Semiconductor structure fabrication methods and semiconductor structures
By forming a multilayer isolation structure on the substrate and controlling the etching process, the problem of isolation structure depression caused by the removal of the oxide layer on the substrate surface is solved, ensuring the integrity of the epitaxial layer and improving the performance and yield of PMOS devices.
Patent Information
- Application Number
- CN202211020370.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-24
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-08-24
AI Technical Summary
Before the formation of the germanium-silicon layer, the oxide layer removal process on the substrate surface causes the shallow trench isolation structure to sink, resulting in charge leakage and affecting the performance and yield of PMOS devices.
By forming a multilayer isolation structure on the substrate and controlling the etching process, the top surface of the isolation stack is made flat, avoiding turf defects and ensuring the integrity of the epitaxial layer.
This effectively avoids charge leakage from devices on the epitaxial layer, improving the performance and yield of the semiconductor structure.
Smart Images

Figure CN117693184B_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to the field of semiconductor technology, and in particular to a method for fabricating a semiconductor structure and the semiconductor structure itself. Background Technology
[0002] With the development of integrated circuits, the feature size of semiconductor devices is constantly decreasing. Traditional channel materials can no longer meet the drive current requirements of PMOS devices. It is necessary to use epitaxial growth to form a germanium-silicon (SiGe) layer on the substrate surface as the channel material of PMOS devices to improve its mobility, thereby increasing the operating saturation current (Idsat) and response speed of PMOS devices and improving the performance of PMOS devices.
[0003] Epitaxial growth of germanium-silicon layers places high demands on the substrate surface. Contamination or residual oxide layers on the substrate surface can lead to lattice defects such as stacking faults, dislocations, and slip lines during epitaxial growth. Therefore, the substrate needs to be pre-cleaned before epitaxial growth of the germanium-silicon layer to remove the oxide layer on the substrate surface. However, the pre-cleaning process consumes part of the shallow trench isolation (STI) structure, causing the top surface of the STI structure to dishing. If the dishing region between the isolation structure and the substrate in the circuit area is too deep, it can lead to delamination problems and easily cause charge leakage in PMOS devices. Summary of the Invention
[0004] The following is an overview of the subject matter described in detail in this disclosure. This overview is not intended to limit the scope of the claims.
[0005] This disclosure provides a method for fabricating a semiconductor structure and the semiconductor structure itself.
[0006] The first aspect of this disclosure provides a method for fabricating a semiconductor structure, the method comprising:
[0007] A substrate is provided, the substrate including a first region and a second region, the first region including a plurality of independently disposed first active regions, adjacent first active regions being separated by a first trench, and an isolation stack being formed in the first trench;
[0008] A barrier layer is formed, covering the top surface of the second region;
[0009] An epitaxial layer is formed, covering the top surface of the first active region;
[0010] The barrier layer and a portion of the isolation stack located in the first region are etched away, wherein the height of the joints of the top surfaces of the isolation stacks retained in the first region is substantially the same.
[0011] The isolation stack includes a first isolation layer, a second isolation layer, and a third isolation layer sequentially covering the first trench. The first isolation layer and the third isolation layer have the same etch selectivity, and the first isolation layer and the second isolation layer have different etch selectivity. Removing a portion of the isolation stack located in the first region includes:
[0012] A portion of the second isolation layer is removed, and the top surface of the remaining second isolation layer is lower than the top surfaces of the first isolation layer and the third isolation layer;
[0013] Remove a portion of the first isolation layer and a portion of the third isolation layer, leaving the top surfaces of the retained first isolation layer, the third isolation layer, and the second isolation layer at approximately the same height.
[0014] The barrier layer includes:
[0015] An initial barrier layer is formed to cover the top surface of the substrate, and the initial barrier layer and the first isolation layer have the same etching selectivity.
[0016] The initial barrier layer located in the first region is removed, exposing the top surface of the first active region, and the retained initial barrier layer forms the barrier layer.
[0017] The method for fabricating the semiconductor structure further includes:
[0018] Clean the first region to remove the oxide film on the top surface of the first active region.
[0019] The removal of a portion of the first isolation layer and a portion of the third isolation layer includes:
[0020] Etching of the barrier layer and the first region is performed, and etching is stopped at the top surface of the substrate that exposes the second region. The barrier layer, a portion of the first isolation layer located in the first region, and a portion of the third isolation layer located in the first region are removed. The top surfaces of the first isolation layer, the second isolation layer, and the third isolation layer retained in the first trench are substantially at the same height.
[0021] The barrier layer includes:
[0022] A first barrier layer, a second barrier layer, and a third barrier layer are formed on the top surface of the substrate in sequence. The first barrier layer and the first isolation layer have the same etching selectivity, the second barrier layer and the second isolation layer have the same etching selectivity, and the first barrier layer and the third barrier layer have the same etching selectivity.
[0023] The thickness of the second barrier layer is greater than the total thickness of the first barrier layer and the third barrier layer.
[0024] The method for fabricating the semiconductor structure further includes:
[0025] Etch the first region to remove the third barrier layer and the second barrier layer located in the first region;
[0026] The third barrier layer located in the second region and the first barrier layer located in the first region are etched away, exposing the top surface of the first active region.
[0027] The etching process removes the barrier layer and a portion of the isolation stack located in the first region, including:
[0028] The second barrier layer located in the second region and a portion of the second isolation layer located in the first region are etched away, and the top surface of the second isolation layer retained in the first trench is lower than the top surfaces of the first isolation layer and the third isolation layer.
[0029] The first barrier layer located in the second region, as well as a portion of the first isolation layer and a portion of the third isolation layer located in the first region, are etched away. The top surfaces of the first isolation layer, the second isolation layer, and the third isolation layer retained in the first trench are substantially at the same height.
[0030] The method for fabricating the semiconductor structure further includes:
[0031] A protective layer is formed to cover the top surface of the epitaxial layer, the protective layer comprising a first material.
