A method for preparing a chromium-free corrosion-resistant refractory composite material for RH refining furnace
By preparing a chromium-free refractory composite material containing an anti-corrosion layer of MgO and magnesium aluminate sol solution and a bonding layer of gradient components, the problem of existing refractory materials generating toxic hexavalent chromium compounds under high temperature conditions has been solved and achieved Efficient anti-corrosion and anti-penetration properties extend the service life of the material.
Patent Information
- Application Number
- CN202311589569.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-11-27
AI Technical Summary
Existing refractory materials easily react with kiln materials under high temperature conditions to form toxic hexavalent chromium compounds, causing environmental pollution, and a single material cannot simultaneously guarantee the fire resistance and corrosion resistance of the inner layer and the bonding of the outer layer, strong peeling resistance, and small expansion coefficient. performance.
The preparation method of chromium-free corrosion-resistant refractory composite materials is adopted, including an anti-corrosion layer and a bonding layer. The anti-corrosion layer is composed of MgO, magnesium aluminate sol solution, SiO2, etc., and the bonding layer is suppressed by setting a gradient component concentration gradient area. Molding, the connection layer contains materials such as Al2O3, SiO2, ZrO2, etc., and is spliced and fired to form a composite material.
It achieves excellent resistance to chemical erosion and medium penetration in high temperature and corrosive environments, extends the service life of the material, improves the stability and durability of the composite material, and meets the working environment requirements of the RH refining furnace.
Smart Images

Figure CN117682877B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of refractory composite material preparation, and in particular to a method for preparing a chromium-free corrosion-resistant refractory composite material for an RH refining furnace. Background Art
[0002] In order to achieve the goal of modernization of the cement industry, a lot of research work has been carried out in the field of refractory materials at home and abroad, hoping to find materials to replace magnesia-chrome bricks. However, the results of these alternative materials have not been satisfactory so far.
[0003] Under high temperature conditions, chromium-containing refractory materials react with alkali metal oxides in kiln gas and kiln materials to produce toxic soluble hexavalent chromium compounds. For a long time, magnesia-chrome bricks have been used as lining materials for cement rotary kilns. However, this type of brick will leave hexavalent chromium after use and seep into groundwater, causing serious harm to the environment. In order to solve this problem, the cement industry urgently needs chromium-free lining materials to reduce the risk of groundwater pollution.
[0004] Magnesium spinel bricks are considered to be a material with excellent thermal shock stability, resistance to chlorine and sulfur corrosion, and are therefore regarded as the development trend of chromium-free alkaline refractory materials in cement rotary kiln firing zones. However, there are some problems with magnesium spinel bricks. First, it is easy to adhere to the kiln lining in the kiln. Secondly, at excessively high temperatures, the spinel component in magnesium spinel bricks easily reacts with C3S or C3A in cement clinker to generate low-melting-point C12A7, resulting in kiln lining sintering and corrosion of spinel minerals. These problems limit the application of magnesium spinel bricks in cement rotary kiln firing zones. Moreover, a single refractory material cannot simultaneously guarantee the fire resistance and corrosion resistance of the inner layer to molten steel and the ability of the outer layer to be easy to bond, easy to bond, strong in anti-stripping, and small in expansion coefficient. Therefore, it is urgent to overcome these problems and prepare higher-quality chromium-free corrosion-resistant refractory composite materials. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing a chromium-free corrosion-resistant and refractory composite material for an RH refining furnace. The composite material prepared by the method comprises an anti-corrosion layer and a bonding layer, wherein the bonding layer comprises a bonding layer and a connecting layer. The preparation method comprises the following steps:
[0006] S1. Preparation of anti-corrosion layer:
[0007] In terms of mass percentage, 10-14wt% of MgO, 3-5wt% of magnesium aluminate sol, 0.6-0.8wt% of SiO2, 0.3-0.4wt% of R2O and the balance of Al2O3 are mixed for 30-50min to obtain an anti-corrosion layer blank, which is then pressed under a pressure of 100-300MPa to obtain an anti-corrosion layer; the water content in the magnesium aluminate sol accounts for 1-2wt% of the total weight of the magnesium aluminate sol;
[0008] S2, preparing the bonding layer;
[0009] S2-1, preparing a single bonding layer:
[0010] Dividing the component concentration gradient regions of the bonding layer: starting from the contact surface between the anti-corrosion layer and the bonding layer and pointing to the edge of the bonding layer away from the anti-corrosion layer, the bonding layer is divided into four component concentration gradient regions: a first region, a second region, a third region, and a fourth region; pouring into the bonding layer mold in sequence according to the four component concentration gradient regions, and pressing and molding under a pressure of 100 to 300 MPa to obtain the bonding layer;
[0011] S2-2, preparing the connecting layer;
[0012] S3. Preparation of composite materials:
[0013] S3-1. Splicing and pressing composite materials
[0014] According to the design requirements, the anti-corrosion layer, the bonding layer and the connecting layer are spliced into an original blank, and the original blank is pressed and formed under a pressure of 300 to 400 MPa and then dried to obtain a composite blank;
[0015] S3-2, sintered composite blank
[0016] The composite blank is placed in a corundum tube furnace, fired at a temperature of 1600-1750°C for 3-5 hours, and then the furnace is stopped for insulation for 2-3 hours to obtain a composite material.
