A geological drill bit with gauge protection structure and its manufacturing method
By welding the inner and outer gauge protection blocks to the drill teeth, and combining cold pressing and low-temperature sintering processes, the gauge protection problem of geological drill bits was solved, improving the strength and lifespan of the drill bits and reducing production costs.
Patent Information
- Application Number
- CN202311811583.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-26
AI Technical Summary
Existing geological drill bits have deficiencies in their gauge protection structure, resulting in poor bonding force between the drill teeth and the steel body, short drill bit life, and high production costs.
The design incorporates an inner and outer sprue retaining blocks welded to the drill teeth, combined with cold pressing and low-temperature sintering processes to form a three-layer drill tooth structure. A welding platform and welding limiting structure are installed on the steel body to improve the bonding strength and wear resistance between the drill teeth and the steel body.
It improves the strength and bonding force of drill teeth, reduces drill tooth breakage accidents, lowers production costs, and increases the service life and drilling efficiency of drill bits.
Smart Images

Figure CN117722135B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to geological drill bits used in geological exploration or engineering exploration drilling, specifically to a geological drill bit with a gauge protection structure and its manufacturing method. Background Technology
[0002] Currently, the vast majority of tools used in solid mineral exploration and engineering exploration are diamond geological drill bits. There are two main methods for manufacturing existing diamond geological drill bits:
[0003] One method is the medium-frequency integral hot-pressing sintering method. In this method, a mixture of diamond and metal powder is first poured into a pre-designed graphite mold. A steel blank is then placed on the powder, and a medium-frequency hot-pressing sintering machine is used to heat and pressurize the mixture using medium-frequency electromagnetic induction, sintering the metal powder and diamond into drill teeth that are then bonded to the steel body. This method has the following drawbacks: ① Due to the integral sintering process, uneven internal structures such as the sprue result in uneven overall density. ② The sintered density is relatively low, leading to poor bonding between the drill teeth and the steel body. ③ The bonding strength between the drill teeth and the steel body is affected by parameters such as the transition layer composition, the steel material, and the sintering temperature. Furthermore, the temperature of medium-frequency induction sintering exhibits a skin effect, resulting in temperature differences between the inside and outside of the sintering chamber. To ensure the bonding strength between the drill teeth and the steel body, it is sometimes necessary to increase the sintering temperature. However, high-temperature sintering leads to diamond loss, reducing sharpness and lifespan, and also increases energy consumption. ④ The graphite mold experiences high wear during the sintering process, resulting in high production costs.
[0004] Another method is electroplating. Electroplating uses a sand-embedding method, depositing diamonds onto the surface of a steel body, directly depositing layers of nickel to coat the diamonds and form the drill bit structure. While this method avoids high-temperature damage to the diamonds, it has significant drawbacks: firstly, the electroplated layer has high stress and is prone to delamination if not handled properly; secondly, the diamond concentration is uncontrollable and cannot be adjusted to suit different rocks; thirdly, the production cycle is too long, typically requiring 7-15 days per batch; and finally, electroplating produces significant pollution, resulting in drill bits with good sharpness but a shorter lifespan.
[0005] The applicant's previous research, disclosed in invention patent CN103953286A, revealed a welded high-matrix geological drill bit and its manufacturing method, comprising high-matrix drill teeth, sprue blocks, and a steel body. The high-matrix drill teeth and sprue blocks are sintered separately and then tightly joined to form drill tooth crowns, which are laser-welded onto the steel body. The high-matrix drill teeth consist of a working tooth layer containing rock-breaking abrasive particles, a transition tooth layer without abrasive particles, and a welded tooth layer without abrasive particles. The total height of the high-matrix drill teeth is 15–35 mm. The sprue blocks can be manufactured by sintering elemental powders, various metal powders, or alloy powders. This invention, by employing independent sintering of high-matrix drill teeth and designing an adaptive wear nozzle block, significantly reduces sintering temperature, minimizes diamond damage, and increases drill tooth height, resulting in substantial improvements in drilling efficiency and lifespan. However, this application suffers from a gauge retention issue. Because the weld layer, designed to enhance bonding strength, typically lacks diamond, it is prone to wear at the root of the weld layer during high-speed drill operation, leading to tooth loss and failure before the drill teeth are fully consumed. Even if the gauge retention issue could be addressed by embedding polycrystalline diamonds on the inner and outer surfaces of the drill teeth, this mechanically embedded polycrystalline diamond gauge retention method has a small area and is not ideal. Summary of the Invention
[0006] The technical problem to be solved by the present invention is to provide a geological drill bit with a gauge-maintaining structure that can solve the problem of gauge maintenance in geological drill bits, and a method for manufacturing the same.
