Coated particles and their preparation methods, separators and batteries
By coating conductive particles with a thermally responsive insulating film onto a lithium-ion battery separator, the problem of insufficient temperature resistance of lithium-ion battery separators is solved by utilizing the exposure of conductive particles at high temperatures to form an electronic conductive network and the thermal response characteristics of polymer components, thus achieving high-temperature safety and stability of the battery.
Patent Information
- Application Number
- CN202211102980.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-09-09
AI Technical Summary
The existing lithium-ion battery separators have insufficient temperature resistance, which makes them prone to internal short circuits during thermal runaway. Current technologies to improve the temperature resistance of the separators cannot effectively prevent thermal runaway.
Conductive particles are coated with a thermally responsive insulating film. When exposed at high temperatures, these particles form an electronic conductive network, enabling self-discharge. By combining the thermal response characteristics of different polymer components, lithium-ion transport channels and gaseous material shuttles are controlled at different temperatures, thereby improving battery safety.
Under normal conditions, the battery maintains normal operation. At high temperatures, it reduces the state of charge through micro-short circuits and self-discharge, suppresses thermal runaway, and improves battery safety and stability.
Smart Images

Figure CN117691302B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery technology, and in particular to a coated particle and its preparation method, a separator and a battery. Background Technology
[0002] In lithium-ion batteries, the separator is used to separate the positive and negative electrodes. Because it does not contain any groups that participate in electrochemical reactions, it is generally considered an inert element in the battery, serving only a separating function. The separator itself is electrically insulating and also has micropores that allow electrolyte ions in the electrolyte to pass through, thus exhibiting ion-conducting properties.
[0003] As a key component of power batteries, the separator's primary function is to ensure battery safety. Currently, power batteries generally use microporous membranes made of polyolefin materials, mainly polyethylene (PE) and polypropylene (PP) separators. These separators suffer from insufficient temperature resistance and are prone to shrinkage, which are weaknesses in battery safety. In the process of thermal runaway, separator shrinkage leading to internal short circuits is one of the key factors.
[0004] To address the temperature resistance issues of polyolefin separators, existing technologies mainly focus on simply improving the temperature resistance of the separator: (1) constructing a temperature-resistant coating on the surface of the polyolefin separator; (2) preparing a temperature-resistant non-polyolefin-based separator. However, simply improving the temperature resistance of the separator cannot effectively prevent the occurrence of battery thermal runaway.
[0005] Therefore, improving battery safety has become a technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0006] The technical problem solved by the embodiments of the present invention is how to improve battery safety.
[0007] To address the above problems, embodiments of the present invention provide a coated particle, comprising: conductive particles;
[0008] A thermally responsive insulating film is used to coat the conductive particles. When the temperature is greater than 60°C, the thermally responsive insulating film deforms so that at least a portion of the surface of the conductive particles can be exposed.
[0009] Optionally, the thermally responsive insulating film comprises a first polymer component and a second polymer component, wherein the temperature resistance of the second polymer component is greater than that of the first polymer component.
[0010] Optionally, the material of the thermally responsive insulating film includes at least one of polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, styrene-butadiene rubber, polyamide-imide, polyethersulfone, polyphenylene sulfide, polyvinyl chloride, polyamic acid, poly(m-phenylene isophthalamide), poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene.
[0011] Optionally, the particle size of the conductive particles ranges from 0.01 μm to 3 μm.
[0012] Optionally, the conductive particles are selected from at least one of carbon black, graphene, carbon nanotubes, nickel, cobalt, manganese, zinc, tin, copper, and aluminum.
[0013] Optionally, the conductive particles can be coated onto the thermally responsive insulating film by methods including atomization drying, ball milling, surface grafting, or interfacial polymerization.
[0014] To address the above problems, embodiments of the present invention provide a method for preparing coated particles, comprising:
[0015] Conductive particles are dispersed in a liquid phase to prepare a uniform coating solution, and the coating solution is atomized and dried at a temperature of 60℃ to 250℃ to obtain coated particles containing a thermally responsive insulating film.
[0016] Optionally, the liquid phase contains at least one of the following: polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, styrene-butadiene rubber, polyamide-imide, polyethersulfone, polyphenylene sulfide, polyvinyl chloride, polyamic acid, poly(m-phenylene isophthalamide), poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene.
[0017] Optionally, the liquid phase includes a first liquid phase and a second liquid phase, wherein the polymer component of the second liquid phase has a higher temperature resistance than the polymer component of the first liquid phase.
[0018] Optionally, the solvent of the liquid phase is selected from at least one of water, ethanol, methanol, 1,4-dioxane, toluene, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, 1,2-dichloroethane, chloroform, tetrahydrofuran, acetone, and ethyl acetate.
[0019] To address the aforementioned problems, embodiments of the present invention provide a diaphragm comprising the aforementioned coated particles.
[0020] To address the aforementioned problems, embodiments of the present invention provide a diaphragm, comprising a base membrane and the aforementioned coated particles, wherein the coated particles are uniformly distributed on one or both sides of the surface of the base membrane.
[0021] Optionally, the diaphragm is prepared by the following steps:
[0022] (1) Disperse the coated particles in the third liquid phase to prepare a uniform third mixture;
[0023] (2) The third mixture is loaded onto one or both sides of the base membrane and dried at a temperature of 40°C to 150°C to obtain the diaphragm.
[0024] Optionally, the third liquid phase contains at least one of polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, and styrene-butadiene rubber latex.
[0025] Optionally, the base film is prepared by the following steps:
[0026] 1) Spread the film-forming solution evenly into a liquid film with a thickness of 10μm to 400μm;
[0027] 2) Place the liquid film in a coagulation bath for 0.1 h to 30 h to obtain a solid film;
[0028] 3) The solid film is subjected to thermosetting treatment at a temperature of 150℃~450℃ to obtain the base film.
[0029] Optionally, the film-forming solution contains at least one of polyvinyl chloride, polyethersulfone, polyamic acid, poly(m-phenylene isophthalamide), poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene.
[0030] Optionally, the solvent of the third liquid phase is selected from at least one of water, ethanol, methanol, 1,4-dioxane, toluene, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, 1,2-dichloroethane, chloroform, tetrahydrofuran, acetone, and ethyl acetate.
[0031] Optionally, the thickness of the diaphragm is 5 μm to 20 μm.
[0032] To address the aforementioned problems, embodiments of the present invention also provide a battery comprising the aforementioned separator.
[0033] Compared with the prior art, the technical solution of the embodiments of the present invention has the following advantages:
[0034] The coated particles provided in this invention have a thermally responsive insulating film covering the surface of conductive particles, separating adjacent conductive particles so that they do not contact each other. When the temperature rises to near the melting point of the thermally responsive insulating film, the polymer structure in the film changes, causing it to contract and expose at least some conductive particles. Utilizing this characteristic, when the coated particles are loaded onto a base film or formed separately and applied to a battery, at temperatures above 60°C (a high-temperature operating environment for batteries), the conductive particles expose the surface of the thermally responsive insulating film, allowing at least some adjacent conductive particles to contact each other. This contact forms a continuous conductive network, enabling electrons to transfer between the positive and negative electrodes, thus preventing micro-short circuits and self-discharge in the battery.
[0035] It can be seen that when the coated particles are loaded onto the base film or used alone as a battery separator, the battery separator can perform its basic functions under normal conditions, ensuring the normal operation of the battery. On the other hand, as the temperature rises and the battery tends to experience thermal runaway, the coated particles on the surface of the separator can expose the surface of the thermally responsive insulating film, increasing the electronic conductivity of the separator. This causes uniform micro-short circuits and self-discharge in the battery, reduces the battery's state of charge, releases the battery's electrochemical energy, and improves the thermal stability of the electrode materials. This helps to delay the occurrence of thermal crosstalk caused by gaseous substances shuttling between the positive and negative electrodes at high temperatures, thereby suppressing thermal runaway and improving battery safety.