[0017] Description: When the anti-corrosion layer comes into contact with different types of RH refined slag, it reacts with CaO and SiO2 in the RH refined slag and has excellent resistance to chemical erosion and penetration.
[0018] When the corrosion-resistant layer comes into contact with molten steel and slag, MgO, magnesium-aluminum spinel and non-flaky MgAlON spinel absorb Fe2+, Mn2+, Cr3+ and other ions in the molten steel or slag to form a solid solution transition layer of MgO, MnO, FeO and Mg, Mn, Fe, etc., which changes the structure of the material and the composition of the contact slag. The dense layer formed improves the pore structure in the corrosion-resistant layer and reduces the pore diameter.
[0019] The combined effect of the two provides a new pathway for the corrosion-resistant layer refractory material to react with molten steel or slag penetration, prolongs the reaction time with molten steel or slag, improves the material's resistance to chemical corrosion and medium penetration, and makes the corrosion-resistant layer more resistant to corrosion.
[0020] Furthermore, in the first region described in step S2, the following components are uniformly mixed according to mass percentage:
[0021] Mix 50-70wt% Al2O3, 4-6wt% SiO2, 1-3wt% ZrO2, 0.5-1.5wt% La2O3, 1-2wt% CaO, 3-5wt% magnesium aluminate sol solution, 0.3-0.4wt% R2O, 1-2wt% Fe2O3 and the balance MgO;
[0022] In the second region, the following components are uniformly mixed according to mass percentage:
[0023] Mix 45-65wt% Al2O3, 3-5wt% SiO2, 1-3wt% ZrO2, 0.5-1.5wt% La2O3, 1-2wt% CaO, 2-4wt% magnesium aluminate sol solution, 0.2-0.3wt% R2O, 1-2wt% Fe2O3 and the balance MgO;
[0024] In the third region, the following components are uniformly mixed according to mass percentage:
[0025] Mix 40-60wt% Al2O3, 2-4wt% SiO2, 1-3wt% ZrO2, 0.5-1.5wt% La2O3, 1-2wt% CaO, 1-3wt% magnesium aluminate sol solution, 0.1-0.2wt% R2O, 1-2wt% Fe2O3 and the balance MgO;
[0026] In the fourth region, the following components are uniformly mixed according to mass percentage:
[0027] Mix 35-55wt% Al2O3, 4-6wt% SiO2, 1-3wt% ZrO2, 0.5-1.5wt% La2O3, 1-2wt% CaO, 1-2wt% Fe2O3 and the balance MgO.
[0028] Description: By setting the component ratio concentration in a gradient, the connection between the anti-corrosion layer and the bonding layer is made more stable, cracks are avoided at the connection between the anti-corrosion layer and the bonding layer, and the stability of the composite material is enhanced.
[0029] Furthermore, in step S2-2, the preparation step of the connecting layer is: uniformly mixing the following components according to mass percentage: 42.5~62.5wt% Al2O3, 2~4wt% SiO2, 1~3wt% ZrO2, 0.5~1.5wt% La2O3, 1~2wt% CaO, 0.2~0.3wt% R2O, 1~2wt% Fe2O3, 3~7wt% ZnO, 2~4wt% HA and the remainder MgO.
[0030] Description: Al2O3 provides high temperature stability, SiO2 enhances wear resistance, ZrO2 increases thermal shock resistance, La2O3 and CaO improve corrosion resistance, R2O adjusts the melting point and adhesion of the material, Fe2O3 increases the strength and pressure resistance of the material, and MgO, as the supporting material of the main alumina material, has good thermal expansion and thermal shock resistance, and can obtain good chemical stability, heat resistance and mechanical properties in the preparation process of the connecting layer. Hydrated alumina, HA, is made by flash calcination of aluminum hydroxide or boehmite. Its hydration product Al3 can be used as a refractory castable to provide early strength. At the same time, its self-bonding system avoids the formation of low melting point phases, which can improve the high temperature service performance of refractory castables. Adding ZnO to combine with HA accelerates the setting time.
