A lead-acid battery grid corrosive agent formula and preparation method thereof

By using a specific formula of grid corrosive in lead-acid batteries, a uniform thickness of basic lead carbonate is formed, which solves the problem of insufficient grid corrosion layer thickness, improves plate conductivity and battery consistency, and simplifies the process. Ensures the stability of battery performance.

CN117737735BActive Publication Date: 2024-10-25JIANGSU LEOCH BATTERY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311701698.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-12
Publication Date
2024-10-25
Estimated Expiration
2043-12-12

AI Technical Summary

Technical Problem

The grid corrosion layer in existing lead-acid batteries has uneven thickness and insufficient depth, resulting in insufficient strength of the corrosion layer and affecting plate performance and battery consistency.

Method used

A lead-acid battery grid corrosive formula is used, including pure water, sodium silicate, glacial acetic acid, hydrogen peroxide, baking soda and ammonium carbonate. Basic lead carbonate is formed on the grid surface through specific proportions and stirring steps to promote uniformity. A thick lead sulfate corrosion layer is formed.

Benefits of technology

The uniform thickness and high conversion efficiency of the grid corrosion layer are achieved, the plate conductivity and battery consistency are improved, the process is simplified, and the raw materials will not have a negative impact on battery performance in subsequent manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117737735B_ABST
    Figure CN117737735B_ABST
Patent Text Reader

Abstract

The present invention proposes a lead-acid battery grid corrosive agent formula and a preparation method thereof, which comprises pure water, sodium silicate, glacial acetic acid, hydrogen peroxide, baking soda, and ammonium carbonate, and can accelerate the corrosion of the grid surface to form basic lead carbonate. When the grid paste is cured, the basic lead carbonate easily reacts with sulfuric acid in the lead paste to form lead sulfate crystals, which promotes the formation of a grid corrosion layer. The formula is applied to the grid surface before the paste is applied, and is sealed and static at room temperature without light to accelerate the corrosion of the surface lead (lead alloy), and finally form basic lead carbonate on the grid surface. The corrosive agent can promote the formation of basic lead carbonate on the grid surface, and the crystal layer has a uniform thickness, grows on the grid surface, and is closely attached to the grid lead (lead alloy). The corrosion layer thus generated has good contact with the grid alloy, uniform thickness, and no obvious stratification. The plate is not easy to deform or creep when in use, the current density is evenly distributed during charging and discharging, the lead paste is well combined with the grid, and the battery life is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lead-acid battery manufacturing, and in particular relates to a lead-acid battery grid corrosive agent formula and a preparation method thereof. Background Art

[0002] In the manufacture of lead-acid batteries, a corrosion layer will form on the surface of the grid lead (lead alloy). The corrosion layer is between the grid and the lead paste. Therefore, the battery charge and discharge current will pass through the corrosion layer. The performance of the corrosion layer has a great impact on the performance of the plate and the battery. A good corrosion layer should be in full contact with the grid and the lead paste, fit each other without obvious stratification, have uniform thickness and no faults, and the lead paste and the grid should fit firmly and not loosen easily. The composition of the corrosion layer is mainly composed of PbOn and lead sulfate of different crystal forms. The formation principle is that the lead on the surface of the lead (lead alloy) forms basic lead carbonate with water and carbon dioxide, which is converted into lead sulfate during the curing stage, and a corrosion layer is formed when the plate is formed. This formula provides a cheap and effective method to quickly form basic lead carbonate on the surface of the grid, which is conducive to the formation of the grid corrosion layer in the subsequent process. Before applying the grid paste, apply the formula solution on the surface of the grid and let it stand for a period of time, and basic lead carbonate will form on the surface of the grid. No additional process is added, the operation is simple, and the effect is good. Summary of the invention

[0003] To achieve the above-mentioned purpose, the technical scheme of the present invention is as follows: a lead-acid battery grid corrosive agent formula, the corrosive agent formula includes the following parts by weight: 85-100 parts of pure water, 2-4 parts of sodium silicate, 0.5-1.5 parts of glacial acetic acid, 3-10 parts of hydrogen peroxide, 1-3 parts of baking soda, and 3-5 parts of ammonium carbonate.

[0004] As an improvement of the present invention, 90 parts of pure water, 4 parts of sodium silicate, 1 part of glacial acetic acid, 10 parts of hydrogen peroxide, 1 part of baking soda, and 3 parts of ammonium carbonate.

[0005] As an improvement of the present invention, the conductivity of the pure water used is configured to be ≤10µs / cm.