[0032] The second region includes multiple independently configured second active regions, adjacent second active regions are separated by second trenches, and the isolation stack is formed in the second trenches. The first active region and the second active region have different conductivity types.
[0033] The first region includes a PMOSFET region, and the second region includes an NMOSFET region.
[0034] A second aspect of this disclosure provides a semiconductor structure, the semiconductor structure comprising:
[0035] The substrate includes a first region and a second region, wherein the first region includes a plurality of independently disposed first active regions, and adjacent first active regions are separated by a first trench.
[0036] A first isolation structure is disposed in the first trench. The first isolation structure includes a multi-layer structure that sequentially covers the first trench. The height of the joint of the top surfaces of each layer of the first isolation structure is basically the same.
[0037] An epitaxial layer covers the top surface of the first active region.
[0038] The first isolation structure includes:
[0039] The first isolation layer covers the bottom wall of the first trench and part of the sidewall of the first trench;
[0040] A second isolation layer covers the first isolation layer;
[0041] A third isolation layer covers the second isolation layer;
[0042] The top surfaces of the first isolation layer, the second isolation layer, and the third isolation layer are at approximately the same height.
[0043] The epitaxial layer includes a first material, and in a cross-section perpendicular to the top surface of the substrate, the concentration of the first material on the top and bottom surfaces of the epitaxial layer is greater than the concentration of the first material in the middle of the epitaxial layer.
[0044] The second region includes multiple independently configured second active regions, adjacent second active regions are separated by a second trench, and a second isolation structure is provided in the second trench. The first active region and the second active region have different conductivity types.
[0045] The first region includes a PMOSFET region, and the second region includes an NMOSFET region.
[0046] In the semiconductor structure fabrication method and semiconductor structure disclosed herein, after forming an epitaxial layer on the top surface of the first active region, a portion of the isolation stack located in the first region is etched away to ensure that the top surface of the isolation stack retained in the first region is free of turf defects. This can prevent charge leakage in the devices subsequently formed on the epitaxial layer, ensuring that the formed semiconductor structure has excellent performance and higher yield.
[0047] After reading and understanding the accompanying diagrams and detailed descriptions, the other aspects can be understood. Attached Figure Description
[0048] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments of the present disclosure and, together with the description, serve to explain the principles of these embodiments. In these drawings, similar reference numerals are used to denote similar elements. The drawings described below are some embodiments of the present disclosure, but not all embodiments. Other drawings will be readily available to those skilled in the art based on these drawings without inventive effort.
[0049] Figure 1This is a flowchart illustrating a method for fabricating a semiconductor structure according to an exemplary embodiment.
[0050] Figure 2 This is a flowchart illustrating a method for fabricating a semiconductor structure according to an exemplary embodiment.
[0051] Figure 3 This is a flowchart illustrating a method for fabricating a semiconductor structure according to an exemplary embodiment.
[0052] Figure 4 This is a schematic diagram of the structure of a substrate according to an exemplary embodiment.
[0053] Figure 5 This is a schematic diagram of the structure for forming an initial barrier layer according to an exemplary embodiment.
[0054] Figure 6 This is a schematic diagram illustrating the structure for forming a photoresist layer according to an exemplary embodiment.
[0055] Figure 7 This is a schematic diagram of a structure for forming a barrier layer according to an exemplary embodiment.
[0056] Figure 8 This is a schematic diagram illustrating the structure for cleaning and removing oxide films according to an exemplary embodiment.
[0057] Figure 9 This is a schematic diagram of a structure for forming an epitaxial layer according to an exemplary embodiment.
[0058] Figure 10 This is a schematic diagram of the structure of a portion of the second isolation layer etched away according to an exemplary embodiment.
[0059] Figure 11 This is a schematic diagram of a structure for forming a barrier layer according to an exemplary embodiment.
[0060] Figure 12 This is a schematic diagram illustrating the structure for forming a photoresist layer according to an exemplary embodiment.
[0061] Figure 13 This is a schematic diagram illustrating the structure of removing the third and second blocking layers in the first region according to an exemplary embodiment.
[0062] Figure 14 This is a schematic diagram illustrating the structure of removing the first barrier layer in the first region according to an exemplary embodiment.
[0063] Figure 15 This is a schematic diagram of a structure for forming an epitaxial layer according to an exemplary embodiment.
[0064] Figure 16This is a schematic diagram of the structure of a portion of the second isolation layer etched away according to an exemplary embodiment.
[0065] Figure 17 This is a schematic diagram of a semiconductor structure formed according to an exemplary embodiment.
[0066] Figure label:
[0067] 100, Substrate; 101, First region; 102, Second region; 110, First active region; 111, Oxide film; 120, First trench; 130, Second active region; 140, Second trench; 200, Isolation stack; 210, First isolation layer; 220, Second isolation layer; 230, Third isolation layer; 250, First isolation structure; 260, Second isolation structure; 300, Barrier layer; 300a, Initial barrier layer; 310, First barrier layer; 320, Second barrier layer; 330, Third barrier layer; 350, Photoresist layer; 400, Epitaxial layer; 410, Protective layer. Detailed Implementation
[0068] To make the objectives, technical solutions, and advantages of the embodiments of this disclosure clearer, the technical solutions in the disclosed embodiments will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this disclosure. All other embodiments obtained by those skilled in the art based on the embodiments of this disclosure without creative effort are within the scope of protection of this disclosure. It should be noted that, unless otherwise specified, the embodiments and features in the embodiments of this disclosure can be arbitrarily combined with each other.
