Semi-interpenetrating network polymer, composite material, dielectric film and preparation method thereof
By introducing semi-interpenetrating network structure and nanofillers into polymer dielectrics, the problem of insufficient energy storage performance of polymer dielectrics in high temperature environments is solved, and high-efficiency energy storage and high-performance dielectric films in a wide temperature range are achieved.
Patent Information
- Application Number
- CN202311665378.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-12-06
AI Technical Summary
The existing polymer dielectrics lack energy storage capacity and reliability in high temperature environments, especially at temperatures of 150°C and above, the conductivity loss increases and the breakdown field strength decreases, resulting in a significant reduction in charge and discharge efficiency and energy storage density.
Using semi-interpenetrating network polymer, consisting of thermoplastic polymer, bismaleimide resin and catalyst, it forms excellent dielectric energy storage performance through cross-linking and curing, and is suitable for dielectrics in a wide temperature range (room temperature to 150°C) Thin film, nanofillers and molecular semiconductors are added to improve performance.
Under high temperature and strong electric field conditions above 150°C and above 600 MV/m, excellent device performance for a long time is achieved, energy storage density and charge and discharge efficiency are improved, and high dielectric constant and low dielectric loss are maintained.
Smart Images

Figure CN117700991B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of dielectric materials and energy storage materials, and in particular to semi-interpenetrating network polymers, composite materials, dielectric films and preparation methods thereof. Background Art
[0002] Film capacitors with polymer dielectrics play an irreplaceable role in the field of electronics and electrical due to their fast charging and discharging speed, high power density, good voltage resistance, self-healing properties and chemical corrosion resistance. With the increasing demand for miniaturization and lightweight of electronic equipment and their application in extreme environments, higher requirements are placed on the energy storage capacity and reliability of polymer dielectrics at high temperatures. Under a constant external electric field, when the external temperature is close to the glass transition temperature of the polymer, the leakage current inside the dielectric will increase exponentially, and the leakage current will be converted into Joule heat, resulting in large conductivity losses, which will not only lead to a significant reduction in charging and discharging efficiency, but also a significant reduction in breakdown field strength, leading to failure or damage of power equipment. Therefore, in addition to having excellent dielectric properties such as high dielectric constant and low dielectric loss, polymer dielectrics used in high temperature environments also need to have low conductivity loss and high breakdown field strength to ensure high charging and discharging efficiency and high discharge energy density.
[0003] At present, high-temperature polymer dielectrics for film capacitors are mainly thermoplastic engineering plastics with high glass transition temperature (Tg), such as polyetherimide (PEI), polyphenylene sulfide (PPS), polyester (PET), polyetheretherketone (PEEK), etc. Although these engineering plastics have a high Tg and meet the mechanical temperature resistance requirements, their high-temperature dielectric energy storage performance is still unsatisfactory. For example, the conductivity loss will still increase significantly at a high temperature of 150°C, resulting in a significant decrease in breakdown field strength, charge and discharge efficiency, and energy storage density. Therefore, it is of great application value to study new polymer dielectric materials with excellent dielectric energy storage performance in a wide temperature range (room temperature to 150°C).
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a semi-interpenetrating network polymer, a composite material, a dielectric film and a preparation method thereof. The semi-interpenetrating network polymer provided in the embodiment of the present invention has excellent dielectric energy storage performance. When the polymer is made into a film capacitor, it has excellent device performance in a wide temperature range (room temperature to 150°C), and is suitable for power electronic devices and microelectronic devices such as energy storage capacitors, embedded capacitors and organic field effect transistors in high temperature environments.
[0006] The present invention is achieved in that:
[0007] In a first aspect, the present invention provides a semi-interpenetrating network polymer, wherein the raw materials are composed of a thermoplastic polymer, a bismaleimide resin and a catalyst, wherein the mass ratio of the thermoplastic polymer to the bismaleimide resin is (1.8:1)-(19:1), and the amount of the catalyst used is 0.05-2wt% of the amount of the bismaleimide resin used.
[0008] In an optional embodiment, the mass ratio of the thermoplastic polymer to the bismaleimide resin is (7:3)-(9:1);
[0009] Preferably, the amount of the catalyst is 0.1-1wt% of the amount of the bismaleimide resin;
[0010] Preferably, the thermoplastic polymer comprises any one of polyetherimide, polysulfone, polycarbonate and polyamide ether imide;
[0011] Preferably, the bismaleimide resin is selected from the compounds represented by the following structural formula:
[0012] , R1 includes an aromatic group;
[0013] Preferably, R1 is selected from any one of the following structural formulas:
[0014] , , , , and , wherein n represents the number of repeating units, preferably 1-10;
[0015] Preferably, the catalyst comprises a free radical initiator, preferably a peroxide; more preferably any one of di-tert-butyl peroxyisopropylbenzene, di-tert-butyl peroxide and diisopropylbenzene peroxide.
[0016] In a second aspect, the present invention provides a method for preparing the semi-interpenetrating network polymer described in the aforementioned embodiment, comprising: mixing a thermoplastic polymer, a bismaleimide resin and a catalyst for cross-linking and curing.
[0017] In an optional embodiment, the conditions for cross-linking the solid include: performing a curing reaction at multiple temperature stages;
[0018] Preferably, it comprises: performing a multi-stage temperature curing reaction at a temperature of 150-250°C;
[0019] Preferably, the method comprises: curing at 150-190° C. for 1.5-2.5 hours, then curing at 200-215° C. for 1.5-2.5 hours, and then curing at 220-250° C. for 3-4 hours.
[0020] In a third aspect, the present invention provides a semi-interpenetrating network composite material, wherein the raw materials are composed of nanofillers, molecular semiconductors, thermoplastic polymers, bismaleimide resins and catalysts, wherein the mass ratio of the thermoplastic polymer to the bismaleimide resin is (1.8:1)-(19:1), the amount of the catalyst used is 0.05-2wt% of the amount of the bismaleimide resin used; the amount of the nanofiller added is 0-5wt% of the total mass, the amount of the molecular semiconductor added is 0-3wt% of the total mass, and the nanofiller and the molecular semiconductor contain at least one.