[0006] As an improvement of the present invention, the content of hydrogen peroxide in the etchant is 2% to 5%.

[0007] As an improvement of the present invention, the content of sodium silicate in the etchant is 3% to 5%.

[0008] As an improvement of the present invention, the content of glacial acetic acid in the etchant does not exceed 1.5%.

[0009] In the present invention, no corrosive agent is used. The grid corrosion layer is formed by the lead on the grid surface and the oxygen in the air to form lead oxide, which is then converted into lead sulfate. The thickness of this corrosion layer is uneven and the depth is insufficient, resulting in insufficient strength of the corrosion layer. The basic lead carbonate formed by the use of the corrosive agent is formed by liquid corrosion of the grid, and the thickness is deep and uniform. When it is converted into lead sulfate, the efficiency is high and the reaction is sufficient, which is beneficial to the final PbO n Formation, due to the high conversion efficiency of the corrosion layer and the relatively large n value, the produced plate has high conductivity, uniform discharge and good battery consistency.

[0010] As an improvement of the present invention, a method for preparing a lead-acid battery grid corrosive agent formula is provided, characterized in that the preparation method comprises the following steps:

[0011] Step 1: Prepare the additive: slowly add hydrogen peroxide into pure water in a dark and dark place at room temperature, stirring while adding. After the hydrogen peroxide is added, continue stirring and add glacial acetic acid, and after the addition is complete, obtain the additive, seal it and let it stand for use;

[0012] Step 2: Prepare the main solution: stir pure water and add sodium silicate, baking soda and ammonium carbonate and stir until all additives are dissolved to obtain the main solution;

[0013] Step 3: Prepare the corrosive agent: add the additive in step 1 to the main liquid in step 2 and stir to obtain the corrosive agent.

[0014] As an improvement of the present invention, in a cool and lightless environment at room temperature, 10 parts of pure water, 10 parts of 30% concentration hydrogen peroxide and 1 part of glacial acetic acid are mixed and stirred at a speed of 150-200 r / min for 5 minutes to obtain an additive.

[0015] As an improvement of the present invention, 80 parts of pure water are stirred at room temperature, 4 parts of sodium silicate, 1 part of baking soda and 3 parts of ammonium carbonate are added, and the mixture is stirred at a speed of 200-300 r / min for 10 minutes to obtain a main liquid.

[0016] As an improvement of the present invention, the main liquid is stirred, and after the additive is added, the etching agent is obtained after stirring at a speed of 200-300 r / min for 5 minutes.

[0017] Compared with the prior art, the beneficial effects of the present invention are as follows: the lead-acid battery grid corrosive agent configured by the present invention is quick to configure, the raw materials are easy to obtain, and after being applied on the grid surface, basic lead carbonate can be quickly formed, which is beneficial to the subsequent formation of the grid corrosion layer. At the same time, all additives and products in this formula will volatilize, decompose or have no negative impact on battery performance during subsequent battery manufacturing. Hydrogen peroxide will decompose into water and oxygen at the subsequent high temperature of curing, glacial acetic acid is easy to volatilize, sodium bicarbonate and sodium carbonate will form sodium sulfate with sulfuric acid during the paste coating process, and sodium sulfate and sodium silicate have no effect on battery performance. The remaining carbonate reacts with sulfuric acid to form CO2 and escapes, and there will be no residue. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Attached Figure 1 This is the process of grid corrosion layer formation. DETAILED DESCRIPTION

[0019] The present invention will be further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0020] Example: Figure 1 As shown, a lead-acid battery grid corrosive agent formula includes the following parts by weight: 90 parts of pure water, 4 parts of sodium silicate, 1 part of glacial acetic acid, 10 parts of hydrogen peroxide, 1 part of baking soda, and 3 parts of ammonium carbonate.

[0021] As an improvement of this embodiment, the conductivity of the pure water used is configured to be ≤10µs / cm.

[0022] As an improvement of this embodiment, the content of hydrogen peroxide in the etchant is 2% to 5%.

[0023] As an improvement of this embodiment, the content of sodium silicate in the etchant is 3% to 5%.

[0024] As an improvement of this embodiment, the content of glacial acetic acid in the etchant does not exceed 1.5%.