[0069] Currently, shallow trench isolation structures typically employ an oxide-nitride-oxide (ONO) structure. The pre-cleaning process before epitaxial formation of the germanium-silicon layer may remove some of the oxide from the shallow trench isolation structure, forming a trench near the active region. This trench continues to deepen in subsequent processes, reaching a depth of approximately 15 nm after epitaxial layer formation. The top of the nitride in the shallow trench isolation structure is higher than the oxide, resulting in a "grass-like" defect on the top surface. This "grass-like" defect easily accumulates charge, forming an electron trap. This causes charge to diffuse towards the "grass-like" area in the subsequently formed PMOS device, leading to gate oxide charge leakage and ultimately reducing device performance and yield in the semiconductor structure.
[0070] This disclosure provides a method for fabricating a semiconductor structure in exemplary embodiments, such as... Figure 1 As shown, Figure 1 A flowchart illustrating a method for fabricating a semiconductor structure according to an exemplary embodiment of the present disclosure is shown. Figures 4-17The diagram below illustrates the various stages of semiconductor structure fabrication. Figures 4-17 The methods for fabricating semiconductor structures are introduced.
[0071] This embodiment does not limit the semiconductor structure. The following description will take Dynamic Random Access Memory (DRAM) as an example, but this embodiment is not limited to this. Other semiconductor structures are also possible in this embodiment.
[0072] like Figure 1 As shown, an exemplary embodiment of this disclosure provides a method for fabricating a semiconductor structure, comprising the following steps:
[0073] Step S110: Provide a substrate, the substrate including a first region and a second region, the first region including a plurality of independently disposed first active regions, adjacent first active regions being separated by a first trench, and an isolation stack being formed in the first trench.
[0074] like Figure 4 As shown, substrate 100 can be a semiconductor substrate, which may include a silicon substrate, a germanium (Ge) substrate, a silicon germanide (SiGe) substrate, a silicon-on-insulator (SOI) substrate, or a germanium-on-insulator (GOI) substrate, etc. The semiconductor substrate may also be doped with ions. In this embodiment, substrate 100 is a silicon substrate.
[0075] The substrate 100 includes one or more first regions 101, each first region 101 including a plurality of independently disposed first active regions 110, with adjacent first active regions 110 separated by first trenches 120. The substrate 100 also includes a second region 102, which is the other region of the substrate 100 besides the first regions 101, and semiconductor devices can be formed in the second region 102.
[0076] The isolation stack 200 includes a multi-layer structure that sequentially covers the first trench 120. In this embodiment, the isolation stack 200 includes a first isolation layer 210, a second isolation layer 220, and a third isolation layer 230 that sequentially cover the first trench 120. The first isolation layer 210 covers the bottom wall and sidewalls of the first trench 120, the second isolation layer 220 covers the first isolation layer 120, and the third isolation layer 230 covers the second isolation layer 220 and fills the unfilled area of the first trench 120. The etching selectivity ratios of the first isolation layer 210 and the third isolation layer 230 are the same, while the etching selectivity ratios of the first isolation layer 210 and the second isolation layer 220 are different.
[0077] In this embodiment, the first isolation layer 210 and the third isolation layer 230 are made of the same material, while the first isolation layer 210 and the second isolation layer 220 are made of different materials. For example, the materials of the first isolation layer 210 and the third isolation layer 230 may include silicon oxide, and the material of the second isolation layer 220 may include silicon nitride.
[0078] Step S120: Form a barrier layer to cover the top surface of the second region.
[0079] like Figure 5 or Figure 11 As shown, the barrier layer 300 may include a single layer or a stacked structure. The barrier layer 300 at least covers the top surface of the second region 102 to avoid damage to the device in the second region 102 by subsequent processes of the first region 101.
[0080] Step S130: Form an epitaxial layer covering the top surface of the first active region.
[0081] Reference Figure 4 As shown, the substrate 100 is exposed to the process environment, and the surface of the first active region 110 may be oxidized by the environment to form an oxide film 111. In this embodiment, before forming the epitaxial layer 400, the first active region 110 is processed to remove the oxide film 111 on the surface of the first active region 110.
[0082] like Figure 8 or Figure 14 As shown, since the materials of the first isolation layer 210 and the third isolation layer 230 are also oxides, during the process of removing the oxide film 111, a portion of the first isolation layer 210 and a portion of the third isolation layer 230 exposed in the first region 101 are also removed. This results in the top surfaces of the first isolation layer 210 and the third isolation layer 230 exposed in the first region 101 being lower than the top surface of the second isolation layer 220 after the oxide film 111 on the surface of the first active region 110 is removed, forming a depression on the top surface of the isolation stack 200. In particular, the thickness of the first isolation layer 210 is less than that of the third isolation layer 230, resulting in a faster etching rate for the first isolation layer 210, forming a narrow and deep groove between the first active region 110 and the second isolation layer 220.
[0083] In this embodiment, the epitaxial layer 400 is formed using the following implementation method:
[0084] like Figure 9 or Figure 15As shown, a substrate 100 is placed in a reaction chamber, with the top surface of the first active region 110 serving as a seed crystal. A gas source for forming the epitaxial layer 400 is introduced into the reaction chamber, and the epitaxial layer 400 is epitaxially grown on the first active region 110 using a chemical vapor deposition process. The material of the epitaxial layer 400 may include silicon, germanium, silicon germanide, silicon carbide, gallium arsenide, or indium gallium ionide. The epitaxial layer 400 may be doped with conductive dopant ions, and the silicon concentration at the top and bottom surfaces of the epitaxial layer 400 is greater than the silicon concentration in the middle of the epitaxial layer 400.
[0085] Step S140: Etch away the barrier layer and part of the isolation stack located in the first region, where the height of the joints of the top surfaces of the isolation stacks retained in the first region is basically the same.
[0086] like Figure 10 , Figure 17 As shown, refer to Figure 7 , Figure 8 , Figure 9 The etching process of the barrier layer 300 and the etching process of the isolation stack 200 located in the first region 101 can be performed simultaneously, or the etching process of the barrier layer 300 can be performed simultaneously only with the etching process of a portion of the isolation stack 200 located in the first region 101. In this embodiment, the etching depth of the isolation stack 200 located in the first region 101 can be controlled by controlling the thickness of the barrier layer 300, such as... Figure 17 As shown, this is to ensure that the height of the top surface connection of each layer of the isolation stack 200 retained in the first region 101 is substantially the same.