[0007] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0008] A geological drill bit with a gauge protection structure includes drill teeth and a steel body. The drill teeth have a three-layer structure in the axial direction: a working layer, a transition layer, and a welded layer. One end of the steel body is provided with a connecting thread, and the drill teeth are evenly distributed at the other end of the steel body. Unlike existing technologies, the following features are provided:
[0009] It also includes an inner water inlet retaining block and an outer water inlet retaining block, wherein the inner water inlet retaining block is provided with an inner water groove and the outer water inlet retaining block is provided with an outer water groove; both the inner water inlet retaining block and the outer water inlet retaining block are sintered from powder containing abrasive particles;
[0010] Multiple welding platforms are machined circumferentially on the end face of the other end of the steel body, and the drill teeth are welded to the welding platforms; the end face of the steel body between two adjacent drill teeth is also machined with inner welding grooves and outer welding grooves for welding the inner sprue gauge block and the outer sprue gauge block, and there is a welding limiting structure between the inner welding grooves and the outer welding grooves. The top end face of the welding limiting structure is higher than the welding platform. The inner sprue gauge block, the welding limiting structure and the outer sprue gauge block between two adjacent drill teeth together constitute a sprue block;
[0011] After the welding of the inner sprue gauge block, the outer sprue gauge block, and the drill teeth is completed, the plane containing the top end face of the sprue block is higher than the plane containing the top of the welded layer on the drill teeth in the axial direction of the drill bit.
[0012] The depth of the inner and outer welding grooves can be selected according to the drilling object and the specifications of the drill pipe, and is usually 6 to 10 mm; the depth of the inner and outer water channels can be selected according to the drilling object, and is usually 1 to 5 mm, so as to effectively circulate coolant and prevent drill burn-out.
[0013] To improve the bonding strength between the transition layer and the working layer of the drill bit, a boss extending from the transition layer to the working layer can be provided between them, acting as a reinforcing rib. Similarly, from the perspective of improving the bonding strength between the weld layer and the transition layer, it is preferable to provide a boss extending from the weld layer to the transition layer between them.
[0014] Furthermore, the height of the top end face of the welding limiting structure beyond the welding platform is preferably greater than the height of the drill tooth welding layer, so that the drill tooth can withstand greater torque during operation.
[0015] Preferably, the working layer of the drill bit is designed to have a structure in the radial direction consisting of an inner working layer containing abrasive particles, a first interlayer without abrasive particles, a middle working layer containing abrasive particles, a second interlayer without abrasive particles, and an outer working layer containing abrasive particles. This can further improve drilling efficiency and the service life of the drill bit.
[0016] The abrasive grains involved in this application may be diamond, polycrystalline, or a mixture of diamond and polycrystalline.
[0017] In the specific implementation process, when the total height of the drill teeth is selected as 10-30mm, the preferred height of the drill tooth welding layer is 2-3mm, the height of the transition layer is 2-3mm, and the remainder is the height of the working layer (6-24mm); correspondingly, the matching height of the sprue block is 6-10mm.
[0018] The method for preparing a geological drill bit with a gauge protection structure as described above includes the following steps:
[0019] 1) Take steel for making the steel body, machine connecting threads at one end of the steel, and machine multiple welding platforms circumferentially on the end face of the other end of the steel body. The welding platforms are evenly distributed on the end face of the steel body. Then, machine inner and outer welding grooves for welding the inner and outer sprue gauge blocks on the end face of the steel body between two adjacent welding platforms. There is a welding limiting structure between the inner and outer welding grooves. The top end face of the welding limiting structure is higher than the welding platform to obtain the steel body.
[0020] 2) The drill teeth cold-pressed blanks are made by cold pressing forming process, and the resulting cold-pressed blanks are sintered in batches at 830-860℃ to obtain drill teeth;
[0021] 3) Cold pressing molding process is used to make cold pressing blanks of inner nozzle gauge block and outer nozzle gauge block respectively. The cold pressing blanks are sintered in batches at 830-860℃ to obtain inner nozzle gauge block and outer nozzle gauge block.
