A water-based ink-style floral polyurethane material, its preparation method and application
By using a water-ink style floral pattern preparation method, a clear water-ink floral pattern can be formed by utilizing an independently moving baking chamber and a vacuum environment. This solves the problems of easy detachment of polyurethane materials and complex processes in existing technologies, and realizes a polyurethane material with simple preparation, high color fastness and excellent decorative effect.
Patent Information
- Application Number
- CN202311594076.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-27
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-27
AI Technical Summary
Existing technologies produce polyurethane materials with special textured patterns that are prone to peeling off, involve complex processes, and lack materials with a natural and ecological style, thus failing to meet the diverse and personalized needs of users.
The ink-wash style floral pattern is prepared by adding a mixture of polyurethane granules into an independently movable baking chamber, preheating and raising the temperature to form molten material in different color areas in the mold. After cooling, it is cut to form a natural ink-wash floral pattern. The combination of vacuum environment and appropriate temperature, movement speed and grid design ensures the clarity and stability of the pattern.
It is easy to prepare, does not easily peel off, has good color fastness, and has good decorative effect and mechanical properties, meeting the diverse needs of users.
Smart Images

Figure CN117754789B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polyurethane materials technology, specifically relating to a water-ink style floral polyurethane material, its preparation method, and its application. Background Technology
[0002] Polyurethane materials have advantages such as good adhesion, high and low temperature stability, high elasticity, wear resistance, high strength, and easy extensibility. They can be made into materials of different thicknesses, colors, and structures, and are widely used in various fields.
[0003] CN202227183U discloses a high-simulation artificial leather, comprising a leather base layer and animal fine fiber layers and animal skin pattern layers disposed on both sides of the leather base layer. The animal skin pattern layers are laminated to the leather base layer via a polyurethane film layer. This technical solution uses a polyurethane film to adhere the animal skin pattern layers, giving the artificial leather a visually realistic feel similar to genuine leather.
[0004] CN202192821U discloses a glossy printed coated fabric, which comprises, from bottom to top, a polyester calendered base fabric, a first polyurethane film, a second polyurethane film, a printed layer, and a third polyurethane film. The polyester calendered base fabric, the first polyurethane film, the second polyurethane film, the printed coating, and the third polyurethane film are sequentially layered and bonded together seamlessly. The glossy printed coated fabric provided by this technical solution exhibits significantly higher colorfastness than traditional transfer printing, pigment printing, and water-based printing fabrics. Furthermore, its print is brighter than hot stamping, and the printed fabric of this utility model retains its vibrant color even after multiple washes.
[0005] In existing technologies, materials with special textured patterns are typically prepared by printing or laminating pattern layers. However, patterns prepared using this method are prone to rubbing and peeling off, exhibiting poor pattern stability, and require multi-layer fabrication, making the process complex. Furthermore, existing technologies lack polyurethane materials with a natural, eco-friendly style. To meet the diverse and personalized needs of users, it is necessary to develop more types of polyurethane materials with special textured patterns.
[0006] Therefore, there is a need to develop a water-based polyurethane material for creating floral patterns that is simple to prepare, easy to process, does not easily peel off, and has good color fastness. Summary of the Invention
[0007] To address the shortcomings of existing technologies, the present invention aims to provide a water-ink style polyurethane material, its preparation method, and its applications. The water-ink style polyurethane material possesses natural water-ink style patterns and is simple to prepare, easy to process, resistant to peeling, has good colorfastness, and good mechanical properties.
[0008] To achieve this objective, the present invention adopts the following technical solution:
[0009] In a first aspect, the present invention provides a method for preparing a water-based ink-style floral polyurethane material, the method comprising the following steps:
[0010] (1) Add polyurethane granule mixture to each baking chamber of the ink-style floral color preparation device, preheat, raise the temperature, and simultaneously move the baking chamber along the X-axis and Y-axis and drip the material into the mold to obtain a block polyurethane prototype.
[0011] (2) Cool the block polyurethane prototype obtained in step (1) and cut it along the direction perpendicular to the dripping to obtain the water-ink style polyurethane material.
[0012] The polyurethane granule mixture is a granule mixture comprising polyurethane granules and polyurethane masterbatch, wherein the colors of the polyurethane granules and the polyurethane masterbatch are different.
[0013] The temperature increase refers to raising the temperature to 180-220℃ (e.g., 182℃, 185℃, 188℃, 190℃, 192℃, 195℃, 198℃, 200℃, 202℃, 205℃ or 208℃, etc.);
[0014] The ink-wash style floral pattern preparation device includes a mold and at least two independently movable baking chambers, with a perforated grid at the bottom of each baking chamber.