[0036] Furthermore, in the coated particles provided in this embodiment of the invention, the thermally responsive insulating film comprises a first polymer component and a second polymer component, wherein the temperature resistance of the second polymer component is greater than that of the first polymer component. When the temperature is greater than 60°C, the thermally responsive insulating film formed by the first polymer component first undergoes thermal contraction and movement, causing the conductive particles to be exposed on the surface of the thermally responsive insulating film; as the temperature further increases, the thermally responsive insulating film formed by the second polymer component begins to undergo thermal contraction and movement until it reaches a viscous flow state.
[0037] Utilizing this characteristic, when the coated particles are loaded onto a base film or formed into a film alone for use in batteries, due to the different temperature resistances of the first and second polymer components, as the battery temperature rises, when the temperature is below the melting point of the second polymer component, the conductive particles coated by the first polymer component come into contact with each other, forming an electronic conductive network. When the temperature approaches the melting point of the second polymer component, the thermally responsive insulating film formed by the second polymer component begins to contract until it reaches a viscous flow state. The molten second polymer component blocks the lithium-ion transport channels of the battery, causing a significant decrease in the porosity of the separator. This effectively prevents gaseous substances from shuttling between the positive and negative electrodes, thereby further suppressing the occurrence of battery thermal runaway and increasing battery safety. As can be seen, the coated particles provided in the embodiments of the present invention, on the one hand, the presence of the second polymer component can control the degree of exposure of conductive particles in the coated particles, control the self-discharge rate of the battery, prevent excessively severe internal short circuits in the battery, and avoid safety hazards caused by sudden and violent heat release of the battery; on the other hand, by controlling the self-discharge of the battery through the first polymer component, the state of charge of the positive and negative electrodes of the battery is reduced, the stability of the positive and negative electrodes is improved, and it is beneficial to delay the occurrence of thermal crosstalk caused by gaseous substances shuttling between the positive and negative electrodes at high temperatures, while reducing the amount and intensity of thermal crosstalk reaction. Attached Figure Description
[0038] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of this application. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0039] Figure 1 This is a scanning electron microscope image of coated particles provided in an embodiment of the present invention. Detailed Implementation
[0040] As can be seen from the background technology, simply improving the temperature resistance of the separator cannot effectively prevent the occurrence of battery thermal runaway.
[0041] Analysis revealed that under heating conditions, the positive electrode of the battery releases reactive oxygen species, while the negative electrode releases strong reducing gases such as hydrogen, methane, and ethylene. These gases can cross between the positive and negative electrodes, triggering exothermic reactions and causing thermal runaway. Even with a highly temperature-resistant separator, gases can still penetrate the micropores of the separator, creating crosstalk. Therefore, simply improving the temperature resistance of the separator cannot prevent thermal runaway. Current solutions for improving battery safety focus only on enhancing the temperature resistance of the separator, neglecting the importance of preventing thermal crosstalk reactions. Consequently, battery safety issues remain prominent.
[0042] To address the above problems, embodiments of the present invention provide a coated particle, comprising:
[0043] Conductive particles;
[0044] A thermally responsive insulating film is used to coat the conductive particles. When the temperature is greater than 60°C, the thermally responsive insulating film deforms so that at least a portion of the surface of the conductive particles can be exposed.
[0045] It should be noted that the thermally responsive insulating film mentioned in this article refers to a film with an electronic conductivity of 10. -10 Polymer films with a strength of S / m or less, and thermally responsive insulating films are made of materials including crystalline polymers and amorphous polymers. The polymers can be either homopolymers or block copolymers.
[0046] It should be noted that when the temperature exceeds 60°C, the thermally responsive insulating film deforms, exposing at least a portion of the surface of the conductive particles. This means that after the coated particles are assembled into a battery, when the battery temperature rises above 60°C, the structure of the thermally responsive insulating film changes, and the thermal contraction causes some of the conductive particles' surfaces to be exposed. The degree to which the conductive particles expose the thermally responsive insulating film is related to the battery temperature and the melting or softening point of the thermally responsive insulating film material.
[0047] It is readily understood by those skilled in the art that when the coated particles are assembled into a battery, due to the battery's weight and the application of external pressure, at least some of the conductive particles exposed on the surface of the thermally responsive insulating film will come into contact with each other, thereby connecting the positive and negative electrodes. The ability of at least some adjacent conductive particles to come into contact means that when the structure of the thermally responsive insulating film changes under temperature rise, the conductive particles can come into contact with each other in any local area on the electrode cross-section, as long as the electronic conductive network formed by the contacting conductive particles can conduct electricity to the positive and negative electrodes. It is also readily understood that because the thermally responsive insulating film loosely coats the conductive particles, although the conductive particles are in contact with each other, gaps will exist between them, which can serve as lithium-ion transport channels.
[0048] Specifically, the melting point of the thermally responsive insulating film is greater than 60°C. The material of the thermally responsive insulating film can be selected from at least one of polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, styrene-butadiene rubber, polyamide-imide, polyethersulfone, polyphenylene sulfide, polyvinyl chloride, polyamic acid, poly(m-phenylene isophthalamide), poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene.
[0049] It should be noted that the melting point of the polymer materials described in this article indicates the state before the polymer molecular chains begin to move and have reached a molten state. During the preparation of the coated particles, residual stress exists due to the stretching of the thermally responsive insulating film. As the temperature rises, this stress is released, resulting in significant contraction. At this point, the temperature is close to the melting point but has not yet reached the melting temperature. It is easy to understand that when the temperature reaches the polymer's melting point, the polymer is already in a fully flowing viscous state. Therefore, as the temperature rises, near the melting point, the small molecules begin to flow, and the thermally responsive insulating film as a whole exhibits good plasticity and can deform.
[0050] In one embodiment, the thermally responsive insulating film is a first polymer with a melting point of 60°C-150°C. When the coated particles containing the thermally responsive insulating film are loaded onto a base film or formed into a film alone and applied to a battery, as the battery temperature rises, the conductive particles coated with the first polymer are exposed on the surface of the thermally responsive film. A conductive network is formed between the contacting conductive particles, allowing electrons to be transferred between the positive and negative electrodes, thus achieving self-discharge. This characteristic can improve the stability of the positive and negative electrodes, help delay the occurrence of thermal crosstalk caused by gaseous substances shuttling between the positive and negative electrodes, and increase the safety of battery use.
[0051] In another embodiment, the thermally responsive insulating film may be simply a second polymer with a melting point greater than 150°C. When the coated particles containing this thermally responsive insulating film are loaded onto a base film or formed into a film alone and applied to a battery, when the temperature approaches the melting point of the second polymer, the thermally responsive insulating film formed by the second polymer begins to contract. The molten second polymer blocks the lithium-ion transport channels of the battery, causing a significant decrease in the porosity of the separator. The lithium-ion transport channels of the battery are blocked, thereby preventing gaseous substances from shuttling between the positive and negative terminals, stopping the battery from discharging, and ensuring the safety of the battery at high temperatures.
[0052] The first polymer and / or the second polymer may be selected from at least one of polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, styrene-butadiene rubber, polyamide-imide, polyethersulfone, polyphenylene sulfide, polyvinyl chloride, polyamic acid, poly(m-phenylene isophthalamide), poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene. If the thermally responsive insulating film is made of multiple materials, the shrinkage movement of the thermally responsive insulating film within different temperature ranges can be controlled by adjusting the proportions of the various materials.