[0022] 4) Weld the drill teeth, the inner water inlet gauge block, and the outer water inlet gauge block to the welding platform, the inner welding groove, and the outer welding groove of the steel body, respectively, to obtain the geological drill bit with gauge protection structure.
[0023] Compared with the prior art, the present invention is characterized by:
[0024] 1. The inner and outer nozzle gauge blocks are sintered from abrasive powder and then welded to the corresponding inner and outer welding grooves. The nozzle block, which is composed of the inner nozzle gauge block, the welding limiting structure, and the outer nozzle gauge block, is similar to the working surface of a borehole expander. Compared with the traditional gauge protection method of mechanically embedding diamond polycrystals on each drill tooth, it has a larger area and better protection effect. It can not only protect the wear of the weld layer of the drill teeth, but also effectively protect the wear of the working parts of the steel body, so that the drilled hole diameter is consistent and the subsequent drilling work is smooth.
[0025] 2. A welding platform is designed on the end face of the steel body. The plane containing the top face of the nozzle block, which consists of an inner nozzle gauge block, a welding limiting structure, and an outer nozzle gauge block, is higher than the plane containing the top of the weld layer on the drill bit, forming an inlaid structure. This allows the drill bit to withstand greater torsional forces during operation. The drill bit is designed as an axial three-layer structure. The weld layer ensures the welding strength between the drill bit and the steel body, and the transition layer ensures the bonding force between the weld layer and the working layer. Furthermore, by designing bosses that act as reinforcing ribs at the junctions of the transition layer and the working layer, and between the transition layer and the weld layer, the bonding force between them is improved. These designs effectively improve the strength of the drill bit and the connection strength between the drill bit and the steel body, thereby effectively dealing with complex working conditions in different strata, reducing drill bit breakage accidents, and improving product reliability.
[0026] 3. In the manufacturing method described in this invention, the drill teeth, inner sprue gauge block, and outer sprue gauge block are individually cold-pressed and then batch-sintered. Compared with the traditional integral medium-frequency hot pressing sintering, this method results in higher internal density and better uniformity. The sintering temperature is reduced from 910–950℃ required for integral medium-frequency hot pressing sintering to 830–860℃, and the sintering time is reduced from 20–25 minutes to 10–15 minutes. This results in less diamond damage and better drill bit performance. Furthermore, the graphite mold used in sintering production is a modular design that can be reused (5–10 times), while the mold for integral sintering is larger, and most cores can only be used once. Therefore, the method described in this invention significantly reduces costs.
[0027] 4. The advantages of the method described in this invention are more pronounced in large-diameter drill bits (such as those with a diameter of Φ96mm or larger). If large-diameter drill bits are produced using traditional methods, firstly, the sintering induction coil needs to be larger, resulting in greater energy loss, a more significant temperature difference between the inner and outer rings, and less guaranteed product performance; secondly, the graphite outer ring and core need to be made larger, increasing costs. However, by sintering the drill teeth, inner and outer sprue gauge blocks separately, these components remain essentially unchanged, resulting in more stable performance and lower costs. Attached Figure Description
[0028] Figure 1 This is a three-dimensional structural diagram of one embodiment of the geological drill bit described in this invention.
[0029] Figure 2 for Figure 1 The structural diagram of the steel body in the embodiment is shown in (a) and (b) is a top view of the steel body.
[0030] Figure 3 for Figure 1 A three-dimensional structural diagram of the drill teeth in the implementation method.
[0031] Figure 4 for Figure 1 A three-dimensional structural diagram of the inner water inlet diameter protection block in the implementation method.
[0032] Figure 5 for Figure 1 A three-dimensional structural diagram of the outer and inner water inlet gauge blocks in the implementation method.
[0033] The numbers on the map are:
[0034] 1. Steel body, 101 welding platform, 102 inner welding groove, 103 outer welding groove, 104 limiting structure, 2. Drill teeth, 201 welding layer, 202 transition layer, 203 working layer, 2031 inner working layer, 2032 first interlayer, 2033 intermediate working layer, 2034 second interlayer, 2035 outer working layer, 3. Inner water inlet retaining block, 301 inner water tank, 4. Outer water inlet retaining block, 401 outer water tank. Detailed Implementation
[0035] To better explain the technical solution of the present invention, the present invention will be described in further detail below with reference to the accompanying drawings, but the embodiments of the present invention are not limited thereto.