[0087] In this embodiment, removing a portion of the isolation stack 200 located in the first region 101 can be achieved through the following implementation:
[0088] like Figure 10 Or such as Figure 16 As shown, firstly, a portion of the second isolation layer 220 is removed, and the top surface of the remaining second isolation layer 220 is lower than the top surfaces of the first isolation layer 210 and the third isolation layer 230.
[0089] In this embodiment, the etching process of the second isolation layer 220 has a high etching selectivity compared to the first isolation layer 210 and the third isolation layer 230, ensuring that the heights of the first isolation layer 210 and the third isolation layer 230 remain unchanged during the etching of the second isolation layer 220.
[0090] like Figure 17 As shown, then, part of the first isolation layer 210 and part of the third isolation layer 230 are removed, and the top surfaces of the retained first isolation layer 210, the third isolation layer 230 and the second isolation layer 220 are basically at the same height.
[0091] In this embodiment, the barrier layer 300 includes at least a material with the same etching selectivity as the material of the first isolation layer 210. The etching process of the barrier layer 300 is performed at least simultaneously with the etching process of a portion of the first isolation layer 210 and a portion of the third isolation layer 230 located in the first region 101. The etching depth of the first isolation layer 210 and the third isolation layer 230 in the first region 101 can be controlled by adjusting the thickness of the barrier layer 300, so that the top surface height of each layer of the isolation stack 200 retained in the first region 101 is substantially the same at the junction.
[0092] In the semiconductor structure fabrication method of this embodiment, after forming an epitaxial layer on the top surface of the first active region, a portion of the isolation stack located in the first region is etched away to make the top surface of the isolation stack retained in the first region flat, without local protrusions or depressions, and without turf defects. This can prevent charge leakage of the devices subsequently formed on the epitaxial layer, ensuring that the formed semiconductor structure has excellent performance and higher yield.
[0093] According to an exemplary embodiment, this embodiment is a description of the above embodiments. This embodiment includes all the steps of the above embodiments. The difference between this embodiment and the above embodiments is that, after forming the epitaxial layer, this embodiment also performs the following steps:
[0094] like Figure 10 Or such as Figure 16 As shown, a protective layer 410 is formed, covering the top surface of the epitaxial layer 400, and the protective layer 410 includes a first material.
[0095] In this embodiment, the first material and the first active region 110 are the same material. For example, the material of the first active region 110 includes silicon, and the first material includes silicon.
[0096] In this embodiment, the protective layer 410 covers the epitaxial layer 400 to protect it and prevent damage during subsequent etching of the barrier layer 300 and the isolation stack 200 exposed in the first region 101. This ensures the top surface of the epitaxial layer 400 remains intact and prevents charge leakage from devices subsequently formed on the epitaxial layer 400. Furthermore, since the protective layer 410 is exposed to the process environment, the first material will be oxidized to an oxide during subsequent processes. The oxidized protective layer 410 can be removed during the etching of the isolation stack 200 in the first region 101, eliminating the need for an additional step to remove the protective layer 410. This ensures that no first material or oxide residue remains on the formed epitaxial layer 400, while also maintaining a streamlined semiconductor manufacturing process.
[0097] like Figure 2 As shown, an exemplary embodiment of this disclosure provides a method for fabricating a semiconductor structure, comprising the following steps:
[0098] Step S210: Provide a substrate, the substrate including a first region and a second region, the first region including a plurality of independently disposed first active regions, adjacent first active regions being separated by a first trench, and an isolation stack being formed in the first trench.
[0099] like Figure 4 As shown, the substrate 100 is a silicon substrate, the first region 101 includes a PMOSFET region, and the second region 102 includes an NMOSFET region.
[0100] The substrate 100 includes one or more first regions 101, each first region 101 including a plurality of independently disposed first active regions 110, with adjacent first active regions 110 separated by a first trench 120. The second region 102 includes a plurality of independently disposed second active regions 130, with adjacent second active regions 130 separated by a second trench 140. The first active regions 110 and the second active regions 130 have different conductivity types.
[0101] In this embodiment, the first active region 110 has a P-type conductivity type and is used to form a PMOS device. The second active region 130 has an N-type conductivity type and is used to form an NMOS device.
[0102] like Figure 4 As shown, the isolation stack 200 in this embodiment is the same as that in the above embodiment. The isolation stack 200 includes a first isolation layer 210, a second isolation layer 220 and a third isolation layer 230 stacked in sequence. The material of the first isolation layer 210 includes silicon oxide, the material of the second isolation layer 220 includes silicon nitride and the material of the third isolation layer 230 includes silicon oxide. The difference between this embodiment and the above embodiment is that the isolation stack 200 not only fills the first trench 120 but also fills the second trench 140, and the isolation stack 200 is also formed in the second trench 140.
[0103] Step S220: Form a barrier layer to cover the top surface of the second region.
[0104] In this embodiment, the barrier layer 300 is formed using the following implementation method:
[0105] like Figure 5 As shown, refer to Figure 4First, an initial barrier layer 300a is formed, covering the top surface of the substrate 100. The initial barrier layer 300a and the first isolation layer 210 have the same etching selectivity. For example, atomic layer deposition (ALD) can be used to deposit the initial barrier layer 300a. In this embodiment, the material of the initial barrier layer 300a can be the same as that of the first isolation layer 210. For example, the material of the first isolation layer 20 includes silicon oxide, and the material of the initial barrier layer 300a also includes silicon oxide.
[0106] Then, the initial barrier layer 300a located in the first region 101 is removed, exposing the top surface of the first active region 110, and the retained initial barrier layer 300a forms the barrier layer 300.