[0021] In an optional embodiment, the mass ratio of the thermoplastic polymer to the bismaleimide resin is (7:3)-(9:1);
[0022] Preferably, the amount of the catalyst is 0.1-1wt% of the amount of the bismaleimide resin;
[0023] Preferably, the amount of the nanofiller added is 0.5-1.5wt% of the total mass;
[0024] Preferably, the added amount of the molecular semiconductor is 0.5-1.0 wt% of the total mass;
[0025] Preferably, the thermoplastic polymer comprises any one of polyetherimide, polysulfone, polycarbonate and polyamide ether imide;
[0026] Preferably, the bismaleimide resin is selected from the compounds represented by the following structural formula:
[0027] , R1 includes an aromatic group;
[0028] Preferably, R1 is selected from any one of the following structural formulas:
[0029] , , , , and , wherein n represents the number of repeating units, preferably 1-10;
[0030] Preferably, the catalyst comprises a free radical initiator, preferably a peroxide; more preferably any one of di-tert-butyl peroxyisopropylbenzene, di-tert-butyl peroxide and diisopropylbenzene peroxide;
[0031] Preferably, the nanofiller includes at least one of nano-aluminum oxide, nano-silicon dioxide, nano-boron nitride, nano-titanium dioxide, nano-magnesium oxide, nano-hafnium dioxide, etc.;
[0032] Preferably, the particle size of the nanofiller of nano boron nitride is 0.1-100 μm, preferably 1 μm;
[0033] Preferably, the particle size of other nanofillers except nano boron nitride is 5-100 nm, preferably 10-50 nm;
[0034] Preferably, the molecular semiconductor includes any one of aromatic ester compounds, aromatic anhydride compounds, perylene compounds, quinone compounds and aromatic phenanthracene compounds;
[0035] Preferably, the molecular semiconductor includes one of [6,6]-phenyl-C61-butyric acid methyl ester, [6,6]-phenyl C71 butyric acid methyl ester, 1,4,5,8-naphthalenetetracarboxylic anhydride, 2,6-dibromonaphthalene-1,4,5,8-tetracarboxylic dianhydride, 1,7-dibromo-3,4,9,10-perylenetetracarboxylic dianhydride, 1,6,7,12-tetrachloro-3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,5,6-tetrafluoro-7,7,8,8-tetracyanodimethyl-p-benzoquinone, and tribenzo[de,kl,rst]pentaphen.
[0036] In a fourth aspect, the present invention provides a method for preparing the semi-interpenetrating network composite material described in the aforementioned embodiment, comprising: mixing a nanofiller, a molecular semiconductor, a bismaleimide resin and a catalyst for cross-linking and curing;
[0037] Preferably, the multi-stage temperature curing reaction is carried out at a temperature of 150-250°C;
[0038] Preferably, the method comprises: curing at 150-190° C. for 1.5-2.5 hours, then curing at 200-215° C. for 1.5-2.5 hours, and then curing at 220-250° C. for 3-4 hours.
[0039] In a fifth aspect, the present invention provides a semi-interpenetrating network dielectric film, which is prepared by the semi-interpenetrating network polymer described in the aforementioned embodiment.
[0040] In a sixth aspect, the present invention provides a method for preparing a semi-interpenetrating network dielectric film, comprising: dissolving and mixing a thermoplastic polymer, a bismaleimide resin and a catalyst in a polar solvent, and then coating the mixture on a substrate, drying the mixture to form an uncured film, and then performing multi-stage temperature curing;
[0041] Preferably, it comprises: performing a multi-stage temperature curing reaction at a temperature of 150-250°C;
[0042] Preferably, the method comprises: curing at 150-190° C. for 1.5-2.5 hours, then curing at 200-215° C. for 1.5-2.5 hours, and then curing at 220-250° C. for 3-4 hours.
[0043] In a seventh aspect, the present invention provides a semi-interpenetrating network composite material film, which is prepared by the semi-interpenetrating network composite material described in the aforementioned embodiment.
[0044] The present invention has the following beneficial effects: The embodiment of the present invention provides a new semi-interpenetrating network polymer, which has excellent device performance in a wide temperature range (room temperature to 150°C) when prepared as a dielectric film, and is suitable for power electronic devices and microelectronic devices such as energy storage capacitors, embedded capacitors and organic field effect transistors in high temperature environments. In particular, it can be used for a long time under high temperature and strong electric field conditions of 150°C and above 600MV / m. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0046] Figure 1 The energy storage density diagram of the semi-interpenetrating network dielectric film prepared in Examples 1 to 4 of the present invention;
[0047] Figure 2 The energy storage density of the semi-interpenetrating network dielectric film prepared in Examples 5 and 6 of the present invention;
[0048] Figure 3 This is a diagram of the energy storage density of the semi-interpenetrating network dielectric film prepared in Examples 7 and 8 of the present invention;
[0049] Figure 4 The energy storage density diagram of the dielectric film prepared in Comparative Examples 1 to 5 of the present invention;
[0050] Figure 5 The graphs showing the dielectric constant and dielectric loss of the semi-interpenetrating network dielectric films prepared in Examples 1 to 3 of the present invention as a function of frequency are shown;
[0051] Figure 6 The graphs showing the dielectric constant and dielectric loss of the semi-interpenetrating network dielectric films prepared in Examples 7 and 8 of the present invention as a function of frequency are shown;
[0052] Figure 7The dielectric constant and dielectric loss of the dielectric films prepared in Comparative Examples 3 and 5 of the present invention vary with frequency;
[0053] Figure 8 This is a SEM image of the dielectric film provided in Comparative Example 3 of the present invention;
[0054] Fig. 9 This is a SEM image of the semi-interpenetrating network dielectric film provided in Example 2 of the present invention. DETAILED DESCRIPTION
[0055] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0056] Existing dielectric films for commercial film capacitors, such as biaxially oriented polypropylene film (BOPP), cannot work at temperatures above 100°C. In order to prepare polymer dielectrics that can work at high temperatures (greater than 140°C), domestic and foreign researchers and the industry have conducted extensive research on engineering plastics with high glass transition temperatures, such as polyetherimide (PEI), polyphenylene sulfide (PPS), polyester (PET), and polyetheretherketone (PEEK). Although this type of polymer dielectric with a high glass transition temperature has excellent mechanical temperature resistance, its dielectric energy storage temperature resistance is still difficult to meet application requirements. For example, under the dual conditions of high temperature and strong electric field of 150°C and above 600MV / m, its leakage current will increase significantly, resulting in low charge and discharge efficiency, and at the same time will cause the breakdown field strength to decrease, resulting in low energy storage density.
[0057] Therefore, the embodiment of the present invention provides a new semi-interpenetrating network polymer, which has excellent dielectric energy storage temperature resistance. Specifically, its raw materials are composed of a thermoplastic polymer, a bismaleimide resin and a catalyst, wherein the mass ratio of the thermoplastic polymer to the bismaleimide resin is (1.8:1)-(19:1), and the amount of the catalyst is 0.05-2wt% of the amount of the bismaleimide resin.
[0058] For example, the mass ratio of the thermoplastic polymer to the bismaleimide resin can be 1.8:1, 5:1, 9:1, 10:1, 15:1, 18:1, 19:1, etc., any value between (1.8:1) and (19:1), or a range value between any two values, for example, preferably (7:3) to (9:1).