[0025] As an improvement of this embodiment, a method for preparing a lead-acid battery grid corrosive agent formulation comprises the following steps:

[0026] Step 1: Prepare the additive: slowly add hydrogen peroxide into pure water in a dark and dark place at room temperature, stirring while adding. After the hydrogen peroxide is added, continue stirring and add glacial acetic acid, and after the addition is complete, obtain the additive, seal it and let it stand for use;

[0027] Step 2: Prepare the main solution: stir pure water and add sodium silicate, baking soda and ammonium carbonate and stir until all additives are dissolved to obtain the main solution;

[0028] Step 3: Prepare the corrosive agent: add the additive in step 1 to the main liquid in step 2 and stir to obtain the corrosive agent.

[0029] As an improvement of the present embodiment, in a cool and lightless environment at room temperature, 10 parts of pure water, 10 parts of 30% hydrogen peroxide and 1 part of glacial acetic acid are mixed and stirred at a speed of 150-200 r / min for 5 minutes to obtain an additive.

[0030] As an improvement of the present embodiment, 80 parts of pure water are stirred at room temperature, 4 parts of sodium silicate, 1 part of baking soda and 3 parts of ammonium carbonate are added, and the mixture is stirred at a speed of 200-300 r / min for 10 minutes to obtain the main liquid.

[0031] As an improvement of this embodiment, the main liquid is stirred, and after the additive is added, the etching agent is obtained after stirring at a speed of 200-300 r / min for 5 minutes.

[0032] In this embodiment, no corrosive agent is used. The grid corrosion layer is formed by the lead oxide formed by the lead on the grid surface and the oxygen in the air, and then converted into lead sulfate. The thickness of this corrosion layer is uneven and the depth is insufficient, resulting in insufficient strength of the corrosion layer. The basic lead carbonate formed by the use of the corrosive agent is formed by liquid corrosion of the grid. The thickness is deep and uniform, and the conversion into lead sulfate is efficient and fully reacted, which is beneficial to the final PbO n Formation, due to the high conversion efficiency of the corrosion layer and the relatively large n value, the produced plate has high conductivity, uniform discharge and good battery consistency.

[0033] It should be noted that the above content only illustrates the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications all fall within the protection scope of the claims of the present invention.

Claims

1. A lead-acid battery grid corrosive agent formula, characterized in that: The corrosive agent formula includes the following parts by weight: 85-100 parts of pure water, 2-4 parts of sodium silicate, 0.5-1.5 parts of glacial acetic acid, 3-10 parts of hydrogen peroxide, 1-3 parts of baking soda, and 3-5 parts of ammonium carbonate.

2. A lead-acid battery grid corrosive agent formulation according to claim 1, characterized in that: 90 parts of pure water, 4 parts of sodium silicate, 1 part of glacial acetic acid, 10 parts of hydrogen peroxide, 1 part of baking soda, and 3 parts of ammonium carbonate.

3. A lead-acid battery grid corrosive agent formulation according to claim 1, characterized in that: The conductivity of pure water used for configuration is ≤10µs / cm.

4. A lead-acid battery grid corrosive agent formulation according to claim 1, characterized in that: The hydrogen peroxide content in the corrosive agent is between 2% and 5%.

5. A lead-acid battery grid corrosive agent formulation according to claim 1, characterized in that: The sodium silicate content in the corrosive agent is 3%~5%.

6. A lead-acid battery grid corrosive agent formulation according to claim 1, characterized in that: The content of glacial acetic acid in the corrosive agent shall not exceed 1.5%.

7. A method for preparing a lead-acid battery grid corrosive agent according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: Step 1: In a cool place without light at room temperature, take pure water, hydrogen peroxide and glacial acetic acid, mix and stir to obtain an additive and let it stand for use; Step 2: Add sodium silicate, baking soda and ammonium carbonate into pure water and stir to obtain a main solution; Step 3: Add the additive in step 1 to the main liquid in step 2 and stir to obtain a corrosive agent.

8. The method for preparing a lead-acid battery grid corrosive agent according to claim 7, characterized in that: In a cool and lightless environment at room temperature, 10 parts of pure water, 10 parts of 30% hydrogen peroxide and 1 part of glacial acetic acid were mixed and stirred at a speed of 150-200 r / min for 5 minutes to obtain an additive.

9. The method for preparing a lead-acid battery grid corrosive agent according to claim 7, characterized in that: Stir 80 parts of pure water at room temperature, add 4 parts of sodium silicate, 1 part of baking soda and 3 parts of ammonium carbonate, and stir at 200-300 r / min for 10 minutes to obtain the main liquid.

10. The method for preparing a lead-acid battery grid corrosive agent according to claim 7, characterized in that: The main liquid is stirred, and after adding the additive, the etching agent is obtained after stirring at a speed of 200-300 r / min for 5 minutes.