[0015] In this invention, a polyurethane granule mixture is added to at least two independently movable baking chambers and preheated to melt the mixture. The polyurethane granules and masterbatch have different colors, creating a molten mixture with different color regions. These molten regions flow together through a sprue and drip into a mold. Due to the movement of the baking chambers and the fluid flow, curved lines and regions with the color of the masterbatch, gradient lines and regions at the boundary between the polyurethane granules and the masterbatch molten mixture, and curved lines and regions with the color of the polyurethane granules are formed in the mold. After cooling and cutting, a watercolor-style floral polyurethane material is obtained. This watercolor-style floral polyurethane material has a natural watercolor pattern and excellent decorative effect. The watercolor-style floral polyurethane material is integrally formed by the polyurethane material and the watercolor pattern, and features simple preparation, convenient processing, resistance to peeling, good color fastness, and good mechanical properties. The temperature is raised to 180-220℃ because if the temperature is too low, the polyurethane granule mixture will have low fluidity and cannot flow smoothly out of the sprue; if the temperature is too high, the molten polyurethane granules and polyurethane masterbatch will have good fluidity, causing the polyurethane masterbatch to flow excessively, resulting in large areas of overlapping color between the polyurethane granules and the polyurethane masterbatch (overlapping color refers to the color formed after two colors are evenly mixed), resulting in unclear pattern lines, chaotic patterns, and poor ink-wash floral pattern effects. The baking chamber moves simultaneously along the X and Y axes. If it only moves along the X or Y axis, it cannot form curved lines with the color of the polyurethane masterbatch, and it is impossible to obtain a natural curved ink-wash floral pattern.
[0016] In this invention, the "ink-and-wash floral pattern" refers to the curved lines and areas with the color of polyurethane masterbatch, the gradient color lines and areas at the boundary of polyurethane particles and polyurethane masterbatch melt, and the curved lines and areas with the color of polyurethane particles. The lines are clearly colored curves with relatively uniform distribution of different colors. There are no large areas of overlapping color regions formed by the colors of polyurethane particles and polyurethane masterbatch. The colors of the polyurethane particles and polyurethane masterbatch are not the same. The colors of the polyurethane particles are not limited to white, and the colors of the polyurethane masterbatch are not limited to black.
[0017] It should be noted that the shape and size of the baking cavity are not specifically limited in this invention, and those skilled in the art can make adjustments according to the actual situation.
[0018] Preferably, the ink-wash style floral pattern preparation device includes 4-6 (e.g. 5) independently movable baking chambers.
[0019] In this invention, the number of independently moving baking chambers is 4-6, which can realize the distribution of multiple areas in a variety of ink-wash pattern. If the number is too large, it will increase machine wear and tear, increase process costs, and increase the difficulty of equipment management.
[0020] Preferably, the mold is provided with an X-axis slide rail, a Y-axis slide rail, an X-axis slider, and a Y-axis slider. The X-axis slider is provided with a groove that slides into the X-axis slide rail. The Y-axis slider is provided with a groove that slides into the Y-axis slide rail. The baking chamber is connected to the Y-axis slide rail via a slider, and the Y-axis slide rail is connected to the X-axis slide rail via the X-axis slider.
[0021] In this invention, the baking chamber simultaneously achieves X-axis and Y-axis movement via a movable slide rail. A motion control device is connected to the movable slide rail and the slider, which can preset the motion parameters of the X-axis and Y-axis. The baking chamber has heating and temperature control functions. A temperature control device is connected to the baking chamber, which can preset the temperature parameters of the baking chamber. The motion control device and the temperature control device can preset the X-axis movement speed, Y-axis movement speed, preheating temperature, and heating temperature of the baking chamber.
[0022] Preferably, the mold includes a cuboid groove.
[0023] Preferably, the X-axis movement speed and Y-axis movement speed of the baking chamber are each independently 0.5-3 m / min, such as 0.6 m / min, 0.8 m / min, 1.2 m / min, 1.4 m / min, 1.6 m / min, 1.8 m / min, 2.0 m / min, 2.2 m / min, 2.4 m / min, 2.6 m / min or 2.8 m / min, etc.
[0024] In this invention, the movement speed of the baking chamber along the X-axis and along the Y-axis are each independently 0.5-3 m / min. Each baking chamber moves back and forth within its X-axis movement distance, and similarly, each baking chamber moves back and forth within its Y-axis movement distance, until the strong dripping of material from the baking chamber ends. The movement distances along the X and Y axes can be set according to the pattern and size of the ink-wash pattern polyurethane material to be prepared. If the movement speed is too high, it is easy for material from the baking chamber to drip into the area of the adjacent baking chamber, and the patterns in different baking chamber areas will affect each other, easily resulting in overlapping color areas and a decrease in the ink-wash pattern effect. If the movement speed is too low, it is easy for the polyurethane granule mixture to flow insufficiently, resulting in a decrease in the ink-wash pattern effect.