[0031] Furthermore, the Al2O3 in step S1 includes three particle sizes: 3-5 mm, 1-3 mm, and 0-1 mm, and the ratio of the three particle sizes is 1:7:5; the particle size of the MgO is 0-1 mm.
[0032] Note: Using three different Al2O3 particle sizes can enhance the density of the composite material and increase the thermal shock resistance after firing.
[0033] Furthermore, the anti-corrosion layer blank in step S1 also includes auxiliary materials accounting for 5 to 10 wt% of the anti-corrosion layer blank; the preparation method of the auxiliary materials is: 0.1 to 0.3 wt% of Na2O, 0.1 to 0.2 wt% of Fe2O3 and the remainder of CaO are uniformly mixed and powdered to obtain a first powder, a binder accounting for 5 to 10% of the mass ratio of the first powder is added and mixed for 5 to 9 minutes, and the same dose of binder is added to the first powder for a second time to obtain the auxiliary materials.
[0034] Description: By adding auxiliary materials, the anti-corrosion layer can be strengthened after firing. The anti-corrosion layer fired from the blank has a stronger densification effect and can reduce the porosity of the anti-corrosion layer. CA6 crystals can improve the toughening effect of the anti-corrosion layer while maintaining the ability to resist high temperatures.
[0035] Furthermore, the preparation method of the auxiliary material is: dry mixing on a planetary ball mill at a speed of 200-300 r / min for 2-3 hours.
[0036] Description: The ball milling process can effectively refine the auxiliary material particles, which helps to ensure the uniform distribution of the various components in the auxiliary materials. The ball milling process can introduce stress and collision, promote the microstructural changes of the auxiliary material particles and increase the surface activity. The refined powder can achieve better uniformity and density.
[0037] Furthermore, the particle sizes of Fe2O3, CaO and Na2O include three types: 1-3 mm, 0-1 mm and 200 mesh fine powder, and the proportions of the three particle sizes are 1:5:2.
[0038] Description: Auxiliary materials with various particle sizes can achieve better uniform mixing and dispersion. Coarse Fe2O3 particles can provide a basis for uniform dispersion, while fine CaO and Na2O powders can be filled between coarse particles to form a more uniform mixing state. Through the combination of particle sizes, better mechanical properties and stability can be achieved. Coarse Fe2O3 particles can increase the strength and stability of the material, while fine CaO and Na2O powders can provide better filling effects and stability of the ceramic structure.
[0039] Furthermore, the binder is pulp waste liquid, the particle size of the first powder includes two types: 1-3 mm and 0-1 mm, and the particle size of the powder of the secondary feed is 200 mesh.
[0040] Description: The first powder has a wide range of particle size distribution, including 1-3mm and 0-1mm. When mixed with pulp waste liquid, it can form a more uniform mixing state, which helps to increase the contact area between the binder and the powder and increase the mutual bonding force between the particles. The pulp waste liquid has good viscosity and adhesion as a binder, which can enhance the bonding force of the powder and improve the stability and durability of the material. The powder of the secondary feed has a finer particle size and is easy to mix and evenly disperse. The finer powder can better fill the gap between the pulp waste liquid and the first powder, which helps to improve the density and uniformity of the mixture.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] (1) The chromium-free corrosion-resistant and refractory composite material prepared by the method of the present invention has higher composite properties by splicing firing. The inner side in contact with molten steel and slag adopts an anti-corrosion layer, and the outer layer adopts a bonding layer with a low expansion coefficient and strong thermal shock resistance. The anti-corrosion layer contains a high proportion of MgO and magnesium aluminate sol liquid. After mixed firing, it has good corrosion resistance and can enable the composite material to maintain stable performance in high temperature and corrosive environment.
[0043] (2) The low expansion coefficient and strong thermal shock resistance of the bonding layer can effectively reduce the thermal stress and thermal shock damage risk of the composite material during the temperature change process, and can improve the service life and durability of the composite material. Al2O3 has high temperature stability, SiO2, ZrO2, and La2O3 have excellent corrosion resistance, and can form a stable oxide protective film after high-temperature firing to block the corrosion of refractory bricks by corrosive substances such as acids and alkalis, thereby extending their service life. CaO and Fe2O3 have high melting points and corrosion resistance, can exist stably at high temperatures, and can form stable compounds with other substances. MgO can stabilize the crystal structure of Al2O3 and increase the shock resistance and stability of refractory bricks. This method can prepare a chromium-free composite material with good corrosion resistance. Its corrosion resistance layer and bonding layer have high chemical stability and heat resistance, and can also meet the working environment requirements of the RH refining furnace. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 is a schematic diagram of the splicing structure of the composite material of Example 1 of the present invention;
[0045] Among them, 1-anti-corrosion layer, 2-adhesive layer, 21-adhesive layer, 22-connecting layer. DETAILED DESCRIPTION
[0046] The present invention is further described in detail below in conjunction with specific implementation methods to better reflect the advantages of the present invention.