[0053] In another specific embodiment, when the material of the thermally responsive insulating film is a block copolymer material, the molecular chain of the polymer material of the thermally responsive insulating film may include a first flexible segment and a second flexible segment, wherein the temperature resistance of the second flexible segment is greater than that of the first flexible segment. For example, the block polymer may include both a first flexible segment with a melting point of 60°C-150°C and a second flexible segment with a melting point greater than 150°C. As the battery temperature gradually increases, microphase separation occurs in the block copolymer. When the temperature is between 60℃ and 150℃, the thermally responsive insulating film containing the first flexible segment contracts, causing conductive particles to contact and form an electronic conductive network. This increases the electronic conductivity of the separator, enabling uniform micro-short circuits and self-discharge, reducing the battery's state of charge, and releasing the battery's electrochemical energy. This effectively suppresses thermal runaway and improves battery safety. When the temperature exceeds 150℃, the thermally responsive insulating film containing the second flexible segment contracts and melts as the temperature continues to rise. This causes the block polymer to become viscous, blocking the gaps between adjacent conductive particles and obstructing lithium-ion transport channels. This significantly reduces the porosity of the separator, blocking the battery's lithium-ion transport channels and stopping the battery from discharging, thus ensuring battery safety at high temperatures.
[0054] The conductive particles may be selected from at least one of carbon black, carbon nanotubes, graphene, nickel, cobalt, manganese, zinc, tin, copper, and aluminum.
[0055] It is easy to understand that the particle size of the conductive particles should not be too large or too small. If the particle size is too large, on the one hand, the conductive particles will cause the membrane to be too thick when coated on it; on the other hand, if the particle size is too large, the irregular conductive particles can easily puncture the membrane. If the particle size is too large, the gaps between the conductive particles will be too large, making it difficult to form suitable gaps for lithium-ion transport. If the particle size is too small, it will be difficult to coat the particles. Moreover, after the conductive particles form an electronic conductive network, the gaps between the contacting conductive particles still need to provide lithium-ion transport channels. If the conductive particles are too dense, the gaps between them will be too small, which may block the ion channels. Therefore, in one specific embodiment, the particle size range of the conductive particles can be 0.01μm-3μm. For example, 0.05μm, 0.1μm, 1μm, 2μm, 2.5μm, etc.
[0056] In one specific embodiment, to obtain coated particles with better coating uniformity and improve the porosity of the conductive particles coated on the thermally responsive film, the conductive particles can be coated onto the thermally responsive insulating film by atomization drying. Of course, in other embodiments, the method of coating the conductive particles onto the thermally responsive insulating film may also include ball milling, surface grafting, or interfacial polymerization.
[0057] The coated particles provided in this invention have a thermally responsive insulating film coating the surface of conductive particles. The thermally responsive insulating film separates adjacent conductive particles, preventing them from contacting each other. When the temperature rises to near the melting point of the thermally responsive insulating film, the polymer structure in the film changes, causing it to contract and expose the conductive particles. At least some adjacent conductive particles can then contact each other. Utilizing this characteristic, when the coated particles are loaded onto a base film or formed independently and applied to a battery, at temperatures above 60°C, the contact between the conductive particles forms a continuous electronic conductive network, allowing electrons to transfer between the positive and negative electrodes, thus achieving self-discharge.
[0058] It can be seen that when the coated particles are loaded onto the base film or used alone as a battery separator, the battery separator can perform its basic functions under normal conditions, ensuring the normal operation of the battery. On the other hand, as the temperature rises and the battery tends to experience thermal runaway, the coated particles on the surface of the separator can expose the surface of the thermally responsive insulating film, increasing the electronic conductivity of the separator. This causes uniform micro-short circuits and self-discharge in the battery, reduces the battery's state of charge, and releases the battery's electrochemical energy. This helps to delay the occurrence of thermal crosstalk caused by gaseous substances shuttling between the positive and negative electrodes at high temperatures, thereby suppressing thermal runaway and improving battery safety.
[0059] In one specific embodiment, the thermally responsive insulating film may comprise a first polymer component. Specifically, the first polymer component may be selected from at least one of polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, styrene-butadiene rubber, polyamide-imide, polyethersulfone, and polyphenylene sulfide.
[0060] When the temperature exceeds 60°C, the molecular chains of the first polymer component begin to move. Utilizing this property, when the coated particles are loaded onto a base film or formed into a film alone for use in a battery, as the battery temperature rises, the conductive particles coated with the first polymer come into contact with each other, forming an electronic conductive network. This is equivalent to connecting the positive and negative electrodes of the battery, allowing electrons to transfer between them and achieving self-discharge. This characteristic improves the stability of the positive and negative electrodes and helps to delay thermal crosstalk caused by gaseous substances shuttling between the positive and negative electrodes.
[0061] In one specific embodiment, in order to control the rate of battery self-discharge, prevent excessively severe internal short circuits in the battery, and avoid safety hazards caused by sudden and intense heat release, the thermally responsive insulating film may further include a first polymer component and a second polymer component, wherein the temperature resistance of the second polymer component is greater than that of the first polymer component.
[0062] It should be explained that the temperature resistance of the second polymer component is greater than that of the first polymer component. This means that as the temperature rises, when the first polymer component undergoes structural deformation due to heat at a certain temperature, the structure of the second polymer component does not change at that temperature.
[0063] Specifically, the second polymer component may be selected from at least one of polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, styrene-butadiene rubber, polyamide-imide, polyethersulfone, and polyphenylene sulfide.
[0064] Of course, in order to improve the strength of the thermally responsive insulating film, in another embodiment, the second polymer material may also be selected from at least one of polyvinyl chloride, polyethersulfone, polyamic acid, poly(m-phenylene isophthalamide), poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene.
[0065] When the temperature is above 60°C, the thermally responsive insulating film formed by the first polymer component first undergoes thermal contraction and movement, causing the conductive particles to be exposed on the surface of the thermally responsive insulating film; as the temperature further increases, the thermally responsive insulating film formed by the second polymer component begins to undergo thermal contraction and movement until it becomes viscous.
[0066] Utilizing this characteristic, when the coated particles are loaded onto a base film or formed into a film alone for use in batteries, due to the different temperature resistances of the first and second polymer components, as the battery temperature rises, when the temperature is below the melting point of the second polymer component, the conductive particles coated by the first polymer component come into contact with each other, forming an electronic conductive network. When the temperature approaches the melting point of the second polymer component, the thermally responsive insulating film formed by the second polymer component begins to contract until it reaches a viscous flow state. The molten second polymer component blocks the lithium-ion transport channels of the battery, significantly reducing the porosity of the separator. This effectively prevents gaseous substances from shuttling between the positive and negative electrodes, thereby further suppressing the occurrence of battery thermal runaway and increasing battery safety. As can be seen, the coated particles provided in the embodiments of the present invention, on the one hand, the presence of the second polymer component can control the degree of exposure of conductive particles in the coated particles, control the self-discharge rate of the battery, prevent excessively severe internal short circuits in the battery, and avoid safety hazards caused by sudden and violent heat release of the battery; on the other hand, by controlling the self-discharge of the battery through the first polymer component, the state of charge of the positive and negative electrodes of the battery is reduced, the stability of the positive and negative electrodes is improved, and it is beneficial to delay the occurrence of thermal crosstalk caused by gaseous substances shuttling between the positive and negative electrodes at high temperatures, while reducing the amount and intensity of thermal crosstalk reaction.
[0067] To address the above problems, embodiments of the present invention also provide a method for preparing coated particles, comprising:
[0068] Conductive particles are dispersed in a liquid phase to prepare a uniform coating solution, and the coating solution is atomized and dried at a temperature of 60℃ to 250℃ to obtain coated particles containing a thermally responsive insulating film.
[0069] In one specific embodiment, the liquid phase contains at least one of the following: polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, styrene-butadiene rubber latex, polyamide-imide, polyethersulfone, polyphenylene sulfide, polyvinyl chloride, polyamic acid, poly(m-phenylene isophthalamide), poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene.