[0025] Preferably, the mesh count of the grating is 120-200 mesh, such as 125 mesh, 130 mesh, 135 mesh, 140 mesh, 145 mesh, 150 mesh, 155 mesh, 160 mesh, 165 mesh, 170 mesh, 175 mesh, 180 mesh, 185 mesh, 190 mesh, or 195 mesh.
[0026] In this invention, the mesh size of the stencil is 120-200 mesh. If the mesh size of the stencil is too large, it is easy for the insufficiently melted polyurethane granule mixture to drip down, causing crystal points, insufficient flow and other defects. If the mesh size of the stencil is too small, it is easy for the material to get stuck, the material to drip in time, the melt flow of the polyurethane masterbatch to be uneven, and the effect of the ink and wash pattern to decrease.
[0027] Preferably, the particulate mixture further includes a hydrolysis-resistant agent and an UV-resistant additive.
[0028] Preferably, the polyurethane granule mixture added to each baking chamber in step (1) independently comprises 20-40 parts by weight (e.g., 22 parts by weight, 24 parts by weight, 26 parts by weight, 28 parts by weight, 30 parts by weight, 32 parts by weight, 34 parts by weight, 36 parts by weight, or 38 parts by weight, etc.) of polyurethane granules and 1-10 parts by weight (e.g., 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, or 9 parts by weight, etc.) of polyurethane colorant. A granular mixture of masterbatch, 1-3 parts by weight (e.g., 1.2 parts by weight, 1.4 parts by weight, 1.6 parts by weight, 1.8 parts by weight, 2 parts by weight, 2.2 parts by weight, 2.4 parts by weight, 2.6 parts by weight, or 2.8 parts by weight) of hydrolysis resistant agent, and 0.1-3 parts by weight (e.g., 0.3 parts by weight, 0.6 parts by weight, 0.9 parts by weight, 1.2 parts by weight, 1.5 parts by weight, 1.8 parts by weight, 2.1 parts by weight, 2.4 parts by weight, or 2.7 parts by weight, etc.) of UV-resistant additive.
[0029] In this invention, the polyurethane granule mixture added to each baking chamber can be adjusted by those skilled in the art according to actual conditions and needs to prepare the ink-wash floral pattern. The weight percentage of the polyurethane masterbatch is preferably 1-10 parts. If the weight percentage of the polyurethane masterbatch is too low, there will be fewer lines or areas of color, uneven distribution of different colors, insufficient color vibrancy, and a decrease in the effect of the ink-wash floral pattern. If the weight percentage of the polyurethane masterbatch is too high, the colors of the polyurethane masterbatch will be too concentrated, uneven distribution of different colors, poor effect of gradient lines or areas, and a decrease in the effect of the ink-wash floral pattern.
[0030] Preferably, the preparation method of the particulate mixture includes the following steps: adding polyurethane particles, polyurethane masterbatch, hydrolysis resistant agent and UV resistant additive into a mixer and mixing at 20-80℃ (e.g. 25℃, 30℃, 35℃, 40℃, 45℃, 50℃, 55℃, 60℃, 65℃, 70℃ or 75℃, etc.) to obtain the particulate mixture.
[0031] In this invention, the raw materials for preparing the particulate mixture are mixed at 20-80°C, which ensures that the polyurethane particles and polyurethane masterbatches in the mixed particulate mixture do not soften or melt, and exist in a complete granular form.
[0032] Preferably, the preheating temperature in step (1) is 100-130℃, such as 103℃, 106℃, 109℃, 112℃, 115℃, 118℃, 121℃, 124℃ or 127℃.
[0033] In this invention, if the preheating temperature is too low, the polyurethane granule mixture will not soften sufficiently and will not drip smoothly after heating; if the preheating temperature is too high, the polyurethane granule mixture will melt before heating, easily forming large areas of overlapping colors, resulting in poor gradient color lines or area effects and poor ink-wash floral patterns.
[0034] Preferably, the preheating time in step (1) is 15-20 min, such as 15.5 min, 16 min, 16.5 min, 17 min, 17.5 min, 18 min, 18.5 min, 19 min or 19.5 min.
[0035] In this invention, if the preheating time is too short, the polyurethane granule mixture will not soften sufficiently and will not drip smoothly; if the preheating time is too long, the polyurethane granule mixture will melt before heating, easily forming large areas of overlapping colors, resulting in poor gradient color lines or areas and poor ink-wash floral patterns.
[0036] Preferably, the dripping rate of each material in the baking chamber in step (1) is independently 25-45 g / min, such as 27 g / min, 29 g / min, 31 g / min, 33 g / min, 35 g / min, 37 g / min, 39 g / min, 41 g / min or 43 g / min, etc.
[0037] Preferably, the steps of preheating, heating, and simultaneously moving the baking chamber along the X and Y axes and dripping material into the mold in step (1) are performed in a vacuum environment.