[0107] like Figure 6 As shown, refer to Figure 5 A photoresist layer 350 is formed, which covers the top surface of the initial barrier layer 300a located in the second region 102. For example... Figure 7 As shown, refer to Figure 6 Then, the initial barrier layer 300a exposed by the photoresist layer 350 is removed by a Certas etching process, exposing the top surface of the first active region 110, and the retained initial barrier layer 300a forms the barrier layer 300. Then, the photoresist layer 350 is removed by plasma ashing.
[0108] In this embodiment, the Certas etching process is a chemical dry etching process. The Certas etching process etches the initial barrier layer 300a. The reaction products of hydrofluoric acid gas and the material of the isolation stack 200 adhere to the top surface of the isolation stack 200, preventing the hydrogen fluoride gas from continuing to react with the isolation stack 200, and can reduce the depression defects formed on the top surface of the isolation stack 200 during the etching process.
[0109] It is understood that in this embodiment, the coverage area of the photoresist layer 350 can be expanded to ensure that the formed barrier layer 300 can expose the top surface of each first active region 110 and the portion of the isolation stack 200 surrounding each first active region 110.
[0110] Step S230: Clean the first region to remove the oxide film on the top surface of the first active region.
[0111] like Figure 8 As shown, refer to Figure 7The first region 101 exposed by the blocking layer 300 is etched to remove the first active region 110 with a thickness of about 3nm to 5nm from the top surface of the first active region 110, so as to remove the oxide film 111 formed by natural oxidation on the top surface of the first active region 110, ensuring that the material on the top surface of the first active region 110 is pure and free of impurities, so that the crystal orientation of the first material in the epitaxial layer 400 (which will be described in detail in subsequent steps) formed on the top surface of the first active region 110 is the same as the silicon crystal orientation in the first active region 110.
[0112] like Figure 8 As shown, during the etching process of removing the oxide film 111 on the top surface of the first active region 110, the portion of the first isolation layer 210 and the third isolation layer 230 exposed in the first region 101 is removed, while the first isolation layer 210 and the third isolation layer 230 are retained above the top surface of the second isolation layer 220, forming a groove between the second isolation layer 220 and the first active region 110.
[0113] Step S240: Form an epitaxial layer covering the top surface of the first active region.
[0114] like Figure 9 As shown, refer to Figure 8 The epitaxial layer 400 is made of silicon germanide. The substrate 100 is placed in the reaction chamber, and silicon source gas and germanium source gas are introduced into the reaction chamber respectively. For example, dichlorosilane (DCS) or silicon tetrahydrodeionide (SiH4) can be introduced into the reaction chamber as silicon source gas, and germanane (GeH4) can be introduced into the reaction chamber as germanium source gas. The silicon source gas and germanium source gas react in the reaction chamber to form silicon germanide, and silicon germanide is deposited on the top surface of the first active region 110 to form the epitaxial layer 400.
[0115] Step S250: Form a protective layer covering the top surface of the epitaxial layer, the protective layer comprising a first material.
[0116] like Figure 9 As shown, after the epitaxial layer 400 is formed, the germanium source gas is stopped from being introduced into the reaction chamber, and dichlorosilane (DCS) or silicon tetrahydrogenate (SiH4) is continued to be introduced into the reaction chamber, and hydrogen chloride (HCl) is introduced into the reaction chamber to deposit silicon on the surface of the epitaxial layer 400 to form a protective layer 410. That is, in this embodiment, the first material is silicon.
[0117] The thickness of the protective layer 410 formed in this embodiment is 2nm to 3nm, for example, it can be 2nm, 2.2nm, 2.4nm, 2.5nm, 2.7nm, 2.9nm or 3nm. The thickness of the protective layer 410 is within this range. In subsequent processes, the silicon in the protective layer 410 is sufficient to be completely oxidized by the process environment to form silicon oxide, so that the protective layer 410 can be etched away in the process of etching the first isolation layer 210 and the third isolation layer 230.
[0118] In this embodiment, after the epitaxial layer 400 is formed, the gas introduced into the reaction chamber is adjusted to form a protective layer 410 on the epitaxial layer 400. There is no need to add equipment for forming the protective layer 410, which reduces production costs and saves time.
[0119] Step S260: Remove part of the second isolation layer, with the top surface of the retained second isolation layer being lower than the top surfaces of the first and third isolation layers.
[0120] like Figure 10 As shown, refer to Figure 9 The second isolation layer 220 exposed in the first region 101 is etched by wet etching. For example, hot phosphoric acid (H3PO4) at a temperature of 150℃~200℃ can be used to etch the second isolation layer 220. Part of the second isolation layer 220 dissolves in the hot phosphoric acid. The hot phosphoric acid that has dissolved part of the second isolation layer 220 is removed. The second isolation layer 220 is etched toward the substrate 100 for about 15nm so that the top surface of the second isolation layer 220 retained in the first region 101 is lower than the top surfaces of the first isolation layer 210 and the third isolation layer 230.
[0121] Step S270: Etch the barrier layer and the first region, stop etching the top surface of the substrate to expose the second region, remove the barrier layer, a portion of the first isolation layer located in the first region, and a portion of the third isolation layer located in the first region, and the top surfaces of the first isolation layer, the second isolation layer, and the third isolation layer retained in the first trench are basically at the same height.
[0122] Reference Figure 10 The barrier layer 300 and the first region 101 are etched using dilute hydrofluoric acid (DHF) to remove all of the barrier layer 300, and simultaneously remove part of the first isolation layer 210 and part of the third isolation layer 230 in the first region 101. Figure 17 As shown, after etching, the top surfaces of the first isolation layer 210, the second isolation layer 220, and the third isolation layer 230 retained in the first trench 120 are basically at the same height, and the top surfaces of the first isolation layer 210, the second isolation layer 220, and the third isolation layer 230 are smoothly connected. The isolation stack 200 retained in the first trench 120 forms the first isolation structure 250, and the isolation stack 200 retained in the second trench 140 forms the second isolation structure 260. The top surface of the first isolation structure 250 is flat and has no depressions or protrusions.
