, The combined liquid-absorbing core consists of two parts: a groove structure and a layer of porous powder material located thereon.

6. The difficult-to-form composite liquid-absorbing core according to claim 5, characterized in that, The groove structure includes a substrate and fins disposed thereon, with grooves formed between the fins. The fin thickness is 0.2~0.3mm, the fin spacing is 0.1-0.2mm, and the groove depth is 0.3-0.8mm.

7. The difficult-to-form composite liquid-absorbing core according to claim 5, characterized in that, The porous powder material layer is formed on top of the trench structure.

8. The difficult-to-form composite liquid-absorbing core according to claim 7, characterized in that, The porous powder material layer has a pore size of 0.04-0.1 mm and a thickness of 1-3 mm.

Citation Information

Patent Citations

  • Integrally-formed water-cooled radiator integrated with vapor chamber and preparation method of integrally-formed water-cooled radiator

    CN115361845A

  • Copper alloy preparation method for improving electric conductivity and strength

    CN115570149A