[0036] like Figure 1 , Figure 2 , Figure 4 and Figure 5 As shown, the geological drill bit with gauge protection structure of the present invention includes drill teeth 2, a steel body 1, an inner gauge protection block 3, and an outer gauge protection block 4. The steel body 1 has a cylindrical hollow structure, and one end is provided with a connecting thread for assembling the geological drill bit. Multiple welding platforms 101 are provided circumferentially on the end face of the other end of the steel body 1. These welding platforms 101 are integrally formed with the steel body 1 and are evenly distributed on the end face of the steel body 1. The drill teeth 2 have a three-layer structure from top to bottom: a working layer 203, a transition layer 202, and a welding layer 201. The powder used in the working layer 203 and the transition layer 202 contains abrasive particles, while the powder used in the welding layer 201 does not contain abrasive particles. The drill teeth 2 are welded to the welding platforms 101 to ensure they are evenly distributed on the steel body 1. The end face of the steel body 1 between adjacent drill teeth 2 is also provided with an inner welding groove 102 and an outer welding groove 103 for welding the inner gauge protection block 3 and the outer gauge protection block 4. 03. A welding limiting structure 104 exists between the inner welding groove 102 and the outer welding groove 103. The welding limiting structure 104 is integrally formed with the steel body 1, and the top end face of the welding limiting structure 104 is higher than the welding platform 101. The inner sprue retaining block 3 is provided with an inner water groove 301, and the outer sprue retaining block 4 is provided with an outer water groove 401. Both the inner sprue retaining block 3 and the outer sprue retaining block 4 are sintered from powder containing abrasive particles. After the welding of the inner sprue retaining block 3 and the outer sprue retaining block 4 is completed, the inner sprue retaining block 3, the welding limiting structure 104 and the outer sprue retaining block 4 between two adjacent drill teeth 2 together form a sprue block. The plane where the top end face of the sprue block is located is higher than the plane where the top of the welding layer 201 on the drill tooth 2 is located. Based on the fact that the plane where the top end face of the sprue block is located is higher than the plane where the top of the welding layer 201 on the drill tooth 2 is located, the drill tooth 2 forms an inlay structure, so that the drill tooth 2 can withstand greater torque when working.
[0037] Based on the above, the structure of drill tooth 2 can be further optimized, such as... Figure 2As shown, a boss extending from the transition layer 202 to the working layer 203 can be provided between the transition layer 202 and the working layer 203 to act as a reinforcing rib, thereby improving the bonding force between the transition layer 202 and the working layer 203 of the drill bit 2. Furthermore, by providing a boss extending from the welding layer 201 to the transition layer 202 between the welding layer 201 and the transition layer 202, the bonding force between the welding layer 201 and the transition layer 202 can be improved. Preferably, the working layer 203 of the drill bit 2 can also be designed to have, in the radial direction, a working inner layer 2031 containing abrasive particles, a first interlayer 2032 without abrasive particles, a working middle layer 2033 containing abrasive particles, a second interlayer 2034 without abrasive particles, and a working outer layer 2035 containing abrasive particles, thereby improving the drilling efficiency and service life of the drill bit.
[0038] In this invention, the welding limiting structure 104 is similar to a partition structure, which restricts the possible movement of the inner sprue gauge block 3 and the outer sprue gauge block 4 in the radial direction of the drill bit, thereby improving the stress strength and welding positioning. The dimensions of the inner sprue gauge block 3 and the inner welding groove 102 must be perfectly matched, and the dimensions of the outer sprue gauge block 4 and the outer welding groove 103 must also be perfectly matched. This way, after the welding of the inner sprue gauge block 3 and the outer sprue gauge block 4 is completed, the outer surface of the outer sprue gauge block 4 can be kept flush with the outer peripheral surface of the steel body 1, and the inner surface of the inner sprue gauge block 3 can be kept flush with the inner peripheral surface of the steel body 1. Moreover, the tops of the inner sprue gauge block 3, the outer sprue gauge block 4, and the welding limiting structure 104 should be flush. At this time, the top end face of the welding limiting structure 104 is the top end face of the sprue block. Preferably, the height of the top end face of the welding limiting structure 104 beyond the welding platform 101 is greater than the height of the welding layer 201 of the drill tooth 2.