[0047] Example 1
[0048] Example 1 is used to illustrate a method for preparing a chromium-free corrosion-resistant and refractory composite material for an RH refining furnace designed by the present invention, characterized in that the composite material prepared by the method comprises an anti-corrosion layer 1 and a bonding layer 2, wherein the bonding layer 2 comprises a bonding layer 21 and a connecting layer 22; the preparation method comprises the following steps:
[0049] S1. Preparing the anti-corrosion layer 1:
[0050] In terms of mass percentage, 12wt% of MgO, 4wt% of magnesium aluminate sol, 0.7wt% of SiO2, 0.35wt% of R2O and the balance of Al2O3 are mixed for 40 minutes to obtain an anti-corrosion layer blank, which is pressed under a pressure of 200MPa to obtain an anti-corrosion layer 1; the water content in the magnesium aluminate sol accounts for 1.5wt% of the total weight of the magnesium aluminate sol;
[0051] The particle sizes of Al2O3 are 3.5-4mm, 1.2-1.5mm, and 0.1-0.5mm, and the ratio of the three particle sizes is 1:7:5; the particle size of MgO is 0.1-0.5mm;
[0052] S2, preparing the bonding layer;
[0053] S2-1, the preparation method of the bonding layer 21 is: divide the component concentration gradient area of the bonding layer 21: starting from the contact surface between the anti-corrosion layer 1 and the bonding layer 21, pointing to the edge of the bonding layer 21 away from the anti-corrosion layer 1, the bonding layer 21 is divided into four component concentration gradient areas: the first area, the second area, the third area, and the fourth area; pour the four component concentration gradient areas into the mold of the bonding layer 21 in sequence, and press and mold under a pressure of 200 MPa to obtain the bonding layer 21;
[0054] S2-2, preparing the connecting layer 22
[0055] In the first region, the following components are uniformly mixed according to mass percentage:
[0056] 60wt% Al2O3, 5wt% SiO2, 2wt% ZrO2, 1wt% La2O3, 1.5wt% CaO, 4wt% magnesium aluminate sol, 0.35wt% R2O, 1.5wt% Fe2O3 and the balance MgO;
[0057] In the second region, the following components are uniformly mixed according to mass percentage:
[0058] Mix 55wt% Al2O3, 4wt% SiO2, 2wt% ZrO2, 1wt% La2O3, 1.5wt% CaO, 3wt% magnesium aluminate sol, 0.25wt% R2O, 1.5wt% Fe2O3 and the balance MgO;
[0059] In the third region, the following components are uniformly mixed according to mass percentage:
[0060] Mix 50wt% Al2O3, 3wt% SiO2, 2wt% ZrO2, 1wt% La2O3, 1.5wt% CaO, 2wt% magnesium aluminate sol, 0.15wt% R2O, 1.5wt% Fe2O3 and the balance MgO;
[0061] In the fourth region, the following components are uniformly mixed according to mass percentage:
[0062] Mix 45wt% Al2O3, 5wt% SiO2, 2wt% ZrO2, 1wt% La2O3, 1.5wt% CaO, 1.5wt% Fe2O3 and the balance MgO;
[0063] The preparation steps of the single connecting layer 22 are as follows: uniformly mix the following components according to mass percentage: 52.5wt% Al2O3, 3wt% SiO2, 2wt% ZrO2, 1wt% La2O3, 1.5wt% CaO, 0.25wt% R2O, 1.5wt% Fe2O3 and the balance MgO;
[0064] S3. Preparation of composite materials:
[0065] S3-1. Splicing and pressing composite materials
[0066] According to the design requirements, the anti-corrosion layer 1, the bonding layer 21 and the connecting layer 22 are spliced into an original blank, and the original blank is pressed and formed under a pressure of 200 MPa and then dried to obtain a composite blank; in this embodiment, the original blank of the refractory brick fired by the composite material is a rectangular parallelepiped, see Figure 1 The original blank is composed of an anti-corrosion layer 1, five bonding layers 21 and four connecting layers 22;
[0067] S3-1, sintered composite blank
[0068] The composite blank was placed in a corundum tube furnace, fired at 1675°C for 4 hours, and then stopped to keep warm for 2.5 hours to obtain a composite material.