[0070] In one specific embodiment, the solvent of the liquid phase is selected from at least one of water, ethanol, methanol, 1,4-dioxane, toluene, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, 1,2-dichloroethane, chloroform, tetrahydrofuran, acetone, and ethyl acetate.
[0071] In one specific embodiment, in order to improve the temperature resistance of the coated particles, the liquid phase may include a first liquid phase and a second liquid phase, wherein the polymer component of the second liquid phase has a higher temperature resistance than the polymer component of the first liquid phase.
[0072] Specifically, the step of obtaining coated particles containing a thermally responsive insulating film includes:
[0073] 1) Disperse the conductive particles in the first liquid phase to prepare a uniform first mixture;
[0074] 2) The first mixed solution is atomized and dried at a temperature of 60–150°C to obtain primary coated particles containing the first film layer;
[0075] 3) Disperse the primary coated particles in the second liquid phase to prepare a homogeneous second mixture;
[0076] 4) The second mixture is atomized and dried at a temperature of 120–250 degrees Celsius to obtain secondary coated particles containing the first and second membrane layers.
[0077] Of course, in other embodiments, the coated particles can also be obtained by dispersing the conductive particles in a mixed solution of the first liquid phase and the second liquid phase.
[0078] In one specific embodiment, the first liquid phase or the second liquid phase contains at least one of polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, and styrene-butadiene rubber latex.
[0079] In one embodiment, the second liquid phase may further contain at least one of polyvinyl chloride, polyethersulfone, polyamic acid, poly(m-phenylene isophthalamide), poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene.
[0080] In one specific embodiment, the solvent of the first liquid phase or the second liquid phase is selected from at least one of water, ethanol, methanol, 1,4-dioxane, toluene, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, 1,2-dichloroethane, chloroform, tetrahydrofuran, acetone, and ethyl acetate.
[0081] The coated particles prepared using the method provided in this invention can avoid simultaneously coating the base film when coating conductive particles, thereby improving the coating effect. Because atomized drying is used, the coated particles are in a rotating state with the airflow in the equipment, making it easier to form spherical particles. The particle morphology and size distribution are easier to control, resulting in better coating uniformity. The thermally responsive insulating layer can be more loosely coated, retaining some voids and pores to provide channels for lithium-ion transport.
[0082] To address the aforementioned problems, this invention also provides a diaphragm comprising the aforementioned coated particles, wherein the coated particles are dispersed in a film-forming solution to obtain a solid membrane, which is then subjected to thermosetting treatment to obtain the diaphragm.
[0083] In one embodiment, the film-forming solution may be selected from at least one of polyvinyl chloride, polyethersulfone, polyamic acid, poly(m-phenylene isophthalamide), aqueous emulsion of styrene-butadiene rubber, poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene.
[0084] To address the aforementioned issues, embodiments of the present invention also provide a diaphragm, comprising a base membrane and the aforementioned coated particles, wherein the coated particles are uniformly distributed on one or both surfaces of the base membrane.
[0085] It should be noted that the coated particles can also be used alone as a separator. Of course, to further improve the separator strength, in one specific embodiment, the thermally responsive insulating film can be used in combination with the base film.
[0086] In one embodiment, the membrane has a strength of 70 MPa to 180 MPa, a porosity of 30% to 65%, an air permeability of 100 s to 350 s, and an electronic conductivity of 10. -10 ~10 -18 S / cm.
[0087] It is easy to understand that the separator cannot be too thick or too thin. If the separator is too thick, it will increase the cost of the separator and the internal resistance of the battery. An excessively thick separator will also occupy the space of other electrochemically active substances, leading to a decrease in energy density. If the separator is too thin, on the one hand, it cannot effectively block the positive and negative electrodes, and on the other hand, it may result in an insufficient load of conductive particles, which is not conducive to self-discharge. Therefore, in a specific embodiment, the thickness of the separator can be 5μm to 20μm, specifically, it can be 7μm, 10μm, 15μm, etc.
[0088] In one specific embodiment, the diaphragm can be prepared by the following steps:
[0089] (1) Disperse the coated particles in the third liquid phase to prepare a uniform third mixture;
[0090] (2) The third mixture is loaded onto one or both sides of the base membrane and dried at a temperature of 40°C to 150°C to obtain the diaphragm.
[0091] The third liquid phase may contain at least one of polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, and styrene-butadiene rubber latex.
[0092] The base film can be prepared by the following steps:
[0093] 1) Spread the film-forming solution evenly into a liquid film with a thickness of 10μm to 400μm;
[0094] 2) Place the liquid film in a coagulation bath for 0.1 h to 30 h to obtain a solid film;
[0095] 3) The solid film is subjected to thermosetting treatment at a temperature of 150℃~450℃ to obtain the base film.
[0096] In one specific embodiment, the film-forming solution may contain at least one of polyvinyl chloride, polyethersulfone, polyamic acid, poly(m-phenylene isophthalamide), poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene.
[0097] In one specific embodiment, the solvent of the third liquid phase is selected from at least one of water, ethanol, methanol, 1,4-dioxane, toluene, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, 1,2-dichloroethane, chloroform, tetrahydrofuran, acetone, and ethyl acetate.
[0098] When the separator provided in this embodiment of the invention is applied to a battery by loading the coated particles onto a base film or forming a separate film, the polymer structure in the thermally responsive insulating film used to coat the conductive particles changes when the temperature is ≥60°C. The thermally responsive insulating film shrinks and moves due to heat, causing the conductive particles to be exposed on the surface of the thermally responsive insulating film. Under the action of the battery electrode's own weight, the conductive particles come into contact with each other to form a continuous electronic conductive network, so that electrons can be transferred between the positive and negative electrodes, realizing self-discharge.
[0099] As can be seen, the separator provided in this embodiment of the invention can, on the one hand, perform its basic function under normal conditions to ensure the normal operation of the battery; on the other hand, as the temperature rises, when the battery tends to experience thermal runaway, the conductive particles on the surface of the separator can expose the surface of the thermally responsive insulating film, increasing the electronic conductivity of the separator, causing uniform micro-short circuits and self-discharge in the battery, reducing the battery's state of charge, releasing the battery's electrochemical energy, and helping to delay the occurrence of thermal crosstalk caused by gaseous substances shuttling between the positive and negative electrodes at high temperatures, thereby suppressing the occurrence of thermal runaway and improving battery safety.
[0100] To address the aforementioned problems, embodiments of the present invention provide a battery comprising the aforementioned separator.
[0101] The battery provided in this embodiment of the invention, because it includes the aforementioned separator, can ensure the normal operation of the battery under normal conditions. On the other hand, as the temperature rises, when the battery tends to experience thermal runaway, the conductive particles on the surface of the separator can expose the surface of the thermally responsive insulating film, increasing the electronic conductivity of the separator. This causes the battery to experience uniform micro-short circuits and self-discharge, reduces the battery's state of charge, and releases the battery's electrochemical energy. This helps to delay the occurrence of thermal crosstalk caused by gaseous substances shuttling between the positive and negative electrodes at high temperatures, thereby suppressing the occurrence of thermal runaway and improving battery safety.
[0102] The coated particles, their preparation method, separator, and battery of the present invention will be further described in detail below with reference to specific embodiments and comparative examples.
[0103] Example 1
[0104] The coated particles are prepared by the following steps:
[0105] 1) Disperse conductive particles (a mixture of carbon black and carbon nanotubes (mass ratio 3 / 1)) in a tetrahydrofuran solution of polyethylene oxide (mass ratio of conductive particles to polyethylene oxide is 7 / 3), with a solid content of 5%, and stir at 30°C for 24 hours to prepare a uniform first mixture.