[0039] The abrasive grains involved in this invention can be diamond, polycrystalline, or a mixture of diamond and polycrystalline.
[0040] In this invention, the depth of the inner welding groove 102 and the outer welding groove 103 can be selected according to the drilling object and the specifications of the drill pipe, and is usually 6 to 10 mm; the depth of the inner water groove 301 and the outer water groove 401 can be selected according to the drilling object, and is usually 1 to 5 mm, so as to effectively circulate coolant and prevent drill burn.
[0041] According to the drilling life requirements, the higher the life requirement, the higher the total height of the drill tooth 2 should be. In a specific embodiment, when the total height of the drill tooth 2 is selected to be 10-30mm, it is preferable that the height of the weld layer 201 of the drill tooth 2 is 2-3mm, the height of the transition layer 202 is 2-3mm, and the remainder is the height of the working layer 203 (6-24mm); correspondingly, the matching height of the nozzle block is 6-10mm.
[0042] The method for preparing the geological drill bit with gauge protection structure according to the present invention includes the following steps:
[0043] 1) Take steel for making steel body 1, process connecting threads at one end of the steel, and process multiple welding platforms 101 circumferentially on the end face of the other end of steel body 1. The welding platforms 101 are evenly distributed on the end face of steel body 1. Then, process inner welding grooves 102 and outer welding grooves 103 for welding inner sprue gauge block 3 and outer sprue gauge block 4 on the end face of steel body 1 between two adjacent welding platforms 101. There is a welding limiting structure 104 between the inner welding groove 102 and the outer welding groove 103. The top end face of the welding limiting structure 104 is higher than the welding platform 101, thus obtaining steel body 1.
[0044] 2) A cold-pressed blank for drill teeth, consisting of a working layer 203, a transition layer 202, and a welding layer 201 arranged sequentially from top to bottom in the axial direction, is produced by cold pressing. The resulting cold-pressed blank is then sintered in batches at 830–860°C to obtain drill teeth 2.
[0045] 3) Cold pressing process is used to make cold pressing blanks of inner nozzle gauge block and outer nozzle gauge block respectively. The cold pressing blanks are sintered in batches at 830-860℃ to obtain inner nozzle gauge block 3 and outer nozzle gauge block 4.
[0046] 4) Weld the drill bit 2, the inner water inlet gauge block 3 and the outer water inlet gauge block 4 to the welding platform 101, the inner welding groove 102 and the outer welding groove 103 of the steel body 1 respectively, and the geological drill bit with gauge protection structure is obtained.
[0047] In this invention, for the steel used to make steel body 1, common steels of 20# to 45# can be selected. Because of the diameter protection measures, it is not necessary to select geological-specific steels such as DZ40 or DZ50. The steel is selected according to... Figure 2 The structure shown is machined to include connecting threads, a welding platform 101, an inner welding groove 102, and an outer welding groove 103. A complete steel body 1 can be directly machined, eliminating the need for further processing, unlike the integral sintering process which requires two machining operations on the steel body 1.
[0048] In this invention, the drill teeth 2 are manufactured by cold pressing followed by batch sintering. The following describes the process... Figure 3 The following explanation uses drill tooth 2 as an example:
[0049] ① Cold pressing is performed in two steps: First, the inner working layer 2031 containing abrasive particles, the middle working layer 2033 containing abrasive particles, the outer working layer 2035 containing abrasive particles, the first interlayer 2032 without abrasive particles, and the second interlayer 2034 without abrasive particles are individually cold pressed until the density is 50% to 60%; Second, the blanks obtained by the above cold pressing are combined according to... Figure 3The structure shown is placed in a mold, and then the powder of the transition layer 202 and the powder of the welding layer 201 are added and cold-pressed until the density is 60-67%, resulting in the following product. Figure 3 The drill tooth cold-pressed blank with the structure shown.