[0038] In this invention, the steps of preheating, heating, and simultaneously moving the baking chamber along the X and Y axes and dripping the material into the mold are carried out in a vacuum environment because bubbles are easily formed in the block polyurethane prototype during the preparation process of the ink-like polyurethane material. Carrying it out in a vacuum environment can reduce the generation of bubbles and reduce the number of bubbles in the resulting ink-like polyurethane material.
[0039] Preferably, the process of preparing the ink-style floral pattern in a vacuum environment specifically includes, after adding the polyurethane granule mixture in step (1), placing the ink-style floral pattern preparation device into a vacuum bag, opening the vacuum valve, and creating a vacuum environment.
[0040] Preferably, the cooling in step (2) includes water cooling.
[0041] In a second aspect, the present invention provides a water-ink style polyurethane material with floral patterns, wherein the water-ink style polyurethane material is prepared by the preparation method described in the first aspect.
[0042] Thirdly, the present invention provides an application of the ink-wash pattern polyurethane material as described in the second aspect in shoe materials or electronic product component materials.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] The preparation method provided by this invention involves adding a polyurethane granule mixture into at least two independently movable baking chambers, preheating and raising the temperature to melt the polyurethane granule mixture, forming a melt with different color areas. The melt flows out along the sprue and drips into a mold, and after cooling and cutting, a watercolor-style floral polyurethane material is obtained. The watercolor-style floral polyurethane material has a natural watercolor pattern, is simple to prepare, easy to process, not easy to peel off, has good color fastness, excellent decorative effect, and good mechanical properties. Attached Figure Description
[0045] Figure 1 This is a schematic diagram of the ink-wash style floral decoration preparation device described in Example 1;
[0046] Wherein, 1-mold; 2-slot; 3-Y-axis slide rail; 4-X-axis slide rail; 5-Y-axis slider; 6-X-axis slider; 7-first baking cavity; 8-second baking cavity; 9-third baking cavity; 10-fourth baking cavity; 11-fifth baking cavity; 12-sixth baking cavity;
[0047] Figure 2 This is a schematic diagram of the structure of the ink-wash style floral decoration preparation device described in Example 2;
[0048] Wherein, 1-mold; 2-slot; 3-Y-axis slide rail; 4-X-axis slide rail; 5-Y-axis slider; 6-X-axis slider; 7-first baking cavity; 8-second baking cavity; 9-third baking cavity; 10-fourth baking cavity;
[0049] Figure 3 The ink-wash pattern is provided in Example 1 for the polyurethane material with ink-wash pattern. Detailed Implementation
[0050] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0051] The sources of some components in the examples and comparative examples are as follows:
[0052] Polyurethane granules, manufacturer: Dongguan Jixin Polymer Technology Co., Ltd., brand: JX-450;
[0053] Polyurethane masterbatch: Black polyurethane masterbatch, manufacturer: Dongguan Jixin Polymer Technology Co., Ltd., brand: JX-S331;
[0054] Hydrolysis resistant agent: Polymeric carbodiimide hydrolysis resistant agent, Manufacturer: Shanghai Youen Chemical Co., Ltd., Grade: UN03;
[0055] UV-protecting adjuvants: bis(2,2,6,6-tetramethyl-4-hydroxypiperidine) sebacate and 2-(2′-hydroxy-5′-methylphenyl)benzotriazole in a mass ratio of 1:1.
[0056] Example 1
[0057] This embodiment provides a water-based ink-style floral polyurethane material and its preparation method. The preparation method of the water-based ink-style floral polyurethane material includes the following steps:
[0058] (1) Add a mixture of 8 parts by weight of polyurethane granules, 1.5 parts by weight of polyurethane masterbatch, 1.5 parts by weight of hydrolysis resistant agent and 1 part by weight of UV resistant additive into the first baking chamber 7.
[0059] A granular mixture of 5 parts by weight of polyurethane granules, 1 part by weight of polyurethane masterbatch, 1.5 parts by weight of hydrolysis resistant agent and 1 part by weight of UV resistant additive is added to the second baking chamber 8.
[0060] A granular mixture of 7 parts by weight of polyurethane granules, 1.5 parts by weight of polyurethane masterbatch, 1.5 parts by weight of hydrolysis resistant agent and 1 part by weight of UV resistant additive is added to the third baking chamber 9.
[0061] A granular mixture of 7 parts by weight of polyurethane granules, 2 parts by weight of polyurethane masterbatch, 1.5 parts by weight of hydrolysis resistant agent and 1 part by weight of UV resistant additive is added to the fourth baking chamber 10.
[0062] A granular mixture consisting of 8 parts by weight of polyurethane granules, 2 parts by weight of polyurethane masterbatch, 1.5 parts by weight of hydrolysis resistant agent and 1 part by weight of UV resistant additive is added to the fifth baking chamber 11.