[0059] The amount of the catalyst used for the bismaleimide resin can be 0.05 wt%, 0.1 wt%, 0.5 wt%, 1 wt%, 1.5 wt% and 2 wt%, any value between 0.05-2 wt% or a range between any two values, for example, preferably 0.1-1 wt%.
[0060] The thermoplastic polymer includes any one of polyetherimide, polysulfone, polycarbonate and polyamide etherimide.
[0061] The bismaleimide resin is selected from the compounds shown in the following structural formula:
[0062] , R1 includes an aromatic group; for example, R1 is selected from any one of the following structural formulas:
[0063] , , , , and , wherein n represents the number of repeating units, preferably 1-10.
[0064] The catalyst includes a free radical initiator, preferably a peroxide; more preferably any one of di-tert-butyl peroxyisopropylbenzene, di-tert-butyl peroxide and diisopropylbenzene peroxide.
[0065] Using a catalyst as an initiator for the chain extension reaction and cross-linking reaction of bismaleimide resin can reduce the reaction temperature and increase the reaction rate. The reaction of bismaleimide resin and thermoplastic polymer can form a semi-interpenetrating network structure, thereby achieving excellent high-temperature energy storage performance of the polymer.
[0066] The present invention provides a method for preparing the semi-interpenetrating network polymer described in the aforementioned embodiment, comprising: mixing a thermoplastic polymer, a bismaleimide resin and a catalyst for cross-linking and curing.
[0067] Specifically, a thermoplastic polymer and a bismaleimide resin are placed in a polar organic solvent according to a certain mass ratio, and heated and dissolved under magnetic stirring until a clear and transparent solution is fully dissolved. Then, a certain amount of catalyst is added dropwise, and stirring and dispersing is continued to obtain a composition slurry A, wherein the solid content of the slurry is 0.1 wt%-20 wt%, for example, any value between 0.1 wt%, 1 wt%, 5 wt%, 10 wt%, 15 wt% and 20 wt%, or a range value between any two values, for example, preferably 1 wt%-2 wt%.
[0068] Then, the curing reaction is carried out at multiple temperature stages; specifically, the curing reaction is carried out at multiple temperature stages at 150-250°C; for example, curing at 150-190°C for 1.5-2.5 hours, then curing at 200-215°C for 1.5-2.5 hours, and then curing at 220-250°C for 3-4 hours. The optimal curing thermal process is: 180°C × 2h+200°C × 2h+230°C × 4h, and protection can be carried out according to this extended range.
[0069] The embodiment of the present invention provides a semi-interpenetrating network dielectric film, which is prepared by the semi-interpenetrating network polymer described in the above embodiment. Specifically,
[0070] After the composition slurry A is evenly coated on a glass substrate, it is baked in a blast oven at 60-90° C. for more than 10 hours to evaporate the solvent as much as possible to obtain an uncured film;
[0071] The glass substrate after the solvent is evaporated is placed in a vacuum oven and subjected to a curing reaction at multiple temperatures between 150°C and 250°C to obtain a cured film; wherein the curing process is preferably performed at 150-190°C for 1.5-2.5 hours, then at 200-215°C for 1.5-2.5 hours, and then at 220-250°C for 3-4 hours.
[0072] After solidification, the conventional operations in the art such as peeling off from the glass substrate and drying are also included, which will not be described in detail in the embodiment of the present invention.
[0073] The invention provides a semi-interpenetrating network composite material, the raw materials of which, in addition to the above-mentioned thermoplastic polymer, bismaleimide resin and catalyst, also include at least one of nano filler and molecular semiconductor.
[0074] The amounts and selection of the thermoplastic polymer, bismaleimide resin and catalyst are the same as those of the aforementioned semi-IPN-forming polymer.
[0075] The amount of nanofiller added is 0-5wt% of the total mass of all raw materials to form the semi-interpenetrating network composite material, for example, 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 4.5 wt% and 5 wt%, any value between 0-5 wt% or a range value between any two values, for example, preferably 0.5-1.5wt%.
[0076] The addition amount of the molecular semiconductor is 0-3wt% of the total mass of all raw materials forming the semi-interpenetrating network composite material, for example, 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt% and 3 wt%, any value between 0-3 wt% or a range value between any two values, for example, preferably 0.5-1.0 wt%.
[0077] The nanofiller includes at least one of nano-aluminum oxide, nano-silicon dioxide, nano-boron nitride, nano-titanium dioxide, nano-magnesium oxide, nano-hafnium dioxide, etc.; wherein the particle size of the nano-boron nitride nanofiller is 0.1-100 μm, preferably 1 μm; the particle size of other nanofillers except nano-boron nitride is 5-100 nm, preferably 10-50 nm.
[0078] The molecular semiconductor includes any one of aromatic ester compounds, aromatic anhydride compounds, perylene compounds, quinone compounds and aromatic phenylphene compounds; preferably, the molecular semiconductor includes one of [6,6]-phenyl-C61-butyric acid methyl ester, [6,6]-phenyl C71 butyric acid methyl ester, 1,4,5,8-naphthalenetetracarboxylic anhydride, 2,6-dibromonaphthalene-1,4,5,8-tetracarboxylic dianhydride, 1,7-dibromo-3,4,9,10-perylenetetracarboxylic dianhydride, 1,6,7,12-tetrachloro-3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,5,6-tetrafluoro-7,7,8,8-tetracyanodimethyl-p-benzoquinone, and tribenzo[de,kl,rst]pentaphenylphene. Its specific structural formula is as follows:
[0079] [6,6]-phenyl-C61-butyric acid methyl ester; [6,6]-phenyl C71 butyric acid methyl ester; 1,4,5,8-Naphthalenetetracarboxylic anhydride; 2,6-Dibromonaphthalene-1,4,5,8-tetracarboxylic dianhydride; 1,7-Dibromo-3,4,9,10-perylenetetracarboxylic dianhydride; 1,6,7,12-Tetrachloro-3,4,9,10-perylenetetracarboxylic dianhydride; 2,3,5,6-tetrafluoro-7,7,8,8-tetracyanodimethyl-p-benzoquinone; Tribenzo[de,kl,rst]pentaphen.
[0080] The embodiment of the present invention provides a method for preparing a semi-interpenetrating network composite material, comprising mixing raw materials and then crosslinking and curing them, wherein the conditions of the crosslinking and curing are consistent with the conditions of the crosslinking and curing to form a semi-interpenetrating network polymer.
[0081] The present invention provides a semi-interpenetrating network composite material film, which is prepared by the semi-interpenetrating network composite material described in the aforementioned embodiment.