[0069] Example 2
[0070] The difference between this embodiment and embodiment 1 is that the anti-corrosion layer blank in step S1 further includes auxiliary materials accounting for 7.5wt% of the anti-corrosion layer blank; the preparation method of the auxiliary materials is: 0.2wt% of Na2O, 0.15wt% of Fe2O3 and the remaining CaO are uniformly mixed and powdered to obtain a first powder, a binder accounting for 7.5% of the mass ratio of the first powder is added and mixed for 7 minutes, and the same amount of binder is added to the first powder for a second time to obtain the auxiliary materials;
[0071] The preparation method of the auxiliary material is: dry mixing and grinding for 2.5 hours at a speed of 250r / min on a planetary ball mill; the particle sizes of Fe2O3, CaO and Na2O include three types: 1.5-2mm, 0.1-0.5mm and 200 mesh fine powder, and the proportion of the three particle sizes is 1:5:2;
[0072] The binder is pulp waste liquid, the particle size of the first powder includes two types: 1-1.5 mm and 0.1-0.5 mm, and the particle size of the powder of the secondary feed is 200 meshes.
[0073] Example 3
[0074] The difference between this embodiment and embodiment 1 is that the anti-corrosion layer blank in step S1 also includes auxiliary materials accounting for 5wt% of the anti-corrosion layer blank.
[0075] Example 4
[0076] The present embodiment is different from the embodiment 1 in that the anti-corrosion layer blank in step S1 further includes auxiliary materials accounting for 10 wt % of the anti-corrosion layer blank.
[0077] Example 5
[0078] The present embodiment is different from the embodiment 1 in that the preparation method of the auxiliary material is as follows: 0.1wt% Na2O, 0.1wt% Fe2O3 and the remainder CaO are uniformly mixed and powdered to obtain a first powder, and a binder accounting for 5% by mass of the first powder is added and mixed for 5 minutes.
[0079] Example 6
[0080] The difference between this embodiment and embodiment 1 is that the preparation method of the auxiliary material is: 0.3wt% Na2O, 0.2wt% Fe2O3 and the remainder CaO are uniformly mixed and powdered to obtain a first powder, and a binder accounting for 10% of the mass ratio of the first powder is added and mixed for 9 minutes.
[0081] Example 7
[0082] This embodiment is different from Embodiment 1 in that 10wt% MgO, 3wt% magnesium aluminate sol, 0.6wt% SiO2, 0.3wt% R2O and the remainder Al2O3 are mixed for 30 minutes to obtain an anti-corrosion layer blank, which is then pressed under a pressure of 100MPa to obtain an anti-corrosion layer 1; the water content in the magnesium aluminate sol accounts for 1wt% of the total weight of the magnesium aluminate sol.
[0083] Example 8
[0084] This embodiment is different from Embodiment 1 in that 14wt% MgO, 5wt% magnesium aluminate sol, 0.8wt% SiO2, 0.4wt% R2O and the remainder Al2O3 are mixed for 50 minutes to obtain an anti-corrosion layer blank, which is then pressed under a pressure of 300MPa to obtain an anti-corrosion layer 1; the water content in the magnesium aluminate sol accounts for 2wt% of the total weight of the magnesium aluminate sol.
[0085] Example 9
[0086] The present embodiment is different from the embodiment 1 in that the composite blank is placed in a corundum tube furnace, fired at 1600° C. for 3 hours, and then the furnace is stopped for heat preservation for 2 hours to obtain a composite material.
[0087] Example 10
[0088] The present embodiment is different from the embodiment 1 in that the composite blank is placed in a corundum tube furnace, fired at 1750° C. for 5 hours, and then the furnace is stopped for heat preservation for 3 hours to obtain a composite material.
[0089] Embodiment 11
[0090] The difference between this embodiment and embodiment 1 is that in the first region described in step S2, the following components are uniformly mixed according to mass percentage:
[0091] Mix 50wt% Al2O3, 4wt% SiO2, 1wt% ZrO2, 0.5wt% La2O3, 1wt% CaO, 3wt% magnesium aluminate sol, 0.3wt% R2O, 1wt% Fe2O3 and the balance MgO;
[0092] In the second region, the following components are uniformly mixed according to mass percentage:
[0093] Mix 45wt% Al2O3, 3wt% SiO2, 1wt% ZrO2, 0.5wt% La2O3, 1wt% CaO, 2wt% magnesium aluminate sol, 0.2wt% R2O, 1wt% Fe2O3 and the balance MgO;
[0094] In the third region, the following components are uniformly mixed according to mass percentage:
[0095] 40wt% Al2O3, 2wt% SiO2, 1wt% ZrO2, 0.5wt% La2O3, 1wt% CaO, 1wt% magnesium aluminate sol, 0.1wt% R2O, 1wt% Fe2O3 and the balance MgO are mixed;
[0096] In the fourth region, the following components are uniformly mixed according to mass percentage:
[0097] 35wt% of Al2O3, 4wt% of SiO2, 1wt% of ZrO2, 0.5wt% of La2O3, 1wt% of CaO, 1wt% of Fe2O3 and the balance of MgO are mixed.