[0123] like Figure 17 As shown, refer to Figure 10In this embodiment, the protective layer 410 is exposed to the process environment. The silicon in the protective layer 410 is oxidized to silicon oxide. When the barrier layer 300 and the first region 101 are cleaned with dilute hydrofluoric acid (DHF), the oxidized protective layer 410 is removed by dilute hydrofluoric acid, avoiding damage to the epitaxial layer 400 by the etching process. The top surface of the epitaxial layer 400 is flat and without defects, which is beneficial to improving the performance and yield of the PMOS device formed on the epitaxial layer 400.
[0124] The semiconductor structure fabrication method of this embodiment uses a material with the same etching selectivity as the first isolation layer and the third isolation layer as a barrier layer. When the barrier layer is etched away, the etching rates of the first isolation layer, the third isolation layer and the barrier layer exposed in the first region are the same. The etching depth of the first isolation layer and the third isolation layer in the first region can be controlled by the process of removing the barrier layer, so that the top surface of the isolation stack retained in the first region is flat, without local protrusions or depressions, and without turf defects. This provides a good process platform for forming PMOS devices in the first region, ensuring that the formed semiconductor structure has excellent performance and higher yield, and avoiding charge leakage in the PMOS devices subsequently formed on the epitaxial layer.
[0125] like Figure 3 As shown, an exemplary embodiment of this disclosure provides a method for fabricating a semiconductor structure, comprising the following steps:
[0126] Step S310: Provide a substrate, the substrate including a first region and a second region, the first region including a plurality of independently disposed first active regions, adjacent first active regions being separated by a first trench, and an isolation stack being formed in the first trench.
[0127] like Figure 4 As shown, the substrate 100 provided in this embodiment is the same as the substrate 100 provided in step S210 of the above embodiment, and will not be described again here. The isolation stack 200 in this embodiment is the same as that in the above embodiment. The isolation stack 200 includes a first isolation layer 210, a second isolation layer 220 and a third isolation layer 230 stacked sequentially. The material of the first isolation layer 210 includes silicon oxide, the material of the second isolation layer 220 includes silicon nitride and the material of the third isolation layer 230 includes silicon oxide.
[0128] Step S320: Form a first barrier layer, a second barrier layer and a third barrier layer stacked sequentially on the top surface of the substrate.
[0129] like Figure 11As shown, the barrier layer 300 formed in this embodiment is a stacked structure with the same etching characteristics as the isolation stack 200. The barrier layer 300 includes a first barrier layer 310, a second barrier layer 320 and a third barrier layer 330 stacked on the substrate 100, so as to adjust the etching depth of each layer of the isolation stack 200 in subsequent processes by adjusting the thickness of each layer of the barrier layer 300.
[0130] like Figure 11 As shown, refer to Figure 4 A first barrier layer 310, a second barrier layer 320, and a third barrier layer 330 can be sequentially formed on the top surface of the substrate 100 using an atomic layer deposition process. The etching selectivity ratios of the first barrier layer 310 and the first isolation layer 210 are the same, the etching selectivity ratios of the second barrier layer 320 and the second isolation layer 220 are the same, and the etching selectivity ratios of the first barrier layer 310 and the third barrier layer 330 are the same. In this embodiment, the material of the first barrier layer 310 includes silicon oxide, the material of the second barrier layer 320 includes silicon nitride, and the material of the third barrier layer 330 includes silicon oxide.
[0131] In this embodiment, the thickness of the second barrier layer 320 is greater than the total thickness of the first barrier layer 310 and the third barrier layer 330, to allow for the increase in depth of the first isolation layer 210 and the third isolation layer 230 due to process influences. For example, the thickness of the first barrier layer 310 is 6nm, the thickness of the second barrier layer 320 is 12nm, and the thickness of the third barrier layer 330 is 5.5nm.
[0132] Step S330: Etch the first region to remove the third barrier layer and the second barrier layer located in the first region.
[0133] like Figure 12 As shown, firstly, a photoresist layer 350 is formed, which covers the third barrier layer 330 located in the second region 102.
[0134] Reference Figure 13 Then, the third barrier layer 330 exposed by the photoresist layer 350 is removed by the Certas etching process, exposing the second barrier layer 320 located in the first region 101. Then, the photoresist layer 350 is removed by plasma ashing, exposing the third barrier layer 330 located in the second region 102.
[0135] Reference Figure 13 Then, the second barrier layer 320 of the first region 101 is removed by thermal phosphoric acid, exposing the first barrier layer 310 located in the first region 101.
[0136] Step S340: Etch away the third barrier layer located in the second region and the first barrier layer located in the first region to expose the top surface of the first active region.
[0137] like Figure 14 As shown, refer to Figure 13 The first barrier layer 310 in the first region 101 and the third barrier layer 330 in the second region 102 are removed by the Certas etching process.
[0138] like Figure 14 As shown, in this embodiment, the materials of the first barrier layer 310 and the third barrier layer 330 are both silicon oxide. In the process of removing the first barrier layer 310 and the third barrier layer 330 by the Certas etching process, the oxide film 111 formed by natural oxidation on the surface of the first active region 110 can be removed at the same time. There is no need to clean and remove the oxide film 111 on the surface of the first active region 110, which reduces the number of process steps.
[0139] Step S350: Form an epitaxial layer covering the top surface of the first active region.
[0140] like Figure 15 As shown, the steps for forming the epitaxial layer 400 in this embodiment are the same as those for forming the epitaxial layer 400 in step S240 of the above embodiment, and will not be repeated here.
[0141] Step S360: Form a protective layer covering the top surface of the epitaxial layer, the protective layer comprising a first material.