[0106] 2) Spray dry the first mixture at 65℃ (flow rate 15ml / min~35ml / min) to obtain primary coated particles containing the first shell layer;
[0107] 3) Disperse the primary particles in a polyvinylidene fluoride N-methylpyrrolidone solution (8wt%) (the mass ratio of primary particles to polyvinylidene fluoride is 8 / 2) to prepare a homogeneous second mixture;
[0108] 4) Spray dry the second mixture at a temperature of 125°C (flow rate 15ml / min~35ml / min) to obtain secondary coated particles containing a second shell, thus producing coated particles.
[0109] Electron microscopy was performed on the coated particles of Example 1, see... Figure 1 .according to Figure 1 It can be seen that the coated particles are spherical in shape, and the particle size of the conductive particles is about 0.4μm.
[0110] The base film is prepared by the following steps:
[0111] 1) Polyamic acid and poly(m-phenylene isophthalamide) (mass ratio 3 / 1) were dissolved in a mixed solution of N-methylpyrrolidone and chloroform (volume ratio 5 / 1) with a solid content of 13.5%. The solution was stirred at 80°C for 24 hours to obtain a homogeneous solution. The solution was then coated into a liquid film with a thickness of 100 μm.
[0112] 2) Place the above liquid film in a coagulation bath (water / ethanol, volume ratio 4 / 1) for 0.5 h to obtain a solid film;
[0113] 3) The solid film was subjected to thermosetting treatment at temperatures of 60℃, 120℃, 180℃, 240℃ and 300℃ for 0.2h in sequence to obtain the base film.
[0114] The diaphragm is prepared by the following steps:
[0115] The secondary coated particles were dispersed in the third liquid phase (an aqueous solution of polyacrylic acid, 5 wt%), with a mass ratio of secondary coated particles to polyacrylic acid of 9 / 1, to prepare a homogeneous third mixture.
[0116] The third mixture was sprayed onto both sides of the base membrane and dried at 55°C to obtain the diaphragm sample.
[0117] The performance parameters of the diaphragm samples at room temperature (25℃) are shown in Table 1. The diaphragm samples were heat-treated at 60℃, 80℃, 150℃ and 180℃ for 1h, respectively. After heat treatment, the thickness, thermal shrinkage rate, porosity, air permeability and electronic conductivity of the diaphragm samples were measured. The performance parameters are shown in Table 1.
[0118] The method for testing heat shrinkage rate is as follows:
[0119] 1) Cut the diaphragm sample into a 2cm x 2cm square and place it between two glass slides;
[0120] 2) Place them in environments of 25℃, 60℃, 80℃, 150℃, and 180℃ respectively for 30 minutes, then remove them and observe their shape at room temperature;
[0121] 3) Calculate the area shrinkage rate of the sample before and after heat treatment.
[0122] Thickness, porosity, air permeability, and electronic conductivity were all tested using conventional instrumentation methods known to those skilled in the art, and will not be described in detail here.
[0123] Performance Test 1
[0124] 1) The separator sample from Example 1 was used as the separator for a soft-pack lithium-ion battery with a rated capacity of 5Ah (the positive electrode active material was LiNi). 0.8 Co 0.1 Mn 0.1 O2 (NCM811), with natural graphite as the negative electrode active material, the battery was charged to full charge (4.2V, 100% SOC) at 0.1C rate at 25℃.
[0125] 2) Place the fully charged batteries in environments of 25℃, 80℃, and 150℃ for 10 hours respectively, and monitor the voltage and temperature changes of the batteries. The changes are expressed in V... min and T max The values represent the lowest and highest voltages detected. The test results are shown in Table 2.
[0126] 3) After the battery has been left to stand, it was placed back in an environment of 25°C for 10 hours, and then its capacity retention rate R was tested at a rate of 0.1C. The test results are shown in Table 2.
[0127] Performance Test 2
[0128] 1) The separator sample from Example 1 was used as the separator for a soft-pack lithium-ion battery with a rated capacity of 5Ah (the positive electrode active material was LiNi). 0.8 Co 0.1 Mn 0.1 O2 (NCM811), with natural graphite as the negative electrode active material, the battery was charged to full charge (4.2V, 100% SOC) at 0.1C rate at 25℃.
[0129] 2) Place the fully charged battery in an accelerating calorimeter and test it within a temperature range from room temperature to 220°C, monitoring the changes in battery voltage and temperature, expressed in V. min and T max The values represent the lowest and highest monitored voltages, with rmax representing the maximum rate of temperature rise of the battery. The test results are shown in Table 3.
[0130] Example 2
[0131] The coated particles are prepared by the following steps:
[0132] 1) Disperse conductive particles (a mixture of carbon black and carbon nanotubes (mass ratio 3 / 1)) in a tetrahydrofuran solution of polyethyleneimine (mass ratio of conductive particles to polyethyleneimine is 8 / 2), with a solid content of 7%, and stir at 30°C for 24 hours to prepare a uniform first mixture.
[0133] 2) Spray dry the first mixture at a temperature of 65℃ (flow rate 15ml / min~35ml / min) to obtain primary coated particles.
[0134] The base film is prepared by the following steps:
[0135] 1) Polyamic acid and poly(m-phenylene isophthalamide) (mass ratio 3 / 1) were dissolved in a mixed solution of N-methylpyrrolidone and chloroform (volume ratio 5 / 1) with a solid content of 13.5%. The solution was stirred at 80°C for 24 hours to obtain a homogeneous solution. The solution was then coated into a liquid film with a thickness of 100 μm.
[0136] 2) Place the above liquid film in a coagulation bath (water / ethanol, volume ratio 4 / 1) for 0.5 h to obtain a solid film;
[0137] 3) The solid film was subjected to thermosetting treatment at temperatures of 60℃, 120℃, 180℃, 240℃ and 300℃ for 0.2h in sequence to obtain the base film.
[0138] The diaphragm is prepared by the following steps:
[0139] 1) Disperse the primary coated particles in the second liquid phase (aqueous solution of carboxymethyl cellulose, 2 wt%), with the mass ratio of primary coated particles to carboxymethyl cellulose being 8 / 2, to prepare a homogeneous second mixture;
[0140] 2) The second mixture is sprayed onto both sides of the base film and dried at 50°C to obtain the target sample. The performance parameters of the sample are shown in Table 1.
[0141] Performance testing
[0142] 1) The sample from Example 2 was used as the separator for a soft-pack lithium-ion battery with a rated capacity of 5Ah (the positive electrode active material was LiNi). 0.8 Co 0.1 Mn 0.1 O2 (NCM811), with natural graphite as the negative electrode active material, the battery was charged to full charge (4.2V, 100% SOC) at 0.1C rate at 25℃.
[0143] 2) Place the fully charged battery in an accelerating calorimeter and test it within a temperature range from room temperature to 220°C, monitoring the changes in battery voltage and temperature, expressed in V. min and T max Indicates the lowest and highest monitored voltages, expressed in r. max The maximum rate of temperature rise of the battery is indicated in Table 3. The test results are shown in Table 3.
[0144] Combining the data from Example 2 in Table 1 and the data from Example 2 in Table 3, it can be concluded that the performance data of the separator sample at room temperature is close to that of the comparative separator, indicating that the separator prepared by this invention can ensure the normal operation of the battery at room temperature. Furthermore, after the separator is assembled into a battery, the battery will not experience thermal runaway within a temperature range below 220°C, thereby effectively improving battery safety.
[0145] Example 3
[0146] The coated particles are prepared by the following steps:
[0147] 1) Disperse conductive particles (a mixture of carbon black and carbon nanotubes (mass ratio 3 / 1)) in a tetrahydrofuran solution of polymethyl methacrylate (mass ratio of conductive particles to polymethyl methacrylate is 7 / 3), with a solid content of 5%, and stir at 30°C for 24 hours to prepare a uniform first mixture.