[0098] Example 12
[0099] The difference between this embodiment and embodiment 1 is that in the first region described in step S2, the following components are uniformly mixed according to mass percentage:
[0100] 70wt% Al2O3, 6wt% SiO2, 3wt% ZrO2, 1.5wt% La2O3, 2wt% CaO, 5wt% magnesium aluminate sol, 0.4wt% R2O, 2wt% Fe2O3 and the balance MgO are mixed;
[0101] In the second region, the following components are uniformly mixed according to mass percentage:
[0102] Mix 65wt% Al2O3, 5wt% SiO2, 3wt% ZrO2, 1.5wt% La2O3, 2wt% CaO, 4wt% magnesium aluminate sol, 0.3wt% R2O, 2wt% Fe2O3 and the balance MgO;
[0103] In the third region, the following components are uniformly mixed according to mass percentage:
[0104] Mix 60wt% Al2O3, 4wt% SiO2, 3wt% ZrO2, 1.5wt% La2O3, 2wt% CaO, 3wt% magnesium aluminate sol, 0.2wt% R2O, 2wt% Fe2O3 and the balance MgO;
[0105] In the fourth region, the following components are uniformly mixed according to mass percentage:
[0106] 55 wt% of Al2O3, 6 wt% of SiO2, 3 wt% of ZrO2, 1.5 wt% of La2O3, 2 wt% of CaO, 2 wt% of Fe2O3 and the balance of MgO are mixed.
[0107] Embodiment 13
[0108] This embodiment is different from Embodiment 1 in that, in step S2, the preparation steps of the single connecting layer 22 are: uniformly mixing the following components according to mass percentage: 42.5wt% Al2O3, 2wt% SiO2, 1wt% ZrO2, 0.5wt% La2O3, 1wt% CaO, 0.2wt% R2O, 1wt% Fe2O3, 3wt% ZnO, 2wt% HA and the remainder MgO.
[0109] Embodiment 14
[0110] This embodiment is different from Embodiment 1 in that, in step S2, the preparation steps of the single connecting layer 22 are: uniformly mixing the following components according to mass percentage: 62.5wt% Al2O3, 4wt% SiO2, 3wt% ZrO2, 1.5wt% La2O3, 2wt% CaO, 0.3wt% R2O, 2wt% Fe2O3, 7wt% ZnO, 4wt% HA and the remainder MgO.
[0111] Embodiment 15
[0112] This embodiment is different from Embodiment 1 in that, in step S2, the preparation steps of the single connecting layer 22 are: uniformly mixing the following components according to mass percentage: 52.5wt% Al2O3, 3wt% SiO2, 2wt% ZrO2, 1wt% La2O3, 1.5wt% CaO, 0.25wt% R2O, 1.5wt% Fe2O3, 5wt% ZnO, 3wt% HA and the remainder MgO.
[0113] Experimental example
[0114] In this experimental example, the preparation method in the above-mentioned embodiment 1 is used as a control group, and different experimental groups are designed by changing different process parameters in the preparation method to verify the performance of the refractory composite material. The design scheme is as follows:
[0115] Control group: using the preparation method and process parameters in Example 1;
[0116] Experimental Group 1: The parameters were the same as those of the control group except for the following: In the first region described in step S2, the following components were uniformly mixed according to mass percentage: 50wt% Al2O3, 4wt% SiO2, 1wt% ZrO2, 0.5wt% La2O3, 1wt% CaO, 3wt% magnesium aluminate sol, 0.3wt% R2O, 1wt% Fe2O3 and the remainder MgO were mixed.
[0117] Experimental Group 2: The parameters were the same as those of the control group except for the following: In the first region described in step S2, the following components were uniformly mixed according to mass percentage: 70wt% Al2O3, 6wt% SiO2, 3wt% ZrO2, 1.5wt% La2O3, 2wt% CaO, 5wt% magnesium aluminate sol, 0.4wt% R2O, 2wt% Fe2O3 and the remainder MgO were mixed.