[0142] like Figure 15 As shown, the steps for forming the protective layer 410 in this embodiment are the same as those for forming the protective layer 410 in step S250 of the above embodiment, and will not be repeated here.
[0143] Step S370: Etch away the second barrier layer located in the second region and a portion of the second isolation layer located in the first region, wherein the top surface of the second isolation layer retained in the first trench is lower than the top surfaces of the first isolation layer and the third isolation layer.
[0144] like Figure 16 As shown, refer to Figure 15 The second barrier layer 320 located in the second region 102 and the second isolation layer 220 located in the first region 101 are etched by hot phosphoric acid wet etching. All of the second barrier layer 320 in the second region 102 is removed, and the top surface of the first barrier layer 310 in the second region 102 is exposed. The etching is stopped, and the second isolation layer 220 located in the first region 101 is etched towards the substrate 100 for about 12nm to 15nm. The top surface of the second isolation layer 220 retained in the first region 101 is lower than the top surfaces of the first isolation layer 210 and the third isolation layer 230.
[0145] Step S380: Etch away the first barrier layer located in the second region and part of the first isolation layer and part of the third isolation layer located in the first region. The top surfaces of the first isolation layer, the second isolation layer and the third isolation layer retained in the first trench are basically at the same height.
[0146] like Figure 17 As shown, refer to Figure 16 The etching process involves removing the first barrier layer 310 in the second region 102 and a portion of the first isolation layer 210 and a portion of the third isolation layer 230 in the first region 101 by etching with dilute hydrofluoric acid (DHF). This exposes the top surface of the substrate 100 in the second region 102, and the etching stops thereafter. After etching, the top surfaces of the retained first isolation layer 210, second isolation layer 220, and third isolation layer 230 in the first trench 120 are at approximately the same height. Furthermore, the dilute hydrofluoric acid etching process simultaneously removes the protective layer 410, exposing the top surface of the epitaxial layer 400.
[0147] In the semiconductor structure fabrication method of this embodiment, a stacked structure with the same etching characteristics as each layer of the isolation stack is formed as a barrier layer. The etching depth of each layer of the isolation stack can be adjusted by adjusting the thickness of each layer of the barrier layer, so that the top surface of the isolation stack in the first region is free of grass defects, providing a good process platform for forming PMOS devices in the first region and avoiding charge leakage of PMOS devices formed on the epitaxial layer in the future.
[0148] This disclosure provides an exemplary embodiment of a semiconductor structure, such as Figure 17 As shown, the semiconductor structure includes a substrate 100, a first isolation structure 250, and an epitaxial layer 400. The substrate 100 includes a first region 101 and a second region 102. The first region 101 includes a plurality of independently disposed first active regions 110, and adjacent first active regions 110 are separated by a first trench 120. The first isolation structure 250 is disposed in the first trench 120. From the trench wall of the first trench 120 towards the center, the first isolation structure 250 includes a multilayer structure that sequentially covers the first trench 120. The height of the junction of the top surfaces of each layer of the first isolation structure 250 is substantially the same.
[0149] In some embodiments, such as Figure 17 As shown, the first isolation structure 250 includes a first isolation layer 210, a second isolation layer 220, and a third isolation layer 230 that sequentially cover the first trench 120. The first isolation layer 210 covers the bottom wall and part of the side wall of the first trench 120. The second isolation layer 220 covers the first isolation layer 210, and the third isolation layer 230 covers the second isolation layer 220. The top surfaces of the first isolation layer 210, the second isolation layer 220, and the third isolation layer 230 are at approximately the same height.
[0150] In some embodiments, such as Figure 17 As shown, the epitaxial layer 400 includes a first material, and in a cross section perpendicular to the top surface of the substrate 100, the silicon concentration at the top and bottom surfaces of the epitaxial layer 400 is greater than the silicon concentration in the middle of the epitaxial layer 400.
[0151] In some embodiments, such as Figure 17 As shown, the second region 102 includes multiple independently configured second active regions 130. Adjacent second active regions 130 are separated by a second trench 140. A second isolation structure 260 is provided in the second trench 140. The first active region 110 and the second active region 130 have different conductivity types.
[0152] In this embodiment, as Figure 17 As shown, the first region 101 includes a PMOSFET region, and the second region 102 includes an NMOSFET region. The first active region 110 has a P-type conductivity type and is used to form a PMOS device. The second active region 130 has an N-type conductivity type and is used to form an NMOS device.
[0153] In this embodiment, the top surface of the first isolation structure 250 has no depressions or protrusions, which can prevent the top defects of the first isolation structure 250 from forming an electron trap, causing the devices on the epitaxial layer 400 to leak charge to the first isolation structure 250, thus ensuring that the semiconductor structure has good electroforming performance.
[0154] The various embodiments or implementation methods described in this specification are presented in a progressive manner. Each embodiment focuses on the differences from other embodiments, and the same or similar parts between the embodiments can be referred to each other.
[0155] In the description of this specification, references to the terms "embodiment," "exemplary embodiment," "some implementation," "illustrated implementation," "example," etc., refer to specific features, structures, materials, or characteristics described in connection with an implementation or example that are included in at least one implementation or example of this disclosure.
[0156] In this specification, the illustrative expressions of the terms used do not necessarily refer to the same implementation or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more implementations or examples.
[0157] In the description of this disclosure, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this disclosure and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this disclosure.
[0158] It is understood that the terms "first," "second," etc., as used in this disclosure may be used to describe various structures, but these structures are not limited by these terms. These terms are only used to distinguish one structure from another.
[0159] In one or more accompanying drawings, the same elements are represented by similar reference numerals. For clarity, many parts in the drawings are not drawn to scale. Furthermore, certain well-known parts may not be shown. For simplicity, a structure obtained after several steps may be depicted in a single drawing. Many specific details of this disclosure, such as the structure, materials, dimensions, processing methods, and techniques of the devices, are described below to provide a clearer understanding of the disclosure. However, as those skilled in the art will understand, this disclosure may be implemented without adhering to these specific details.