[0148] 2) Spray dry the first mixture at a temperature of 75℃ (flow rate 15ml / min~35ml / min) to obtain primary coated particles containing the first shell layer.
[0149] The base film is prepared by the following steps:
[0150] 1) Dissolve poly(m-phenylene isophthalamide) in a mixed solution of N-methylpyrrolidone and chloroform (volume ratio 5 / 1) with a solid content of 14.5% and stir at 80°C for 24 hours to prepare a homogeneous solution. Then, coat the solution into a liquid film with a thickness of 100 μm.
[0151] 2) Place the above liquid film in a coagulation bath (water / ethanol, volume ratio 1 / 6) for 0.5 h to obtain a solid film;
[0152] 3) The solid film was subjected to thermosetting treatment at temperatures of 60℃, 120℃, 180℃, 240℃ and 300℃ for 0.2h in sequence to obtain the base film.
[0153] The battery separator is prepared by the following steps:
[0154] 1) Disperse the primary coated particles in the second liquid phase (aqueous solution of sodium alginate, 2wt%), with the mass ratio of primary coated particles to sodium alginate being 7 / 3, to prepare a homogeneous second mixture;
[0155] 2) The second mixture was sprayed onto both sides of the base film and dried at 60°C to obtain the target sample. The performance parameters of the sample are shown in Table 1.
[0156] Performance testing
[0157] 1) The sample from Example 3 was used as the separator for a soft-pack lithium-ion battery with a rated capacity of 5Ah (the positive electrode active material was LiNi). 0.8 Co 0.1 Mn 0.1 O2 (NCM811), with natural graphite as the negative electrode active material, the battery was charged to full charge (4.2V, 100% SOC) at 0.1C rate at 25℃.
[0158] 2) Place the fully charged battery in an accelerating calorimeter and test it within a temperature range from room temperature to 220°C, monitoring the changes in battery voltage and temperature, expressed in V. min and T maxIndicates the lowest and highest monitored voltages, expressed in r. max The maximum rate of temperature rise of the battery is indicated in Table 3. The test results are shown in Table 3.
[0159] Combining the data from Example 3 in Table 1 and Table 3, it can be concluded that the performance data of the separator sample at room temperature is close to that of the comparative separator, indicating that the separator prepared by this invention can ensure the normal operation of the battery at room temperature. Furthermore, after the separator is assembled into a battery, the battery will not experience thermal runaway within a temperature range below 220°C, thereby effectively improving battery safety.
[0160] Example 4
[0161] The coated particles are prepared by the following steps:
[0162] 1) Disperse conductive particles (a mixture of carbon black and carbon nanotubes (mass ratio 3 / 1)) in a tetrahydrofuran solution of polyamide imide (mass ratio of conductive particles to polyamide imide is 7 / 3), with a solid content of 5%, and stir at 30°C for 24 hours to prepare a uniform first mixture.
[0163] 2) Spray dry the first mixture at 65℃ (flow rate 15ml / min~35ml / min) to obtain primary coated particles containing the first shell layer;
[0164] 3) Disperse the primary particles in a polyoxypropylene N-methylpyrrolidone solution (8wt%) (the mass ratio of primary coated particles to polyoxypropylene is 7 / 3) to prepare a homogeneous second mixture;
[0165] 4) Spray dry the second mixture at a temperature of 125°C (flow rate 15-35 ml / min) to obtain secondary coated particles containing a second shell.
[0166] The base film is prepared by the following steps:
[0167] 1) Polysulfone was dissolved in a mixed solution of N-methylpyrrolidone and chloroform (volume ratio 6 / 1) with a solid content of 12.5%. The solution was stirred at 80°C for 24 hours to prepare a homogeneous solution. The solution was then coated into a liquid film with a thickness of 100 μm.
[0168] 2) Place the above liquid film in a coagulation bath (water / ethanol / ethylene glycol, volume ratio 1 / 6 / 1) for 0.5 h to obtain a solid film;
[0169] 3) The solid film was subjected to thermosetting treatment at temperatures of 60℃, 120℃, 180℃, 240℃ and 300℃ for 0.2h in sequence to obtain the base film.
[0170] The battery separator is prepared by the following steps:
[0171] 1) Disperse the secondary coated particles in the third liquid phase (aqueous solution of chitosan, 5 wt%), with the mass ratio of secondary coated particles to chitosan being 8.5 / 1.5, to prepare a uniform third mixture.
[0172] 2) The third mixture was sprayed onto both sides of the base film and dried at 65°C to obtain the target sample. The performance parameters of the sample at room temperature (25°C) are shown in Table 1.
[0173] The diaphragm samples were heat-treated at 80℃ and 150℃ for 1h, respectively. After heat treatment, the thickness, thermal shrinkage rate, porosity, air permeability and electronic conductivity of the diaphragm samples were measured. The performance parameters are shown in Table 1.
[0174] Based on the data in Example 4, it can be seen that:
[0175] 1) Under normal temperature conditions (below 60℃), the membrane thickness is 13μm, the porosity is 45%, the air permeability is 202s, and the electronic conductivity is less than 10. -10 S / cm can prevent battery self-discharge and ensure battery cycle performance and power performance under normal conditions.
[0176] 2) At 80℃, the membrane thickness is 13μm, the porosity is 36%, the air permeability is 517s, and the electronic conductivity is 0.0003~0.00001S / cm. The air permeability does not change much, indicating that the lithium-ion transport channels are still unobstructed. The increase in the electronic conductivity of the membrane causes uniform micro-short circuits and self-discharge in the battery, reducing the battery's state of charge and releasing the battery's electrochemical energy.
[0177] 3) At temperatures above 150℃, the membrane thickness is 12μm, the porosity is 2%, the air permeability is greater than 30000s, and the electronic conductivity is 10. -6 S / cm. The thermally responsive insulating film undergoes a structural transformation, reducing the membrane porosity to achieve membrane closure, thereby blocking gas crosstalk between electrodes, preventing thermal crosstalk reactions, and improving battery safety.
[0178] Example 5
[0179] The coated particles are prepared by the following steps:
[0180] 1) Disperse conductive particles (a mixture of carbon black and carbon nanotubes (mass ratio 3 / 1)) in a tetrahydrofuran solution of polyethersulfone (mass ratio of conductive particles to polyethersulfone is 7 / 3), with a solid content of 5%, and stir at 30°C for 24 hours to prepare a uniform first mixture.
[0181] 2) Spray dry the first mixture at 65℃ (flow rate 15ml / min~35ml / min) to obtain primary coated particles containing the first shell layer;
[0182] 3) Disperse the primary coated particles in an N-methylpyrrolidone solution (8 wt%) of polyethylene wax (the mass ratio of primary particles to polyethylene wax is 7 / 3) to prepare a homogeneous second mixture;
[0183] 4) Spray dry the second mixture at a temperature of 125°C (flow rate 15ml / min~35ml / min) to obtain secondary coated particles containing a second shell.
[0184] The base film is prepared by the following steps:
[0185] 1) Dissolve polyamic acid in a mixed solution of N-methylpyrrolidone and chloroform (volume ratio 6 / 1) with a solid content of 12.5%, stir at 80°C for 24 hours to prepare a homogeneous solution, and then coat the solution into a liquid film with a thickness of 100 μm.
[0186] 2) Place the above liquid film in a coagulation bath (water / ethanol / ethylene glycol, volume ratio 1 / 6 / 1) for 0.5 h to obtain a solid film;
[0187] 3) The solid film was subjected to thermosetting treatment at temperatures of 60℃, 120℃, 180℃, 240℃ and 300℃ for 0.2h in sequence to obtain the base film;
[0188] The battery separator is prepared by the following steps:
[0189] 1) Disperse the secondary coated particles in the third liquid phase (an aqueous solution of polybutyl acrylate, 5 wt%), with the mass ratio of the secondary coated particles to polybutyl acrylate being 8.5 / 1.5, to prepare a uniform third mixture.