[0082] Specifically, a certain amount of nanofiller is added to the same organic solvent and ultrasonically dispersed to obtain solution B. Composition slurry A and B are mixed, and the mixture is stirred and dispersed to obtain composition slurry C.
[0083] A certain amount of molecular semiconductor is added to the same organic solvent and stirred and dissolved to obtain solution D. A and D are mixed and stirred and dispersed to obtain composition slurry E.
[0084] Alternatively, solution B, solution D and composition slurry A are mixed to form composition slurry F.
[0085] Then, after uniformly coating the composition slurry C, the composition slurry E or the composition slurry F on the glass substrate, the glass substrate is baked in a blast oven at 60-90° C. for more than 10 hours to evaporate the solvent as much as possible to obtain an uncured film; the glass substrate after the solvent is evaporated is placed in a vacuum oven and subjected to a curing reaction at multiple temperatures between 150° C. and 250° C. to obtain a cured film, wherein the curing process is preferably cured at 150-190° C. for 1.5-2.5 hours, then cured at 200-215° C. for 1.5-2.5 hours, and then cured at 220-250° C. for 3-4 hours.
[0086] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0087] Example 1
[0088] An embodiment of the present invention provides a method for preparing a semi-interpenetrating network dielectric film, comprising:
[0089] Weigh 0.15 g of polyetherimide (PEI) (purchased from Saudi Basic Industries Corporation (SABIC)), 0.05 g of bisphenol A bismaleimide (BPABMI) (purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), and 0.00025 g of di-tert-butylperoxyisopropylbenzene (BIPB) (purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0090] The above solution was heated to 50° C. under magnetic stirring and dissolved and dispersed for 8 hours to allow the solute to be fully and uniformly dissolved in the solvent.
[0091] Clean the glass slide to avoid dust contamination, then put the glass slide in a 70℃ oven to preheat for half an hour, then use a rubber-tipped dropper to draw 5 ml of film-making liquid and apply it on the glass slide, let the glass slide be baked in a 70℃ oven for 10 hours to fully evaporate the solvent to obtain a semi-solidified film.
[0092] The glass sheet loaded with the semi-cured film is placed in a vacuum oven, and the temperature is adjusted to carry out a multi-stage curing reaction. The temperature and time of each stage are: 180°C for two hours, 200°C for two hours, and 230°C for four hours. After natural cooling, the cured film is obtained.
[0093] Soak the glass slide with the cured film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on a clean aluminum foil.
[0094] The film together with the aluminum foil was placed in a vacuum oven and dried at a high temperature of 120° C. for 10 hours to obtain a PEI / BPABMI (75 / 25) semi-interpenetrating network dielectric film.
[0095] Test Example 1
[0096] The energy storage density, dielectric constant and dielectric loss of the PEI / BPABMI (75 / 25) semi-interpenetrating network dielectric film prepared in Example 1 were tested as a function of frequency.
[0097] Results Figure 1 and Figure 5 ,according to Figure 1 and Figure 5 It can be seen that the PEI / BPABMI (75 / 25) semi-IPN dielectric film has high energy storage density and efficiency at 150°C. When the electric field strength is 650MV / m, the charge and discharge efficiency is still 91.9%, and the discharge energy density is 6.76J / cm 3 When the frequency is 1MHz, the dielectric constant is 3.15 and the dielectric loss factor is 0.011.
[0098] Example 2
[0099] An embodiment of the present invention provides a method for preparing a semi-interpenetrating network dielectric film, comprising:
[0100] Weigh 0.15 g of polyetherimide (PEI), 0.05 g of bisphenol A bismaleimide (BPABMI), and 0.0005 g of di-tert-butylperoxyisopropylbenzene (BIPB), and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0101] The above solution was heated to 50° C. under magnetic stirring and dissolved and dispersed for 8 hours to allow the solute to be fully and uniformly dissolved in the solvent.
[0102] Clean the glass slide to avoid dust contamination, then put the glass slide in a 70℃ oven to preheat for half an hour, then use a rubber-tipped dropper to draw 5 ml of film-making liquid and apply it on the glass slide, let the glass slide be baked in a 70℃ oven for 10 hours to fully evaporate the solvent to obtain a semi-solidified film.
[0103] The glass sheet loaded with the semi-cured film after the solvent has evaporated is placed in a vacuum oven, and the temperature is adjusted to carry out a multi-stage curing reaction. The temperature and time of each stage are: 180°C for two hours, 200°C for two hours, and 230°C for four hours. After natural cooling, the cured film is obtained.
[0104] Soak the glass slide with the cured film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on aluminum foil.
[0105] The film together with the aluminum foil was placed in a vacuum oven and dried at a high temperature of 120° C. for 10 hours to obtain a PEI / BPABMI (75 / 25) semi-interpenetrating network dielectric film.
[0106] Test Example 2
[0107] The energy storage density, electrical constant and dielectric loss of the PEI / BPABMI (75 / 25) semi-interpenetrating network dielectric film prepared in Example 2 were tested as a function of frequency.
[0108] Results Figure 1 and Figure 5 ,according to Figure 1 and Figure 5 It can be seen that the PEI / BPABMI (75 / 25) semi-IPN dielectric film has high energy storage density and efficiency at 150°C. When the electric field strength is 600MV / m, the charge and discharge efficiency is still 91.1%, and the discharge energy density is 5.19J / cm 3 . When the frequency is 1MHz, the dielectric constant is 3.39 and the dielectric loss is 0.010.
[0109] The SEM image is shown in Fig. 9 It can be seen that PEI and BPABMI have excellent compatibility, no microscopic phase separation occurs, showing a homogeneous structure, and the film has excellent toughness, and the brittle fracture section in liquid nitrogen still shows a ductile fracture.
[0110] Example 3
[0111] An embodiment of the present invention provides a method for preparing a semi-interpenetrating network dielectric film, comprising:
[0112] Weigh 0.17 g of polyetherimide (PEI), 0.03 g of bisphenol A bismaleimide (BPABMI), and 0.0003 g of di-tert-butylperoxyisopropylbenzene (BIPB), and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0113] The above solution was heated to 50° C. under magnetic stirring and dissolved and dispersed for 8 hours to allow the solute to be fully and uniformly dissolved in the solvent.
[0114] Clean the glass slide to avoid dust contamination, then put the glass slide in a 70℃ oven to preheat for half an hour, then use a rubber-tipped dropper to draw 5 ml of film-making liquid and apply it on the glass slide, let the glass slide be baked in a 70℃ oven for 10 hours to fully evaporate the solvent to obtain a semi-solidified film.
[0115] After the solvent evaporates, the glass sheet loaded with the semi-cured film is placed in a vacuum oven, and the temperature is adjusted to carry out a multi-stage curing reaction. The temperature and time of each stage are: 180°C for two hours, 200°C for two hours, and 230°C for four hours. After natural cooling, the cured film is obtained.