[0118] Experimental Group 3: Except for the following contents, the other parameters are the same as the control group: The preparation steps of the single connecting layer 22 are: uniformly mix the following components according to mass percentage: 42.5wt% Al2O3, 2wt% SiO2, 1wt% ZrO2, 0.5wt% La2O3, 1wt% CaO, 0.2wt% R2O, 1wt% Fe2O3 and the rest MgO.
[0119] Experimental Group 4: Except for the following contents, the other parameters are the same as the control group: The preparation steps of the single connecting layer 22 are: uniformly mix the following components according to mass percentage: 62.5wt% Al2O3, 4wt% SiO2, 3wt% ZrO2, 1.5wt% La2O3, 2wt% CaO, 0.3wt% R2O, 2wt% Fe2O3 and the rest MgO.
[0120] Chromium-free composite material performance test
[0121] Ten different chromium-free composite materials were prepared using the methods of the control group, Example 2, Example 7, Example 8 and Experimental Groups 1 to 4, and the properties of the prepared chromium-free composite materials were tested. The specific test results are shown in Table 1.
[0122] Table 1: Performance test table of 9 different chromium-free composite materials
[0123]
[0124]
[0125] The following conclusions can be drawn from the data in Table 1:
[0126] 1. Investigate the effect of adding auxiliary materials in the preparation of anti-corrosion layer on the performance of the prepared chromium-free composite material.
[0127] Comparing the control group with Example 2, it can be seen that in the two groups of experiments, the various properties of Example 2 are significantly better than those of the control example. Adding auxiliary materials can enhance the comprehensive properties of the composite material, among which the compressive strength and thermal shock stability are significantly improved.
[0128] 2. Investigate the effects of different parameter ratios for preparing anti-corrosion layers on the performance of the prepared chromium-free composite materials.
[0129] When comparing the control group with Example 7 and Example 8, it can be seen that among the three groups of experiments, the control example has the best performance and the best parameter ratio, and Example 7 is better than Example 8.
[0130] 3. Investigate the effects of different parameter ratios of the first region components used in preparing the bonding layer 21 on the performance of the prepared chromium-free composite material.
[0131] When comparing the control group with experimental group 1 and experimental group 2, it can be seen that among the three groups of experiments, experimental group 2 has the best compressive strength and thermal shock stability performance, the control group has the largest density, and there is no obvious difference in other properties. When preparing chromium-free composite materials, the parameter ratio of experimental group 2 can be used preferentially.
[0132] 4. Investigate the effects of different parameter ratios for preparing the connecting layer 22 on the performance of the prepared chromium-free composite material.
[0133] When comparing the control group with experimental group 3 and experimental group 4, it can be seen that the thermal shock stability of the chromium-free composite material is optimal under the parameter ratio of the control group. Compared with experimental group 3 and experimental group 4, the comprehensive performance of experimental group 4 is better.
Claims
1. A method for preparing a chromium-free corrosion-resistant and refractory composite material for an RH refining furnace, characterized in that: The composite material prepared by the method comprises an anti-corrosion layer (1) and a bonding layer (2), wherein the bonding layer (2) comprises a bonding layer (21) and a connecting layer (22); the preparation method comprises the following steps: S1. Preparation of anti-corrosion layer (1): In terms of mass percentage, 10 to 14 wt% of MgO, 3 to 5 wt% of magnesium aluminate sol, 0.6 to 0.8 wt% of SiO2, 0.3 to 0.4 wt% of R2O and the balance of Al2O3 are mixed for 30 to 50 minutes to obtain an anti-corrosion layer blank, which is then pressed under a pressure of 100 to 300 MPa to obtain an anti-corrosion layer (1); the water content in the magnesium aluminate sol accounts for 1 to 2 wt% of the total weight of the magnesium aluminate sol; S2, preparing the bonding layer (2); S2-1, preparing a single bonding layer (21): Dividing the component concentration gradient regions of the bonding layer (21): starting from the contact surface between the anti-corrosion layer (1) and the bonding layer (21), and pointing to the edge of the bonding layer (21) away from the anti-corrosion layer (1), the bonding layer (21) is divided into four component concentration gradient regions: a first region, a second region, a third region, and a fourth region; pouring into the mold of the bonding layer (21) in sequence according to the four component concentration gradient regions, and pressing and molding under a pressure condition of 100 to 300 MPa to obtain the bonding layer (21); S2-2, preparing the connecting layer (22); S3. Preparation of composite materials: S3-1. Splicing and pressing composite materials According to design requirements, the anti-corrosion layer (1), the bonding layer (21) and the connecting layer (22) are spliced into an original blank, and the original blank is pressed and formed under a pressure of 300 to 400 MPa and then dried to obtain a composite blank; S3-2, sintered composite blank The composite blank is placed in a corundum tube furnace, fired at a temperature of 1600-1750°C for 3-5 hours, and then the furnace is stopped for insulation for 2-3 hours to obtain a composite material.