[0190] 2) The third mixture was sprayed onto both sides of the thermosetting substrate and dried at 65°C to obtain the target sample. The performance parameters of the sample are shown in Table 1.
[0191] The diaphragm samples were heat-treated at 80℃ and 150℃ for 1h, respectively. After heat treatment, the thickness, thermal shrinkage rate, porosity, air permeability and electronic conductivity of the diaphragm samples were measured. The performance parameters are shown in Table 1.
[0192] Based on the data in Example 5, it can be seen that:
[0193] 1) Under normal temperature conditions (below 60℃), the membrane thickness is 13μm, the porosity is 49%, the air permeability is 213s, and the electronic conductivity is less than 10. -10S / cm can prevent battery self-discharge and ensure battery cycle performance and power performance under normal conditions.
[0194] 2) At 80℃, the membrane thickness is 13μm, the porosity is 32%, the air permeability is 654s, and the electronic conductivity is 0.0003~0.00001S / cm. The air permeability does not change much, indicating that the lithium-ion transport channels are still unobstructed. The increase in the electronic conductivity of the membrane causes uniform micro-short circuits and self-discharge in the battery, reducing the battery's state of charge and releasing the battery's electrochemical energy.
[0195] 3) At temperatures above 150℃, the membrane thickness is 12μm, the porosity is 1%, the air permeability is greater than 30000s, and the electronic conductivity is 10. -6 S / cm. The thermally responsive insulating film undergoes a structural transformation, reducing the membrane porosity to achieve membrane closure, thereby blocking gas crosstalk between electrodes, preventing thermal crosstalk reactions, and improving battery safety.
[0196] Example 6
[0197] The coated particles are prepared through the following steps:
[0198] 1) Disperse conductive particles (a mixture of carbon black and carbon nanotubes (mass ratio 3 / 1)) in a polyphenylene sulfide N-methylpyrrolidone solution (mass ratio of conductive particles to polyphenylene sulfide is 5 / 5), with a solid content of 10%, and stir at 30°C for 24 hours to prepare a uniform first mixture.
[0199] 2) The first mixture was spray-dried at 125℃ (flow rate 15ml / min~35ml / min) to obtain primary coated particles containing the first shell layer;
[0200] 3) Disperse the primary coated particles in a tetrahydrofuran solution of polytetrafluoroethylene-hexafluoropropylene (12wt%) (the mass ratio of primary coated particles to polytetrafluoroethylene-hexafluoropropylene is 7 / 3) to prepare a homogeneous second mixture;
[0201] 4) Spray dry the second mixture at a temperature of 65°C (flow rate 15ml / min~35ml / min) to obtain secondary coated particles containing a second shell.
[0202] The battery separator is prepared by the following steps:
[0203] 1) Disperse the secondary coated particles in the third liquid phase (aqueous emulsion of styrene-butadiene rubber, 25wt%), with the mass ratio of the secondary coated particles to polystyrene-butadiene rubber being 8.5 / 1.5, to prepare a uniform third mixture.
[0204] 2) The third mixture was coated and dried at 65°C to obtain a thermally responsive functional layer membrane. The performance parameters of the membrane sample are shown in Table 1.
[0205] Performance testing
[0206] 1) The sample from Example 6 was used as the separator for a soft-pack lithium-ion battery with a rated capacity of 5Ah (the positive electrode active material was LiNi). 0.8 Co 0.1 Mn 0.1 O2 (NCM811), with natural graphite as the negative electrode active material, the battery was charged to full charge (4.2V, 100% SOC) at 0.1C rate at 25℃.
[0207] 2) The fully charged battery was placed in an accelerating calorimeter and tested in a temperature range from room temperature to 220°C. The voltage and temperature changes of the battery were monitored. The lowest voltage and highest temperature were represented by Vmin and Tmax, respectively, and the maximum temperature rise rate of the battery was represented by rmax. The test results are shown in Table 3.
[0208] Based on the data from Example 6, it can be concluded that the performance data of the separator sample at room temperature is close to that of the comparative separator, indicating that the separator prepared by this invention can ensure the normal operation of the battery at room temperature. Furthermore, after the separator is assembled into a battery, the battery will not experience thermal runaway within a temperature range below 220°C, thereby effectively improving battery safety.
[0209] Comparative Example 1
[0210] Using a commercially available polyethylene diaphragm with an alumina ceramic coating on both sides as a comparison sample, the performance parameters of the sample at 25℃ (room temperature) are shown in Table 1.
[0211] The samples were heat-treated at 60℃, 80℃, 150℃ and 180℃ for 1 h respectively. The performance parameters of the samples are shown in Table 1.
[0212] For the heat shrinkage rate test method, please refer to Example 1, which will not be repeated here.
[0213] Performance Test 1
[0214] 1) The separator sample of Comparative Example 1 was used as the separator for a soft-pack lithium-ion battery with a rated capacity of 5Ah (the positive electrode active material was LiNi). 0.8 Co 0.1 Mn 0.1 O2 (NCM811), with natural graphite as the negative electrode active material, the battery was charged to full charge (4.2V, 100% SOC) at 0.1C rate at 25℃.
[0215] 2) Place the fully charged batteries in environments of 25℃, 80℃, and 150℃ for 10 hours respectively, and monitor the voltage and temperature changes of the batteries. The changes are expressed in V... min and T max The values represent the lowest and highest voltages detected. The test results are shown in Table 2.
[0216] 3) After the battery has been left to stand, it was placed back in an environment of 25°C for 10 hours, and then its capacity retention rate R was tested at a rate of 0.1C. The test results are shown in Table 2.
[0217] Performance Test 2
[0218] 1) The separator sample of Comparative Example 1 was used as the separator for a soft-pack lithium-ion battery with a rated capacity of 5Ah (the positive electrode active material was LiNi). 0.8 Co 0.1 Mn 0.1 O2 (NCM811), with natural graphite as the negative electrode active material, the battery was charged to full charge (4.2V, 100% SOC) at 0.1C rate at 25℃.
[0219] 2) Place the fully charged battery in an accelerating calorimeter and test it within a temperature range from room temperature to 220°C. Monitor the changes in battery voltage and temperature, respectively expressed in V. min and t max Indicates the lowest and highest monitored voltages, expressed in r. max The maximum rate of temperature rise of the battery is indicated in Table 3. The test results are shown in Table 3.
[0220] Table 1 Performance test results of different diaphragm samples
[0221]
[0222]
[0223] Note a): The sample of Comparative Example 1 underwent severe thermal shrinkage at 150℃ and 180℃ and was not suitable for testing.
[0224] In this invention, the air permeability value refers to the time required for a standard gas pressure and volume to pass through a membrane of a standard area. A higher air permeability value indicates greater resistance to gas passage through the membrane, making it less likely for gas to pass through. For lithium battery separators, a higher air permeability value is more effective in preventing gas crosstalk between electrodes.
[0225] The test results in Table 1 show that commercial polyolefin-based separators exhibit severe thermal shrinkage at temperatures exceeding 150°C, while the separator prepared by this invention does not experience thermal shrinkage even at 180°C. This prevents solid materials inside the battery from directly contacting each other due to separator shrinkage, thereby improving battery safety performance.
[0226] According to Table 1, 1) Under normal temperature conditions (below 60℃), the membrane thickness is 13-15 μm, the porosity is 39%-49%, the air permeability is 186-256 s, and the electronic conductivity is less than 10. -10 S / cm can prevent battery self-discharge and ensure battery cycle performance and power performance under normal conditions.