[0063] A mixture of 8.5 parts by weight of polyurethane granules, 1.8 parts by weight of polyurethane masterbatch, 1.5 parts by weight of hydrolysis resistant agent and 1 part by weight of UV resistant additive is added to the sixth baking chamber 12.
[0064] Then, the ink-style floral color preparation device was placed in a vacuum bag, the vacuum valve was opened to form a vacuum environment, and all 6 baking chambers were preheated at 100°C for 20 minutes and then heated to 190°C. The baking chambers moved along the X and Y axes at the same time and dripped material into the cuboid groove mold 1. The dripping rate was 32g / min, and a block polyurethane prototype was obtained.
[0065] The aforementioned baking chambers move simultaneously along the X-axis and Y-axis. Specifically, the X-axis speed of the first baking chamber 7 is 1.5 m / min and the Y-axis speed is 2 m / min; the X-axis speed of the second baking chamber 8 is 1.7 m / min and the Y-axis speed is 1.8 m / min; the X-axis speed of the third baking chamber 9 is 2.2 m / min and the Y-axis speed is 1.3 m / min; the X-axis speed of the fourth baking chamber 10 is 2.8 m / min and the Y-axis speed is 0.8 m / min; the X-axis speed of the fifth baking chamber 11 is 1.8 m / min and the Y-axis speed is 1.8 m / min; and the X-axis speed of the sixth baking chamber 12 is 2.2 m / min and the Y-axis speed is 1.8 m / min.
[0066] (2) Close the vacuum valve and temperature control switch, cool the block polyurethane prototype obtained in step (1) with circulating water, and cut it along the direction perpendicular to the dripping material to obtain the water-ink style polyurethane material.
[0067] The above-mentioned ink-wash style floral color preparation device, such as Figure 1As shown, the ink-wash style floral pattern preparation device includes six independently movable baking chambers. Each baking chamber has a grating 2 at its bottom, with a mesh size of 150. The mold 1 is a rectangular groove. Above the mold are an X-axis slide rail 4, a Y-axis slide rail 3, an X-axis slider 6, and a Y-axis slider 5. The X-axis slide rails for all six baking chambers are 0.3m long, and the Y-axis slide rails are 0.4m long. Each slider has a groove that slides into the slide rail. The baking chamber is connected to the Y-axis slide rail slider and is located above the mold. The Y-axis slide rail is connected to the X-axis slide rail via the X-axis slider.
[0068] Example 2
[0069] This embodiment provides a water-based ink-style floral polyurethane material and its preparation method. The preparation method of the water-based ink-style floral polyurethane material includes the following steps:
[0070] (1) Add 40 parts by weight of polyurethane granules, 10 parts by weight of polyurethane masterbatch, 3 parts by weight of hydrolysis resistant agent and 3 parts by weight of UV resistant additive granules into the first baking chamber 7.
[0071] Add 40 parts by weight of polyurethane granules, 10 parts by weight of polyurethane masterbatch, 3 parts by weight of hydrolysis resistant agent and 3 parts by weight of UV resistant additive granules into the second baking chamber 8.
[0072] Add 40 parts by weight of polyurethane granules, 10 parts by weight of polyurethane masterbatch, 3 parts by weight of hydrolysis resistant agent and 3 parts by weight of UV resistant additive granules into the third baking chamber 9.
[0073] Add 40 parts by weight of polyurethane granules, 10 parts by weight of polyurethane masterbatch, 3 parts by weight of hydrolysis resistant agent and 3 parts by weight of UV resistant additive granules into the fourth baking chamber 10.
[0074] Then, the ink-style floral pattern preparation device was placed in a vacuum bag, the vacuum valve was opened to form a vacuum environment, and the four baking chambers were preheated at 130°C for 18 minutes and then heated to 180°C. The baking chambers moved along the X and Y axes at the same time and dripped material into the cuboid groove mold 1. The dripping rate was 25g / min, and a block polyurethane prototype was obtained.
[0075] Specifically, the X-axis and Y-axis movements of the aforementioned baking chambers are as follows: the X-axis movement speed of the first baking chamber 7 is 0.5 m / min and the Y-axis movement speed is 3 m / min; the X-axis movement speed of the second baking chamber 8 is 0.5 m / min and the Y-axis movement speed is 3 m / min; the X-axis movement speed of the third baking chamber 9 is 0.5 m / min and the Y-axis movement speed is 3 m / min; and the X-axis movement speed of the fourth baking chamber 10 is 0.5 m / min and the Y-axis movement speed is 3 m / min.
[0076] (2) Close the vacuum valve and temperature control switch, cool the block polyurethane prototype obtained in step (1) with circulating water, and cut it along the direction perpendicular to the dripping material to obtain the water-ink style polyurethane material.