[0160] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this disclosure, and are not intended to limit them. Although this disclosure has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this disclosure.
Claims
1. A method of fabricating a semiconductor structure, the method comprising: The method for fabricating the semiconductor structure includes: A substrate is provided, the substrate including a first region and a second region, the first region including a plurality of independently disposed first active regions, adjacent first active regions being separated by a first trench, an isolation stack being formed in the first trench, the isolation stack including a first isolation layer, a second isolation layer and a third isolation layer sequentially covering the first trench, the first isolation layer and the third isolation layer having the same etching selectivity, and the first isolation layer and the second isolation layer having different etching selectivity; An initial barrier layer is formed to cover the top surface of the substrate, and the initial barrier layer and the first isolation layer have the same etching selectivity. Remove the initial barrier layer located in the first region to expose the top surface of the first active region, and the retained initial barrier layer forms the barrier layer, which covers the top surface of the second region; An epitaxial layer is formed, covering the top surface of the first active region; The barrier layer is removed by etching; A portion of the second isolation layer is removed, and the top surface of the remaining second isolation layer is lower than the top surfaces of the first isolation layer and the third isolation layer; Remove a portion of the first isolation layer and a portion of the third isolation layer, leaving the top surfaces of the retained first isolation layer, the third isolation layer, and the second isolation layer at approximately the same height.
2. The method of fabricating a semiconductor structure of claim 1, wherein, The method for fabricating the semiconductor structure further includes: Clean the first region to remove the oxide film on the top surface of the first active region.
3. The method of fabricating a semiconductor structure of claim 1, wherein, Removing a portion of the first isolation layer and a portion of the third isolation layer includes: Etching of the barrier layer and the first region is performed, and etching is stopped at the top surface of the substrate that exposes the second region. The barrier layer, a portion of the first isolation layer located in the first region, and a portion of the third isolation layer located in the first region are removed. The top surfaces of the first isolation layer, the second isolation layer, and the third isolation layer retained in the first trench are substantially at the same height.
4. The method of fabricating a semiconductor structure of claim 1, wherein, Forming a barrier layer, including: A first barrier layer, a second barrier layer, and a third barrier layer are formed on the top surface of the substrate in sequence. The first barrier layer and the first isolation layer have the same etching selectivity, the second barrier layer and the second isolation layer have the same etching selectivity, and the first barrier layer and the third barrier layer have the same etching selectivity. The thickness of the second barrier layer is greater than the total thickness of the first barrier layer and the third barrier layer.
5. The method for fabricating a semiconductor structure according to claim 4, characterized in that, The method for fabricating the semiconductor structure further includes: Etch the first region to remove the third barrier layer and the second barrier layer located in the first region; The third barrier layer located in the second region and the first barrier layer located in the first region are etched away, exposing the top surface of the first active region.
6. The method for fabricating a semiconductor structure according to claim 5, characterized in that, Etching away the barrier layer and a portion of the isolation stack located in the first region includes: The second barrier layer located in the second region and a portion of the second isolation layer located in the first region are etched away, and the top surface of the second isolation layer retained in the first trench is lower than the top surfaces of the first isolation layer and the third isolation layer. The first barrier layer located in the second region, as well as a portion of the first isolation layer and a portion of the third isolation layer located in the first region, are etched away. The top surfaces of the first isolation layer, the second isolation layer, and the third isolation layer retained in the first trench are substantially at the same height.
7. The method for fabricating a semiconductor structure according to claim 1, characterized in that, The method for fabricating the semiconductor structure further includes: A protective layer is formed to cover the top surface of the epitaxial layer, the protective layer comprising a first material.
8. The method for fabricating a semiconductor structure according to claim 1, characterized in that, The second region includes multiple independently configured second active regions, adjacent second active regions are separated by second trenches, and the isolation stack is formed in the second trenches. The first active region and the second active region have different conductivity types.
9. The method for fabricating a semiconductor structure according to claim 8, characterized in that, The first region includes a PMOSFET region, and the second region includes an NMOSFET region.
10. A semiconductor structure, characterized in that, The semiconductor structure is fabricated according to any one of claims 1-9, wherein the semiconductor structure comprises: The substrate includes a first region and a second region, wherein the first region includes a plurality of independently disposed first active regions, and adjacent first active regions are separated by a first trench. A first isolation structure is disposed in the first trench. The first isolation structure includes a multi-layer structure that sequentially covers the first trench. The height of the joints between the top surfaces of each layer of the first isolation structure is basically the same. An epitaxial layer covers the top surface of the first active region.
11. The semiconductor structure according to claim 10, characterized in that, The first isolation structure includes: The first isolation layer covers the bottom wall of the first trench and part of the sidewall of the first trench; A second isolation layer covers the first isolation layer; A third isolation layer covers the second isolation layer; The top surfaces of the first isolation layer, the second isolation layer, and the third isolation layer are at approximately the same height.
12. The semiconductor structure according to claim 10, characterized in that, The epitaxial layer includes a first material, and in a cross-section perpendicular to the top surface of the substrate, the concentration of the first material at the top and bottom surfaces of the epitaxial layer is greater than the concentration of the first material in the middle of the epitaxial layer.
13. The semiconductor structure according to claim 10, characterized in that, The second region includes multiple independently configured second active regions, adjacent second active regions are separated by a second trench, and a second isolation structure is provided in the second trench. The first active region and the second active region have different conductivity types.
14. The semiconductor structure according to claim 13, characterized in that, The first region includes a PMOSFET region, and the second region includes an NMOSFET region.
Citation Information
Patent Citations
Semiconductor Devices and Methods of Manufacture Thereof
US20090283837A1
Semiconductor devices
US20220189969A1