[0227] 2) Within the temperature range of 60℃ to 150℃, the membrane thickness is 10 to 13 μm, the porosity is 10% to 45%, the air permeability is 300 to 800 s, and the electronic conductivity is 10. -3 ~10 -9 S / cm. The increase in the electronic conductivity of the separator indicates a structural transformation of the thermally responsive insulating film. Conductive particles are exposed on the surface of the thermally responsive insulating film, and an electronic conductive network is formed, causing uniform micro-short circuits and self-discharge in the battery, reducing the battery's state of charge, and releasing the battery's electrochemical energy.
[0228] 3) At temperatures above 150℃, the membrane thickness is 9μm~12μm, the porosity is less than 5%, the air permeability is greater than 30000s, and the electronic conductivity is less than 10. -6 ~10 -8 / cm. The thermally responsive insulating film undergoes a structural transformation, reducing the membrane porosity to achieve membrane closure, thereby blocking gas crosstalk between electrodes, preventing thermal crosstalk reactions, and improving battery safety.
[0229] Table 2. Test results of 5Ah batteries assembled with different separators after standing at 25℃ for 10 hours.
[0230]
[0231] Note a): The sample experienced severe thermal runaway at 150℃ and was not suitable for testing.
[0232] As shown in Table 2, the separator prepared by this invention, due to its loaded and coated particles, can ensure the normal operation of the battery at room temperature and increase the electronic conductivity of the separator at intermediate temperatures (60℃-150℃), thereby enabling uniform micro-short circuits and self-discharge, reducing the battery's state of charge, releasing the battery's electrochemical energy, and reducing the battery's heating rate. Furthermore, at high temperatures (above 150℃), the closed-cell design blocks gas crosstalk between electrodes, preventing thermal crosstalk reactions and improving battery safety.
[0233] Table 3. Accelerated calorimeter test results of 5Ah batteries assembled with different separators.
[0234]
[0235] The test results in Table 3 show that after the separator prepared in this invention is assembled into a battery, the battery will not experience thermal runaway within a temperature range of 220°C, thereby effectively improving the safety of the battery.
[0236] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0237] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A coated particle, characterized in that, include: Conductive particles; as well as A thermally responsive insulating film is used to coat the conductive particles. When the temperature is greater than 60°C, the thermally responsive insulating film deforms so that at least a portion of the surface of the conductive particles can be exposed. The thermally responsive insulating film includes a first film layer and a second film layer. The conductive particles are first coated with the first film layer and then coated with the second film layer by atomization drying. The first film layer contains a first polymer component and the second film layer contains a second polymer component. The second polymer component has a higher temperature resistance than the first polymer component. The melting point of the first polymer component is 60℃-150℃, and the melting point of the second polymer component is greater than 150℃. When the coated particles are loaded onto a base film or formed into a film alone and applied to a battery: Within the temperature range of 60℃ to 150℃, the first film layer undergoes a structural transformation, and conductive particles are exposed on the surface of the thermally responsive insulating film, forming an electronic conductive network, which increases the electronic conductivity of the membrane. When the temperature is above 150°C, the second membrane layer undergoes a structural transformation, reducing the membrane porosity and achieving membrane pore closure.
2. The coated particles as described in claim 1, characterized in that, The thermally responsive insulating film is made of at least one of the following materials: polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, styrene-butadiene rubber, polyamide-imide, polyethersulfone, polyphenylene sulfide, polyvinyl chloride, polyamic acid, poly(m-phenylene isophthalamide), poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene.
3. The coated particles as described in claim 1, characterized in that, The particle size range of the conductive particles is 0.01μm-3μm.
4. The coated particles as described in claim 1, characterized in that, The conductive particles are selected from at least one of carbon black, graphene, carbon nanotubes, nickel, cobalt, manganese, zinc, tin, copper, and aluminum.
5. The coated particles as described in claim 1, characterized in that, The method of coating the conductive particles onto the thermally responsive insulating film further includes ball milling, surface grafting, or interfacial polymerization.
6. A method for preparing coated particles according to any one of claims 1-5, characterized in that, include: Conductive particles are dispersed in a liquid phase to prepare a uniform coating solution, and the coating solution is atomized and dried at a temperature of 60℃~250℃ to obtain coated particles containing a thermally responsive insulating film.
7. The method for preparing coated particles as described in claim 6, characterized in that, The liquid phase contains at least one of the following: polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, styrene-butadiene rubber, polyamide-imide, polyethersulfone, polyphenylene sulfide, polyvinyl chloride, polyamic acid, poly(m-phenylene isophthalamide), poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene.
8. The method for preparing coated particles as described in claim 6, characterized in that, The liquid phase includes a first liquid phase and a second liquid phase, wherein the polymer component of the second liquid phase has a higher temperature resistance than the polymer component of the first liquid phase. The step of obtaining coated particles containing a thermally responsive insulating film includes: 1) Disperse the conductive particles in the first liquid phase to prepare a uniform first mixture; 2) The first mixed solution is atomized and dried at a temperature of 60~150℃ to obtain primary coated particles containing the first film layer; 3) Disperse the primary coated particles in the second liquid phase to prepare a homogeneous second mixture; 4) The second mixture is atomized and dried at a temperature of 120~250 degrees Celsius to obtain secondary coated particles containing the first and second membrane layers.
9. The method for preparing coated particles as described in claim 6, characterized in that, The solvent of the liquid phase is selected from at least one of water, ethanol, methanol, 1,4-dioxane, toluene, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, 1,2-dichloroethane, chloroform, tetrahydrofuran, acetone, and ethyl acetate.
10. A diaphragm, characterized in that, Includes the coated particles as described in any one of claims 1-5.
11. A diaphragm, characterized in that, It includes a base film and coated particles as described in any one of claims 1-5, wherein the coated particles are uniformly distributed on one or both sides of the surface of the base film.
12. The diaphragm as claimed in claim 11, characterized in that, Prepared by the following steps: (1) Disperse the coated particles in the third liquid phase to prepare a uniform third mixture; (2) The third mixture is loaded onto one or both sides of the base membrane and dried at a temperature of 40°C to 150°C to obtain the diaphragm.
13. The diaphragm as claimed in claim 12, characterized in that, The third liquid phase contains at least one of polyethylene, polypropylene, polyethylene glycol, polyethylene oxide, polypropylene oxide, polyethyleneimine, polyvinylidene fluoride, polymethyl methacrylate, polyacrylic acid, carboxymethyl cellulose, chitosan, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, and styrene-butadiene rubber latex.
14. The diaphragm as claimed in claim 11, characterized in that, The base film is prepared by the following steps: 1) Spread the film-forming solution evenly into a liquid film with a thickness of 10μm~400μm; 2) Place the liquid film in a coagulation bath for 0.1 h to 30 h to obtain a solid film; 3) The solid film is subjected to thermosetting treatment at a temperature of 150℃~450℃ to obtain the base film.
15. The diaphragm as claimed in claim 14, characterized in that, The film-forming solution contains at least one of polyvinyl chloride, polyethersulfone, polyamic acid, poly(m-phenylene isophthalamide), poly(p-phenylene terephthalamide), polysiloxane, and polytetrafluoroethylene.
16. The diaphragm as claimed in claim 12, characterized in that, The solvent of the third liquid phase is selected from at least one of water, ethanol, methanol, 1,4-dioxane, toluene, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, 1,2-dichloroethane, chloroform, tetrahydrofuran, acetone, and ethyl acetate.
17. The diaphragm according to any one of claims 11-16, characterized in that, The thickness of the diaphragm is 5μm to 20μm.
18. A battery, characterized in that, It includes the diaphragm as described in any one of claims 10-17.
Citation Information
Patent Citations
Microsphere, diaphragm containing microsphere and lithium ion battery containing diaphragm
CN112615107A
Lithium supplementing material, negative plate and battery
CN113594439A