[0050] The powder composition of the working layer 203 can be designed according to the drilling strata. Preferably, the powder composition of the inner working layer 2031, the intermediate working layer 2033, and the outer working layer 2035 is a mixture of W, Co, Ni, Cu, Mn, Sn powder and abrasive particles, with an abrasive particle concentration preferably of 40-60%. Preferably, the powder composition of the first interlayer 2032 and the second interlayer 2034 is a mixture of Fe and CuSn powder. The transition layer 202 is required to have a high connection strength with the welding layer 201 and the working layer 203. Preferably, the powder of the transition layer 202 consists of 50% powder of the working layer 203 and 50% powder of the welding layer 201, with an abrasive particle concentration of 50-70% of that of the working layer 203. The powder composition of the welding layer 201 can be designed according to the requirements of ordinary carbon steel for laser drilling. Generally, pre-alloyed powder is used to ensure sintering density and strength. In this application, pre-alloyed powder of Fe, Co, and Cu is preferred.
[0051] ② Sintering: The cold-pressed blank is placed into a graphite mold and then sintered in an internal resistance vacuum hot press. The sintering temperature is 830-860℃, the pressure is 25-30MPa, and the holding time is 3-5min. The final sintered product has a density of 97-100%. Depending on the size of the drill teeth 2, 12-30 drill teeth 2 can usually be sintered at one time, which can make 2-5 drill bits. The efficiency is higher than that of sintering a single drill bit as a whole.
[0052] In this invention, only a single layer of powder is needed for both the inner nozzle gauge block 3 and the outer nozzle gauge block 4. The powder composition is preferably a mixture of Fe, Cu, W, Sn powder and abrasive particles, with an abrasive particle concentration of 40-60%. Both the inner nozzle gauge block 3 and the outer nozzle gauge block 4 are manufactured using a cold-pressing and then batch sintering method. Specifically, the appropriate cold-pressing mold is selected according to the drill bit's design dimensions for cold pressing, followed by sintering at 830-860℃ and 25-30MPa for 3-5 minutes. A multi-layer assembly method can be used during sintering, allowing for the sintering of 24-60 blocks at a time.
[0053] In this invention, the drill bit 2 is preferably welded to the welding platform 101 by laser welding, and the inner sprue gauge block 3 and the outer sprue gauge block 4 are preferably welded to the inner welding groove 102 and the outer welding groove 103 by flame brazing or high-frequency brazing, respectively. Before welding, the steel body 1 needs to undergo conventional treatments such as degreasing and rust removal.
[0054] Use of the drill bit described in this invention:
[0055] Will as Figure 1 The drill bit shown is mounted on the drill rod of a geological drilling rig. The rig drives the drill rod to rotate at high speed and drill downwards, while drilling fluid is introduced into the borehole simultaneously. The drill teeth 2, working layer 203, achieves rock-carving drilling. Due to the five-layer structure design of the working layer 203 in the radial direction of the drill bit, the inner working layer 2031 containing abrasive particles, the middle working layer 2033, and the outer working layer 2035 are always higher than the interlayer, forming a triangular tooth structure throughout the operation. The drill teeth 2 can carve into the rock under relatively low pressure, ensuring high-efficiency drilling. The entire drill bit, supported by welding and the welding platform 101, has high fracture resistance. The height of the entire drill teeth 2 can be as low as 30mm, ensuring both high-efficiency drilling and a long service life.
[0056] The specifications of the drill bit described in this invention can be designed according to conventional geological drill bit specifications. The drill teeth 2, steel body 1, inner sprue gauge block 3, and outer sprue gauge block 4 are all designed according to conventional geological specifications, such as Φ36.5mm / Φ21.5mm, Φ75mm / Φ47mm, Φ96mm / Φ63.5mm, etc. A smaller drill bit diameter allows for the welding of more drill teeth 2 produced in a single sintering process, resulting in higher production efficiency; a larger drill bit diameter saves more graphite mold material.