[0116] Soak the glass slide with the cured film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on aluminum foil.
[0117] The film together with the aluminum foil was placed in a vacuum oven and dried at a high temperature of 120° C. for 10 hours to obtain a PEI / BPABMI (85 / 15) semi-interpenetrating network dielectric film.
[0118] Test Example 3
[0119] The energy storage density, dielectric constant and dielectric loss of the PEI / BPABMI (85 / 15) semi-interpenetrating network dielectric film prepared in Example 3 were tested as a function of frequency.
[0120] Results Figure 1 and Figure 5 ,according to Figure 1 and Figure 5 It can be seen that the PEI / BPABMI (85 / 15) semi-IPN dielectric film has high energy storage density and efficiency at 150°C. When the electric field strength is 600MV / m, the charge and discharge efficiency is still 91.2%, and the discharge energy density is 5.83J / cm 3 . When the frequency is 1MHz, the dielectric constant is 3.42 and the dielectric loss is 0.012.
[0121] Example 4
[0122] An embodiment of the present invention provides a method for preparing a semi-interpenetrating network dielectric film, comprising:
[0123] Weigh 0.18 g of polyetherimide (PEI), 0.02 g of N,N'-4,4'-diphenylmethane bismaleimide (BDMBMI), and 0.0002 g of di-tert-butylperoxyisopropylbenzene (BIPB), and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0124] The above solution was heated to 50° C. under magnetic stirring and dissolved and dispersed for 8 hours to allow the solute to be fully and uniformly dissolved in the solvent.
[0125] Clean the glass slide to avoid dust contamination, then put the glass slide in a 70℃ oven to preheat for half an hour, then use a rubber-tipped dropper to absorb 5 ml of film-making liquid and apply it to the glass slide, and let the glass slide be baked in a 70℃ oven for 10 hours to allow the solvent to fully evaporate.
[0126] After the solvent evaporates, the glass sheet loaded with the semi-cured film is placed in a vacuum oven, and the temperature is adjusted to carry out a multi-stage curing reaction. The temperature and time of each stage are: 180°C for two hours, 200°C for two hours, and 230°C for four hours. After natural cooling, the cured film is obtained.
[0127] Soak the glass slide with the cured film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on aluminum foil.
[0128] The film together with the aluminum foil was placed in a vacuum oven and dried at a high temperature of 120° C. for 10 hours to obtain a PEI / BDMBMI (90 / 10) semi-interpenetrating network dielectric film.
[0129] Test Example 4
[0130] The energy storage density of the PEI / BDMBMI (90 / 10) semi-interpenetrating network dielectric film prepared in Example 4 was tested. The results are as follows: Figure 1 As shown in the figure, it has high energy storage density and efficiency at 150°C. When the electric field strength is 650MV / m, the charge and discharge efficiency is still 90.5%, and the discharge energy density is 6.70J / cm 3 .
[0131] Example 5
[0132] An embodiment of the present invention provides a method for preparing a semi-interpenetrating network dielectric film, comprising:
[0133] Weigh 0.18 g of polysulfone (PSU), 0.02 g of bisphenol A bismaleimide (BPABMI), and 0.0002 g of di-tert-butylperoxyisopropylbenzene (BIPB), and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0134] The above solution was heated to 50° C. under magnetic stirring and dissolved and dispersed for 8 hours to allow the solute to be fully and uniformly dissolved in the solvent.
[0135] Clean the glass slide to avoid dust contamination, then put the glass slide in a 70℃ oven to preheat for half an hour, then use a rubber-tipped dropper to absorb 5 ml of film-making liquid and apply it to the glass slide, and let the glass slide be baked in a 70℃ oven for 10 hours to allow the solvent to fully evaporate.
[0136] After the solvent evaporates, the glass sheet loaded with the semi-cured film is placed in a vacuum oven, and the temperature is adjusted to carry out a multi-stage curing reaction. The temperature and time of each stage are: 180°C for two hours, 200°C for two hours, and 230°C for four hours. After natural cooling, the cured film is obtained.
[0137] Soak the glass slide with the cured film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on aluminum foil.
[0138] The film together with the aluminum foil was placed in a vacuum oven and dried at a high temperature of 120° C. for 10 hours to obtain a PSU / BPABMI (90 / 10) semi-interpenetrating network dielectric film.
[0139] Test Example 5
[0140] The energy storage density of the PSU / BPABMI (90 / 10) semi-IPN dielectric film prepared in Example 5 was tested. The results are shown in Figure 2 .like Figure 2 As shown in the figure, it has high energy storage density and efficiency at 150°C. When the electric field strength is 600MV / m, the charge and discharge efficiency is still 90.5%, and the discharge energy density is 6.92J / cm 3 .
[0141] Example 6
[0142] An embodiment of the present invention provides a method for preparing a semi-interpenetrating network dielectric film, comprising:
[0143] Weigh 0.15 g of polysulfone (PSU), 0.05 g of bisphenol A maleimide (BPABMI), and 0.00025 g of di-tert-butylperoxyisopropylbenzene (BIPB), and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0144] The above solution was heated to 50° C. under magnetic stirring and dissolved and dispersed for 8 hours to allow the solute to be fully and uniformly dissolved in the solvent.
[0145] Clean the glass slide to avoid dust contamination, then put the glass slide in a 70℃ oven to preheat for half an hour, then use a rubber-tipped dropper to draw 5 ml of film-making liquid and apply it on the glass slide, let the glass slide be baked in a 70℃ oven for 10 hours to fully evaporate the solvent to obtain a semi-solidified film.
[0146] After the solvent evaporates, the glass sheet loaded with the semi-cured film is placed in a vacuum oven, and the temperature is adjusted to carry out a multi-stage curing reaction. The temperature and time of each stage are: 180°C for two hours, 200°C for two hours, and 230°C for four hours. After natural cooling, the cured film is obtained.
[0147] Soak the glass slide with the cured film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on aluminum foil.
[0148] The film together with the aluminum foil was placed in a vacuum oven and dried at a high temperature of 120° C. for 10 hours to obtain a PSU / BPABMI (75 / 25) semi-interpenetrating network dielectric film.
[0149] Test Example 6
[0150] The energy storage density of the PSU / BPABMI (75 / 25) semi-IPN dielectric film prepared in Example 6 was tested. The results are shown in Figure 2 .like Figure 2 As shown in the figure, it has high energy storage density and efficiency at 150°C. When the electric field strength is 600MV / m, the charge and discharge efficiency is still 90%, and the discharge energy density is 6.05J / cm 3 .