[0077] The above-mentioned ink-wash style floral color preparation device, such as Figure 2 As shown, the ink-wash style floral pattern preparation device includes four independently movable baking chambers. Each baking chamber has a grating 2 at its bottom, with a mesh size of 200. The mold 1 is a rectangular groove. Above the mold are an X-axis slide rail 4, a Y-axis slide rail 3, an X-axis slider 6, and a Y-axis slider 5. The X-axis slide rails for all four baking chambers are 0.3m long, and the Y-axis slide rails are 0.4m long. Each slider has a groove that slides into the slide rail. The baking chamber is connected to the Y-axis slide rail slider and is located above the mold. The Y-axis slide rail is connected to the X-axis slide rail via the X-axis slider.
[0078] Example 3
[0079] This embodiment provides a water-based ink-style floral polyurethane material and its preparation method. The preparation method of the water-based ink-style floral polyurethane material includes the following steps:
[0080] (1) Add 20 parts by weight of polyurethane granules, 1 part by weight of polyurethane masterbatch, 1 part by weight of hydrolysis resistant agent and 1 part by weight of UV resistant additive granules into the first baking chamber.
[0081] Add 20 parts by weight of polyurethane granules, 1 part by weight of polyurethane masterbatch, 1 part by weight of hydrolysis resistant agent and 1 part by weight of UV resistant additive granules into the second baking chamber;
[0082] Add the granular mixture of 20 parts by weight of polyurethane granules, 1 part by weight of polyurethane masterbatch, 1 part by weight of hydrolysis resistant agent and 1 part by weight of UV resistant additive to the third baking chamber.
[0083] Add 20 parts by weight of polyurethane granules, 1 part by weight of polyurethane masterbatch, 1 part by weight of hydrolysis resistant agent and 1 part by weight of UV resistant additive granules into the fourth baking chamber.
[0084] Add 20 parts by weight of polyurethane granules, 1 part by weight of polyurethane masterbatch, 1 part by weight of hydrolysis resistant agent and 1 part by weight of UV resistant additive granules into the fifth baking chamber.
[0085] Add the granular mixture of 20 parts by weight of polyurethane granules, 1 part by weight of polyurethane masterbatch, 1 part by weight of hydrolysis resistant agent and 1 part by weight of UV resistant additive to the sixth baking chamber.
[0086] Then, the ink-style floral pattern preparation device and mold were placed in a vacuum bag, the vacuum valve was opened to form a vacuum environment, and all six baking chambers were preheated at 110°C for 20 minutes and then heated to 220°C. The baking chambers moved along the X and Y axes at the same time and dripped material into the cuboid groove mold. The dripping rate was 45g / min, and a block polyurethane prototype was obtained.
[0087] The aforementioned baking chambers move simultaneously along the X-axis and Y-axis, specifically as follows: the X-axis speed of the first baking chamber is 3 m / min and the Y-axis speed is 0.5 m / min; the X-axis speed of the second baking chamber is 3 m / min and the Y-axis speed is 0.5 m / min; the X-axis speed of the third baking chamber is 3 m / min and the Y-axis speed is 0.5 m / min; the X-axis speed of the fourth baking chamber is 3 m / min and the Y-axis speed is 0.5 m / min; the X-axis speed of the fifth baking chamber is 3 m / min and the Y-axis speed is 0.5 m / min; and the X-axis speed of the sixth baking chamber is 3 m / min and the Y-axis speed is 0.5 m / min.
[0088] (2) Close the vacuum valve and temperature control switch, cool the block polyurethane prototype obtained in step (1) with circulating water, and cut it along the direction perpendicular to the dripping material to obtain the water-ink style polyurethane material.
[0089] The aforementioned ink-wash style floral decoration preparation device includes six independently movable baking chambers. Each baking chamber has a sieve at its bottom, with a mesh size of 120. The mold is a rectangular groove. Above the mold are X-axis slide rails, Y-axis slide rails, X-axis sliders, and Y-axis sliders. The X-axis slide rails for all six baking chambers are 0.3m long, and the Y-axis slide rails are 0.4m long. Each slider has a groove that slidably engages with the slide rail. The baking chamber is connected to the Y-axis slide rail slider and located above the mold. The Y-axis slide rail is connected to the X-axis slide rail via the X-axis slider.
[0090] Example 4
[0091] This embodiment provides a polyurethane material with ink-like floral patterns and its preparation method. The only difference between this embodiment and Example 1 is that the Y-axis movement speed of the first baking chamber in step (1) is adjusted to 4 m / min. The rest is the same as Example 1.
[0092] Example 5
[0093] This embodiment provides a water-ink style polyurethane material and its preparation method. The only difference between this embodiment and Example 1 is that a mixture of 8 parts by weight of polyurethane particles, 0.5 parts by weight of polyurethane masterbatch, 1.5 parts by weight of hydrolysis resistant agent and 1 part by weight of UV resistant agent is added to the first baking chamber. The rest is the same as in Example 1.