Claims
1. A geological drill bit with a gauge protection structure, comprising drill teeth (2) and a steel body (1), wherein the drill teeth (2) have a three-layer structure in the axial direction consisting of a working layer (203), a transition layer (202), and a welded layer (201), one end of the steel body (1) is provided with a connecting thread, and the drill teeth (2) are evenly distributed at the other end of the steel body (1), characterized in that, It also includes an inner water inlet retaining block (3) and an outer water inlet retaining block (4). The inner water inlet retaining block (3) is provided with an inner water groove (301), and the outer water inlet retaining block (4) is provided with an outer water groove (401). Both the inner water inlet retaining block (3) and the outer water inlet retaining block (4) are sintered from powder containing abrasive particles. Multiple welding platforms (101) are machined circumferentially on the end face of the other end of the steel body (1), and the drill teeth (2) are welded to the welding platforms (101); the end face of the steel body (1) between two adjacent drill teeth (2) is also machined with inner welding grooves (102) and outer welding grooves (103) for welding the inner sprue gauge block (3) and the outer sprue gauge block (4), and there is a welding limiting structure (104) between the inner welding groove (102) and the outer welding groove (103). The top end face of the welding limiting structure (104) is higher than the welding platform (101). The inner sprue gauge block (3), the welding limiting structure (104) and the outer sprue gauge block (4) between two adjacent drill teeth (2) together constitute a sprue block; After the welding of the inner sprue retaining block (3), the outer sprue retaining block (4) and the drill tooth (2) is completed, in the axial direction of the drill bit, the plane where the top end face of the sprue block is located is higher than the plane where the top of the welded layer (201) on the drill tooth (2) is located.
2. The geological drill bit with gauge protection structure according to claim 1, characterized in that, A boss extending from the weld layer (201) to the transition layer (202) is provided between the weld layer (201) and the transition layer (202) of the drill tooth (2).
3. The geological drill bit with gauge protection structure according to claim 1, characterized in that, A boss extending from the transition layer (202) to the working layer (203) is provided between the transition layer (202) and the working layer (203) of the drill tooth (2).
4. The geological drill bit with gauge protection structure according to any one of claims 1 to 3, characterized in that, The height of the top end face of the welding limiting structure (104) extending beyond the welding platform (101) is greater than the height of the welding layer (201) of the drill tooth (2).
5. The geological drill bit with gauge protection structure according to any one of claims 1 to 3, characterized in that, The working layer (203) of the drill tooth (2) has a structure in the radial direction consisting of an inner working layer (2031) containing abrasive particles, a first interlayer (2032) without abrasive particles, an intermediate working layer (2033) containing abrasive particles, a second interlayer (2034) without abrasive particles, and an outer working layer (2035) containing abrasive particles, arranged from the inside to the outside.
6. The geological drill bit with gauge protection structure according to any one of claims 1 to 3, characterized in that, When the total height of the drill bit (2) is 10-30 mm, the height of the welding layer (201) is 2-3 mm, the height of the transition layer (202) is 2-3 mm, and the remainder is the height of the working layer (203); the matching height of the nozzle block is 6-10 mm.
7. The method for preparing the geological drill bit with gauge protection structure as described in claim 1, comprising the following steps: 1) Take steel for making steel body (1), process connecting threads at one end of the steel, and process multiple welding platforms (101) along the circumferential direction on the end face of the other end of the steel body (1). The welding platforms (101) are evenly distributed on the end face of the steel body (1). Then, process inner welding grooves (102) and outer welding grooves (103) for welding inner sprue gauge block (3) and outer sprue gauge block (4) on the end face of the steel body (1) between two adjacent welding platforms (101). There is a welding limiting structure (104) between the inner welding groove (102) and the outer welding groove (103). The top end face of the welding limiting structure (104) is higher than the welding platform (101) to obtain steel body (1). 2) The cold-pressed blank of the drill tooth has a three-layer structure of working layer (203), transition layer (202) and welding layer (201) in the axial direction by cold pressing forming process. The cold-pressed blank is sintered in batches at 830-860℃ to obtain the drill tooth (2). 3) The inner nozzle gauge block cold-pressed blank and the outer nozzle gauge block cold-pressed blank were respectively made by cold pressing forming process. The cold-pressed blanks were sintered in batches at 830~860℃ to obtain the inner nozzle gauge block (3) and the outer nozzle gauge block (4). 4) Weld the drill bit (2), the inner water inlet gauge block (3) and the outer water inlet gauge block (4) onto the welding platform (101), the inner welding groove (102) and the outer welding groove (103) of the steel body (1) respectively, and the geological drill bit with gauge protection structure is obtained.
Citation Information
Patent Citations
Diamond bit with multilayer combined type drilling teeth
CN103334701A
Welded high-matrix diamond core bit and manufacturing method thereof
CN103953286A