[0151] Example 7
[0152] An embodiment of the present invention provides a method for preparing a semi-interpenetrating network dielectric film, comprising:
[0153] Weigh 0.15 g of polyetherimide (PEI), 0.05 g of bisphenol A bismaleimide (BPABMI), 0.0005 g of di-tert-butylperoxyisopropylbenzene (BIPB), and 0.002 g of aluminum oxide (Al2O3), and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0154] The above solution was heated to 50° C. under magnetic stirring and dissolved and dispersed for 8 hours to allow the solute to be fully and evenly dissolved in the solvent and the filler to be evenly dispersed in the solvent.
[0155] Clean the glass slide to avoid dust contamination, then put the glass slide in a 70℃ oven to preheat for half an hour, then use a rubber-tipped dropper to draw 5 ml of film-making liquid and apply it on the glass slide, let the glass slide be baked in a 70℃ oven for 10 hours to fully evaporate the solvent to obtain a semi-solidified film.
[0156] After the solvent evaporates, the glass sheet loaded with the semi-cured film is placed in a vacuum oven, and the temperature is adjusted to carry out a multi-stage curing reaction. The temperature and time of each stage are: 180°C for two hours, 200°C for two hours, and 230°C for four hours. After natural cooling, the cured film is obtained.
[0157] Soak the glass slide with the cured film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on aluminum foil.
[0158] The film together with the aluminum foil was placed in a vacuum oven and dried at a high temperature of 120° C. for 10 hours to obtain a PEI / BPABMI / Al2O3 (75 / 25 / 1) semi-interpenetrating network polymer dielectric film.
[0159] Test Example 7
[0160] The energy storage density, dielectric constant and dielectric loss of the PEI / BPABMI / Al2O3 (75 / 25 / 1) semi-interpenetrating network dielectric film prepared in Example 7 were tested as a function of frequency.
[0161] Results Figure 3 and Figure 6 .like Figure 3 As shown in the figure, it has high energy storage density and efficiency at 150°C. When the electric field strength is 550MV / m, the charge and discharge efficiency is still 90%, and the discharge energy density is 5.05J / cm 3 .according to Figure 6 It can be seen that when the frequency is 1 MHz, the dielectric constant is 3.47 and the dielectric loss is 0.014.
[0162] Example 8
[0163] An embodiment of the present invention provides a method for preparing a semi-interpenetrating network dielectric film, comprising:
[0164] Weigh 0.15 g of polyetherimide (PEI), 0.05 g of bisphenol A bismaleimide (BPABMI), 0.0005 g of di-tert-butylperoxyisopropylbenzene (BIPB), and 0.002 g of NTCDA, and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0165] The above solution was heated to 50° C. under magnetic stirring and dissolved and dispersed for 8 hours to allow the solute to be fully and uniformly dissolved in the solvent.
[0166] Clean the glass slide to avoid dust contamination, then put the glass slide in a 70℃ oven to preheat for half an hour, then use a rubber-tipped dropper to absorb 5 ml of film-making liquid and apply it to the glass slide, and let the glass slide be baked in a 70℃ oven for 10 hours to allow the solvent to fully evaporate.
[0167] After the solvent evaporates, the glass sheet is placed in a vacuum oven and the temperature is adjusted to carry out a multi-stage curing reaction. The temperature and time of each stage are: 180°C for two hours, 200°C for two hours, and 230°C for four hours. After natural cooling, a cured film is obtained.
[0168] Soak the glass slide with the cured film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on aluminum foil.
[0169] The film together with the aluminum foil was placed in a vacuum oven and dried at 120° C. for 10 hours to obtain a PEI / BPABMI / NTCDA (75 / 25 / 1) semi-interpenetrating network polymer dielectric film.
[0170] Test Example 8
[0171] The energy storage density, dielectric constant and dielectric loss of the PEI / BPABMI / NTCDA (75 / 25 / 1) semi-interpenetrating network dielectric film prepared in Example 8 were tested as a function of frequency.
[0172] Results Figure 3 and Figure 6 .according to Figure 3 It can be seen that at 150°C, it has high energy storage density and efficiency. When the electric field strength is 550MV / m, the charge and discharge efficiency is still 91.1%, and the discharge energy density is 5.18J / cm 3 .according to Figure 6 It can be seen that when the frequency is 1 MHz, the dielectric constant is 3.49 and the dielectric loss is 0.018.
[0173] Comparative Example 1
[0174] This comparative example provides a method for preparing a dielectric film, comprising:
[0175] Weigh 0.2 g of polyetherimide (PEI) and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0176] The glass bottle containing the membrane-forming solution was placed on a magnetic stirring table heated at 50° C. and stirred for 8 hours to allow the solute to be fully and uniformly dissolved in the solvent.
[0177] Clean the glass slide to avoid dust contamination, and then put the glass slide in a 70℃ oven to preheat for half an hour. Then use a rubber-tipped dropper to suck 1 drop of 5 ml of film-making liquid and apply it on the glass slide. Let the glass slide be baked in a 70℃ oven for 10 hours to fully evaporate the solvent to obtain a pure PEI film.
[0178] The glass sheet from which the solvent has evaporated is placed in a vacuum oven and baked at 200° C. for 12 hours to further remove any possible residual solvent, and after natural cooling, a thermoplastic PEI film from which the solvent is completely removed is obtained.
[0179] Soak the glass slide with PEI film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on aluminum foil.
[0180] The aluminum foil wrapped with the film was placed in a vacuum oven and dried at a high temperature of 120° C. for 10 hours to obtain a PEI thermoplastic film.
[0181] Test Example 9
[0182] The energy storage density of the PEI thermoplastic film prepared in Comparative Example 1 was tested. The results are shown in Figure 4 ,like Figure 4 As shown in the figure, the energy storage density and efficiency at 150°C are both low. Specifically, when the electric field strength is 600MV / m, the charge and discharge efficiency is only 72.4%, and the discharge energy density is 5.28J / cm 3 , which is significantly lower than the energy storage performance corresponding to the dielectric film with a semi-interpenetrating network structure in the above embodiments.
[0183] Comparative Example 2
[0184] This comparative example provides a method for preparing a dielectric film, comprising:
[0185] Weigh 0.2 g of polysulfone (PSU) and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0186] The glass bottle containing the membrane-forming solution was placed on a magnetic stirring table heated at 50° C. and stirred for 8 hours to allow the solute to be fully and uniformly dissolved in the solvent.
[0187] Clean the glass slide to avoid dust contamination, then put the glass slide in a 70℃ oven to preheat for half an hour, then use a rubber-tipped dropper to draw 5 ml of film-making liquid and apply it on the glass slide, let the glass slide be baked in a 70℃ oven for 10 hours to allow the solvent to fully evaporate to obtain a PSU film.