[0094] Example 6
[0095] This embodiment provides a water-ink style polyurethane material and its preparation method. The only difference between this embodiment and Example 1 is that a mixture of 8 parts by weight of polyurethane particles, 12 parts by weight of polyurethane masterbatch, 1.5 parts by weight of hydrolysis resistant agent and 1 part by weight of UV resistant agent is added to the first baking chamber. Otherwise, it is the same as Example 1.
[0096] Example 7
[0097] This embodiment provides a water-ink style polyurethane material and its preparation method. The only difference between this embodiment and Example 1 is that the mesh size of the stencil in step (1) is adjusted to 110 mesh, and the dripping rate is changed to 55 g / min. The rest is the same as Example 1.
[0098] Example 8
[0099] This embodiment provides a water-ink style polyurethane material and its preparation method. The only difference between this embodiment and Example 1 is that the mesh size of the stencil in step (1) is adjusted to 210 mesh, and the dripping rate is changed to 18 g / min. The rest is the same as Example 1.
[0100] Comparative Example 1
[0101] This comparative example provides a polyurethane material with ink-like floral patterns and its preparation method. The only difference between this example and Example 1 is that the temperature rise in step (2) is adjusted to 160°C, and the dripping rate is changed to 0 g / min. The rest is the same as Example 1.
[0102] Comparative Example 2
[0103] This comparative example provides a polyurethane material with ink-like floral patterns and its preparation method. The only difference between this example and Example 1 is that the temperature rise in step (2) is adjusted to 240°C, and the dripping rate is changed to 60g / min. The rest is the same as Example 1.
[0104] Comparative Example 3
[0105] This comparative example provides a water-ink style polyurethane material and its preparation method. The only difference between this material and Example 1 is that no polyurethane masterbatch is added; otherwise, they are the same as in Example 1.
[0106] The following performance tests were conducted on the water-ink pattern polyurethane materials provided in the examples and comparative examples.
[0107] (1) Ink-wash floral pattern: When observing the polyurethane material with ink-wash floral patterns, if the pattern contains curved lines and areas with the color of polyurethane masterbatch, gradient lines and areas at the boundary between polyurethane particles and the molten polyurethane masterbatch, and curved lines and areas with the color of polyurethane particles, and the lines are clearly defined curves without large areas of overlapping color areas formed by the colors of polyurethane particles and polyurethane masterbatch, and the pattern exhibits natural fluid flow characteristics and style, possessing the visual effect of ink-wash floral patterns, and has no or only a small number of overlapping color areas, it is considered to have a good effect.
[0108] If the different colors are unevenly distributed, with overlapping color areas and crystal points, but the curves or areas of the polyurethane masterbatch color, the gradient color lines or areas at the boundary between the polyurethane particles and the polyurethane masterbatch melt, and the curves or areas with the color of the polyurethane particles can still be observed, the effect is considered good.
[0109] If the pattern distribution is chaotic, with large areas of overlapping colors, and the curves or areas of polyurethane masterbatch color, the gradient lines or areas at the boundary between polyurethane particles and the melt of polyurethane masterbatch, and the curves or areas with polyurethane particle color are unclear or nonexistent, and there is no ink-wash pattern, it is considered a poor effect.
[0110] (2) Thickness: The thickness was tested using a Teclock SM-114 thickness gauge.
[0111] (3) Hardness: Tested according to ASTM-D2240 SHORE A.
[0112] (4) Tensile strength and elongation at break: Tested according to ASTM-D412 (Type C). During preparation, the Y-axis movement direction is longitudinal and the X-axis movement direction is transverse.
[0113] (5) Tear strength: Tested according to ASTM-D624 (right angle type). During preparation, the Y-axis movement direction is longitudinal and the X-axis movement direction is transverse.
[0114] The test results are shown in Tables 1 and 2.
[0115] Table 1
[0116]
[0117] Table 2
[0118]
[0119]
[0120] In Table 2, "-" indicates that no test results were obtained.
[0121] According to the test results in Tables 1 and 2, the ink-wash style polyurethane material provided by this invention has ink-wash style patterns, excellent decorative effect, and features simple preparation, convenient processing, resistance to peeling, good color fastness, and good mechanical properties. The longitudinal tensile strength of the ink-wash style polyurethane material provided in Examples 1-8 is 54.8-56.9 MPa.
[0122] Compared with Example 1, if the Y-axis movement speed of the first baking chamber is too fast (Example 4), the first baking chamber is prone to dripping material into the dripping area of the fourth baking chamber. The patterns affect each other, resulting in overlapping color areas and a decrease in the effect of the ink-wash floral pattern. This proves that when the X-axis and Y-axis movement speeds of the baking chamber are within a specific range, the ink-wash floral pattern effect of the polyurethane material is better.