2. The method for preparing a chromium-free corrosion-resistant and refractory composite material for RH refining furnace according to claim 1, characterized in that: In the first region described in step S2, the following components are uniformly mixed according to mass percentage: Mix 50-70wt% Al2O3, 4-6wt% SiO2, 1-3wt% ZrO2, 0.5-1.5wt% La2O3, 1-2wt% CaO, 3-5wt% magnesium aluminate sol solution, 0.3-0.4wt% R2O, 1-2wt% Fe2O3 and the balance MgO; In the second region, the following components are uniformly mixed according to mass percentage: Mix 45-65wt% Al2O3, 3-5wt% SiO2, 1-3wt% ZrO2, 0.5-1.5wt% La2O3, 1-2wt% CaO, 2-4wt% magnesium aluminate sol solution, 0.2-0.3wt% R2O, 1-2wt% Fe2O3 and the balance MgO; In the third region, the following components are uniformly mixed according to mass percentage: Mix 40-60wt% Al2O3, 2-4wt% SiO2, 1-3wt% ZrO2, 0.5-1.5wt% La2O3, 1-2wt% CaO, 1-3wt% magnesium aluminate sol solution, 0.1-0.2wt% R2O, 1-2wt% Fe2O3 and the balance MgO; In the fourth region, the following components are uniformly mixed according to mass percentage: Mix 35-55wt% Al2O3, 4-6wt% SiO2, 1-3wt% ZrO2, 0.5-1.5wt% La2O3, 1-2wt% CaO, 1-2wt% Fe2O3 and the balance MgO.
3. The method for preparing a chromium-free corrosion-resistant and refractory composite material for RH refining furnace according to claim 2, characterized in that: In step S2-2, the preparation steps of the connecting layer (22) are: uniformly mixing the following components according to mass percentage: 42.5~62.5wt% Al2O3, 2~4wt% SiO2, 1~3wt% ZrO2, 0.5~1.5wt% La2O3, 1~2wt% CaO, 0.2~0.3wt% R2O, 1~2wt% Fe2O3, 3~7wt% ZnO, 2~4wt% HA and the remainder MgO.
4. The method for preparing a chromium-free corrosion-resistant and refractory composite material for a RH refining furnace according to claim 1, characterized in that: The Al2O3 in step S1 includes three particle sizes: 3-5 mm, 1-3 mm, and 0-1 mm, and the ratio of the three particle sizes is 1:7:5; the particle size of the MgO is 0-1 mm.
5. The method for preparing a chromium-free corrosion-resistant and refractory composite material for RH refining furnace according to claim 1, characterized in that: Step S1: The anti-corrosion layer blank also includes auxiliary materials accounting for 5 to 10 wt% of the anti-corrosion layer blank; the preparation method of the auxiliary materials is: 0.1 to 0.3 wt% of Na2O, 0.1 to 0.2 wt% of Fe2O3 and the remainder of CaO are uniformly mixed and powdered to obtain a first powder, a binder accounting for 5 to 10% of the mass ratio of the first powder is added and mixed for 5 to 9 minutes, and the same dose of binder is added to the first powder for a second time to obtain the auxiliary materials.
6. The method for preparing a chromium-free corrosion-resistant and refractory composite material for RH refining furnace according to claim 5, characterized in that: The preparation method of the auxiliary material is as follows: dry mixing and grinding for 2 to 3 hours at a speed of 200 to 300 r / min on a planetary ball mill.
7. The method for preparing a chromium-free corrosion-resistant and refractory composite material for RH refining furnace according to claim 5, characterized in that: The particle sizes of Fe2O3, CaO and Na2O include three types: 1-3mm, 0-1mm and 200 mesh fine powder, and the proportions of the three particle sizes are 1:5:
2.
8. The method for preparing a chromium-free corrosion-resistant and refractory composite material for RH refining furnace according to claim 5, characterized in that: The binder is pulp waste liquid, the particle size of the first powder includes two types: 1-3 mm and 0-1 mm, and the particle size of the powder of the secondary feed is 200 meshes.
Citation Information
Patent Citations
Composite refractory material for RH refining furnace and preparation method thereof
CN116655360A
Multilayer sintered ceramic body
CN116867752A
Surface coated cutting tool excellent in deposition chipping resistance and peeling resistance
JP2018024038A
Composite materials and methods for making the same
US5580643A
Refractories for applications in combustion chambers intended for producing energy and / or waste disposal