[0188] The glass sheet after the solvent evaporated was placed in a vacuum oven and baked at 200° C. for 12 hours to further remove the residual solvent as much as possible, and then naturally cooled to obtain a film.
[0189] Soak the glass slide with the cured film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on aluminum foil.
[0190] The film together with the aluminum foil was placed in a vacuum oven and dried at a high temperature of 120° C. for 10 hours to obtain a PSU thermoplastic film.
[0191] Test Example 10
[0192] The energy storage density of the PSU thermoplastic film prepared in Comparative Example 2 was tested. The results are shown in Figure 4 ,like Figure 4 As shown in Figure 2, the energy storage density and efficiency at 150°C are both low. Specifically, when the electric field strength is 550MV / m, the charge and discharge efficiency is only 77.5%, and the discharge energy density is 4.99J / cm 3 , which is significantly lower than the energy storage performance corresponding to the dielectric film with a semi-interpenetrating network structure in the above embodiments.
[0193] Comparative Example 3
[0194] This comparative example provides a method for preparing a dielectric film, comprising:
[0195] Weigh 0.15 g of polyetherimide (PEI), 0.05 g of polyphenylene ether (PPE), and 0.0005 g of di-tert-butylperoxyisopropylbenzene (BIPB), and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0196] The glass bottle containing the membrane-forming solution was placed on a magnetic stirring table heated at 50° C. and stirred for 8 hours to allow the solute to be fully and uniformly dissolved in the solvent.
[0197] Clean the glass slide to avoid dust contamination, then put the glass slide in a 70℃ oven to preheat for half an hour, then use a rubber-tipped dropper to draw 5 ml of film-making liquid and apply it on the glass slide, let the glass slide be baked in a 70℃ oven for 10 hours to fully evaporate the solvent to obtain a semi-solidified film.
[0198] After the solvent evaporates, the glass sheet loaded with the semi-cured film is placed in a vacuum oven, and the temperature is adjusted to carry out a multi-stage curing reaction. The temperature and time of each stage are: 170°C for two hours, 200°C for eight hours, and the cured film is obtained after natural cooling.
[0199] Soak the glass slide with the cured film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on aluminum foil.
[0200] The above film together with aluminum foil was placed in a vacuum oven and dried at a high temperature of 120° C. for 10 hours to obtain a PEI / PPE (75 / 25) thermoplastic / thermosetting blend film.
[0201] Test Example 11
[0202] The energy storage density of the PEI / PPE (75 / 25) thermoplastic / thermosetting blend film prepared in Comparative Example 3 was tested. The results are shown in Figure 4 .like Figure 4 As shown in Figure 2, at 150°C, both the energy storage density and efficiency are low. Specifically, when the electric field strength is 550 MV / m, the charge and discharge efficiency is only 88%, and the discharge energy density is 4.94 J / cm 3 . For a graph of the dielectric constant and dielectric loss versus frequency, see Figure 7 .according to Figure 7 It can be seen that when the frequency is 1MHz, the dielectric constant is 3.03 and the dielectric loss is 0.01. The microstructure of PEI / PPE (75 / 25) is as follows: Figure 8 As shown, due to the poor compatibility of PEI and PPE, microphase separation occurs, resulting in no interpenetrating network structure. The corresponding energy storage performance is significantly lower than that of the dielectric film with a semi-interpenetrating network structure in the above embodiments.
[0203] Comparative Example 4
[0204] This comparative example provides a method for preparing a dielectric film, comprising:
[0205] Weigh 0.15 g of polyetherimide (PEI), 0.028 g of DCPD epoxy resin, 0.022 g of SN485 phenolic curing agent), 0.00025 g of 2E4MZ catalyst, and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0206] The glass bottle containing the membrane-forming solution was placed on a magnetic stirring table heated at 50° C. and stirred for 8 hours to allow the solute to be fully and uniformly dissolved in the solvent.
[0207] Clean the glass slide to avoid dust contamination, then put the glass slide in a 70℃ oven to preheat for half an hour, then use a rubber-tipped dropper to draw 5 ml of film-making liquid and apply it on the glass slide, let the glass slide be baked in a 70℃ oven for 10 hours to evaporate the solvent to obtain a semi-cured film.
[0208] After the solvent evaporates, the glass sheet loaded with the semi-cured film is placed in a vacuum oven, and the temperature is adjusted to carry out a multi-stage curing reaction. The temperature and time of each stage are: 130°C for half an hour, 180°C for two hours, and 200°C for eight hours. After natural cooling, the cured film is obtained.
[0209] Soak the glass slide with the cured film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on aluminum foil.
[0210] The film together with the aluminum foil was placed in a vacuum oven and dried at a high temperature of 120° C. for 10 hours to obtain a PEI / Epoxy (75 / 25) thermoplastic / thermosetting blend film.
[0211] Test Example 12
[0212] The energy storage density of the thermoplastic / thermosetting blended film PEI / Epoxy (75 / 25) prepared in Comparative Example 4 was tested. Figure 4 .like Figure 4 As shown in Figure 2, at 150°C, the energy storage density and energy storage efficiency are both low. Specifically, when the electric field strength is 550 MV / m, the charge and discharge efficiency is only 78%, and the discharge energy density is 4.96 J / cm 3 Since the bismaleimide resin is replaced by epoxy resin, even if an interpenetrating network structure is formed, the high-temperature energy storage performance is significantly lower than that of the dielectric film of the semi-interpenetrating network structure based on BMI in the above-mentioned embodiments.
[0213] Comparative Example 5
[0214] This comparative example provides a method for preparing a dielectric film, comprising:
[0215] Weigh 0.15 g of polyphenylene sulfone (PPSU), 0.05 g of bisphenol A bismaleimide (BPABMI), and 0.0005 g of di-tert-butylperoxyisopropylbenzene (BIPB), and add 10 ml of N-methylpyrrolidone (NMP) to prepare a solution.
[0216] The glass bottle containing the membrane-forming solution was placed on a magnetic stirring table heated at 50° C. and stirred for 8 hours to allow the solute to be fully and uniformly dissolved in the solvent.
[0217] Clean the glass slide to avoid dust contamination, then put the glass slide in a 70℃ oven to preheat for half an hour, then use a rubber-tipped dropper to draw 5 ml of film-making liquid and apply it on the glass slide, let the glass slide be baked in a 70℃ oven for 10 hours to fully evaporate the solvent to obtain a semi-solidified film.
[0218] After the solvent evaporates, the glass sheet loaded with the semi-cured film is placed in a vacuum oven, and the temperature is adjusted to carry out a multi-stage curing reaction. The temperature and time of each stage are: 180°C for two hours, 200°C for two hours, and 230°C for four hours. After natural cooling, a cured film is obtained.