[0123] Compared with Example 1, if the weight percentage of polyurethane masterbatch in the first baking chamber is too low (Example 5), the color distribution of the polyurethane material forming the ink-wash pattern is uneven in different areas of the first baking chamber, the color is not bright enough, and the ink-wash pattern effect is reduced. If the weight percentage of polyurethane masterbatch in the first baking chamber is too high (Example 6), the color of the polyurethane masterbatch in the area of the polyurethane material forming the ink-wash pattern is too concentrated, the gradient lines and area effects are worse, and the ink-wash pattern effect is reduced. This proves that when the weight percentage of polyurethane masterbatch is within a certain range, the ink-wash pattern effect of the polyurethane material is better.
[0124] Compared with Example 1, if the mesh count of the stencil is too small (Example 7), it is easy to cause material jamming, untimely dripping, uneven flow of polyurethane masterbatch, uneven color distribution, and reduced ink-wash pattern effect; if the mesh count of the stencil is too large (Example 8), it is easy to cause insufficiently melted polyurethane granule mixture to drip down, causing crystal points, insufficient flow and other defects, and reduced ink-wash pattern effect. This proves that when the mesh count of the stencil is within a certain range, the ink-wash pattern effect of the polyurethane material is better.
[0125] Compared with Example 1, if the heating temperature is too low (Comparative Example 1), the polyurethane granule mixture has low fluidity and cannot flow smoothly out of the stencil, thus failing to produce the ink-like floral polyurethane material.
[0126] Compared with Example 1, if the temperature is too high (Comparative Example 2), the polyurethane colored masterbatch will flow excessively, resulting in a large area of overlapping color areas formed by the colors of the polyurethane particles and the polyurethane masterbatch. The lines will not be clear and smooth, and the ink-wash floral pattern effect will be poor.
[0127] Compared with Example 1, if no polyurethane masterbatch is added (Comparative Example 3), the ink-wash pattern polyurethane material presents a single color without any ink-wash pattern.
[0128] The applicant declares that the present invention is illustrated by the above embodiments, but the present invention is not limited to the above process steps, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials used in the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a water-ink style floral polyurethane material, characterized in that, The preparation method includes the following steps: (1) Add polyurethane granule mixture to each baking chamber of the ink-wash style floral color preparation device, preheat at 100-130℃ for 15-20 min, and raise the temperature to 180-220℃. The baking chamber moves along the X-axis and Y-axis at the same time and drips the material into the mold to obtain a block polyurethane prototype. The movement speed of the baking chamber along the X-axis and the movement speed along the Y-axis are each 0.5-3 m / min. The polyurethane granule mixture added to each of the baking chambers is independently a granule mixture comprising 20-40 parts by weight of polyurethane granules, 1-10 parts by weight of polyurethane masterbatch, 1-3 parts by weight of hydrolysis resistant agent and 0.1-3 parts by weight of UV resistant agent. The color of the polyurethane granules is different from that of the polyurethane masterbatch. (2) The block polyurethane prototype obtained in step (1) is cooled and cut along the direction perpendicular to the dripping to obtain the ink-style floral polyurethane material. The ink-wash style floral pattern preparation device includes a mold and at least two independently movable baking chambers. The bottom of each baking chamber is provided with a slatted screen with a mesh size of 120-200. The dripping rate of each baking chamber is independently 25-45 g / min.
2. The preparation method according to claim 1, characterized in that, The ink-wash style floral pattern preparation device includes 4-6 independently movable baking chambers.
3. The preparation method according to claim 1, characterized in that, The mold is provided with an X-axis slide rail, a Y-axis slide rail, an X-axis slider, and a Y-axis slider. The X-axis slider is provided with a groove that slides into the X-axis slide rail. The Y-axis slider is provided with a groove that slides into the Y-axis slide rail. The baking chamber is connected to the Y-axis slide rail via a slider, and the Y-axis slide rail is connected to the X-axis slide rail via the X-axis slider.
4. The preparation method according to claim 1, characterized in that, The steps of preheating, heating, and simultaneously moving the baking chamber along the X and Y axes and dripping material into the mold in step (1) are carried out in a vacuum environment.
5. The preparation method according to claim 1, characterized in that, The cooling in step (2) includes water cooling.
6. A polyurethane material with ink-wash style floral patterns, characterized in that, The ink-wash style polyurethane material is prepared by the preparation method described in any one of claims 1-5.
7. The application of the ink-wash style polyurethane material as described in claim 6 in shoe materials or electronic product component materials.
Citation Information
Patent Citations
Bright printing coating fabric
CN202192821U
High-emulation artificial leather
CN202227183U
Gantry type simulation texture drawing machine
CN112277217A
Automated Forming Of Cast Polyurethane
US20140264997A1
Method for creating patterns in cast materials