[0219] Soak the glass slide with the cured film in deionized water. After a period of time, the film will fall off the glass slide by itself. Place the fallen film on an aluminum foil bag.
[0220] The film together with the aluminum foil was placed in a vacuum oven and dried at a high temperature of 120°C for 10 hours to obtain a PPSU / BPABMI (75 / 25) thermoplastic / thermosetting blend film.
[0221] Test Example 13
[0222] The energy storage density of the PPSU / BPABMI (75 / 25) thermoplastic / thermosetting blend film prepared in Comparative Example 5 was tested. The results are shown in Figure 4 .according to Figure 4 It can be seen that the energy storage density and energy storage efficiency at 150°C are both low. Specifically, when the electric field strength is 550MV / m, the charge and discharge efficiency is only 84.8%, and the discharge energy density is 4.79J / cm 3 Due to the large difference in molecular structure between PPSU and BPABMI, microphase separation occurs and no interpenetrating network structure is formed. The high-temperature energy storage performance is significantly lower than that of the semi-interpenetrating network structure dielectric film in the above-mentioned embodiments. The change of dielectric constant and dielectric loss with frequency is shown in Figure 2. Figure 7 .according to Figure 7 It can be seen that when the frequency is 1 MHz, the dielectric constant is 3.35 and the dielectric loss is 0.01.
[0223] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A semi-interpenetrating network dielectric film, It is characterized in that The material is prepared by the following raw materials, wherein the raw materials are composed of a thermoplastic polymer, a bismaleimide resin and a catalyst, wherein the thermoplastic polymer includes any one of polyetherimide, polysulfone and polyamide ether imide; the catalyst is selected from di-tert-butyl peroxyisopropylbenzene; the mass ratio of the thermoplastic polymer to the bismaleimide resin is (1.8:1)-(19:1), and the amount of the catalyst is 0.05-2wt% of the amount of the bismaleimide resin; The bismaleimide resin is selected from the compounds shown in the following structural formula: , R 1 Select any one of the following structural formulas: , , , and , wherein n represents the number of repeating units, and n is 1-10; The preparation method of the semi-interpenetrating network dielectric film includes: mixing a thermoplastic polymer, a bismaleimide resin and a catalyst, and then coating it on a substrate, and then drying it to form an uncured film, and then performing multi-stage temperature curing; the multi-stage temperature curing includes: curing at 150-190°C for 1.5-2.5 hours, then curing at 200-215°C for 1.5-2.5 hours, and then curing at 220-250°C for 3-4 hours.
2. The semi-interpenetrating network dielectric film according to claim 1, It is characterized in that The mass ratio of the thermoplastic polymer to the bismaleimide resin is (7:3)-(9:1).
3. The semi-interpenetrating network dielectric film according to claim 1, It is characterized in that The amount of the catalyst used is 0.1-1 wt % of the amount of the bismaleimide resin used.
4. A semi-interpenetrating network composite film, It is characterized in that The semi-interpenetrating network composite material is prepared by raw materials consisting of nanofillers, molecular semiconductors, thermoplastic polymers, bismaleimide resins and catalysts, wherein the mass ratio of the thermoplastic polymer to the bismaleimide resin is (1.8:1)-(19:1), the amount of the catalyst is 0.05-2wt% of the amount of the bismaleimide resin; the amount of the nanofiller added is 0-5wt% of the total mass, the amount of the molecular semiconductor added is 0-3wt% of the total mass, and the nanofiller and the molecular semiconductor contain at least one; the thermoplastic polymer includes any one of polyetherimide, polysulfone and polyamide ether imide; the bismaleimide resin is selected from the compounds shown in the following structural formula: , R 1 Select any one of the following structural formulas: , , , and , wherein n represents the number of repeating units, and n is 1-10; the catalyst is selected from di-tert-butyl peroxyisopropylbenzene; The preparation method of the semi-interpenetrating network composite material film comprises: mixing nano fillers, molecular semiconductors, thermoplastic polymers, bismaleimide resins and catalysts, coating them on a substrate, drying them to form an uncured film, and then curing them at multiple temperatures; The multi-stage temperature curing includes: curing at 150-190°C for 1.5-2.5 hours, then curing at 200-215°C for 1.5-2.5 hours, and then curing at 220-250°C for 3-4 hours.
5. The semi-interpenetrating network composite film according to claim 4, It is characterized in that The mass ratio of the thermoplastic polymer to the bismaleimide resin is (7:3)-(9:1); The amount of the catalyst used is 0.1-1wt% of the amount of the bismaleimide resin used; The amount of the nanofiller added is 0.5-1.5wt% of the total mass; The added amount of the molecular semiconductor is 0.5-1.0 wt % of the total mass.
6. The semi-interpenetrating network composite film according to claim 5, It is characterized in that The nano filler includes at least one of nano aluminum oxide, nano silicon dioxide, nano boron nitride, nano titanium dioxide, nano magnesium oxide and nano hafnium dioxide.
7. The semi-interpenetrating network composite film according to claim 6, It is characterized in that The particle size of the nanofiller of nano-boron nitride is 0.1-100 μm, and the particle size of other nanofillers except nano-boron nitride is 5-100 nm.
8. The semi-interpenetrating network composite film according to claim 7, It is characterized in that The particle size of the nano-filler of nano-boron nitride is 1 μm; the particle size of other nano-fillers except nano-boron nitride is 10-50 nm.
9. The semi-interpenetrating network composite film according to claim 4, It is characterized in that The molecular semiconductor includes any one of aromatic ester compounds, aromatic acid anhydride compounds, perylene compounds, quinone compounds and aromatic phenanthene compounds.
10. The semi-interpenetrating network composite film according to claim 9, It is characterized in that The molecular semiconductor includes one of [6,6]-phenyl-C61-butyric acid methyl ester, [6,6]-phenyl C71 butyric acid methyl ester, 1,4,5,8-naphthalenetetracarboxylic anhydride, 2,6-dibromonaphthalene-1,4,5,8-tetracarboxylic dianhydride, 1,7-dibromo-3,4,9,10-perylenetetracarboxylic dianhydride, 1,6,7,12-tetrachloro-3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,5,6-tetrafluoro-7,7,8,8-tetracyanodimethyl-p-benzoquinone, and tribenzo[de,kl,rst]pentaphen.
Citation Information
Patent Citations
Polyimide resin composition modified by thermosetting resin
CN101235200A
Fluorine-containing low-dielectric-loss bismaleimide resin, and preparation method and application thereof
CN104479130A
Semi-interpenetrating polymer network polyimide resin composition and film-like adhesive prepared from same
CN106905914A
Polyester imide modified dimaleimide
CN1371941A
Thermosetting resin composition
JP1989289862A