A benzyl side chain-free polyphenylene ether anion exchange membrane and preparation method thereof

By using ether bonds to connect large-volume benzene ring structures and Williamson etherification reaction grafting technology in anion exchange membranes, the problems of stability and low ion conductivity of anion exchange membranes in alkaline environments are solved, and high-performance Alkaline fuel cell membrane materials.

CN117766828BActive Publication Date: 2024-10-25SICHUAN JUXIONG PLASTIC TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310659327.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-05
Publication Date
2024-10-25
Estimated Expiration
2043-06-05

AI Technical Summary

Technical Problem

Anion exchange membrane has poor stability and low ion conductivity in alkaline environment, which hinders the commercial application of alkaline fuel cells.

Method used

Polyphenylene ether is used as the main chain, and the large-volume benzene ring structure is connected through ether bonds to avoid the benzyl structure. A benzyl side chain-free polyphenylene ether anion exchange membrane is designed, and the steric hindrance effect of the benzene ring is used to improve the alkali resistance of the membrane. performance, and graft 4-hydroxyphenylethyl bromide through Williamson etherification reaction, and adjust the grafting rate to optimize membrane performance.

Benefits of technology

The alkali resistance and ionic conductivity of the membrane are improved. The OH- conductivity can reach 50.9mS·cm-1 at 80°C, maintaining good dimensional stability. Piperidine-type AEMs show the highest ionic conductivity and mechanical strength. The elongation at break can reach 17.6%, and the initial conductivity is still 64% after being soaked in 1M NaOH solution for 480 hours.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117766828B_ABST
    Figure CN117766828B_ABST
Patent Text Reader

Abstract

The present invention relates to a membrane material, and in particular to a membrane material for application in anion exchange membrane fuel cells. The present invention uses polyphenylene ether (PPO) as a polymer main chain. Compared with a full carbon main chain without an ether oxygen bond, PPO is insufficient in alkali resistance stability, but the attack of OH to the main chain ether oxygen bond can be effectively alleviated by the reasonable structural design of the side chain, and PPO is a common commercial polymer with a wide range of sources, multiple reactive sites, and excellent film-forming properties. Connecting a bulky benzene ring structure through an ether bond can, on the one hand, utilize the steric hindrance effect of the benzene ring to hinder the attack of OH to AEMs, and on the other hand, the ether bond connected to the benzene ring as an electron-donating group can further improve the alkali resistance of the membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a membrane material, in particular to a membrane material used in an anion exchange membrane fuel cell. Background Art

[0002] In recent years, due to the increasingly serious environmental pollution caused by the consumption of fossil fuels, it is urgent to develop an efficient and clean green energy. Fuel cells, as a part of high-tech clean energy, have the advantages of being pollution-free and easy to build. Among them, alkaline fuel cells (AEMFC) have the advantages of fast reaction kinetics, high electrode reaction efficiency, and no need for non-precious metal catalysts. They are the most ideal high-tech clean energy today. However, the anion exchange membrane (AEMs), a key component in the alkaline fuel cell assembly structure that isolates fuel and gas, transmits ions, and supports reaction catalysts, still has the problems of low ion conductivity and poor alkaline stability, which hinders the commercial application of alkaline fuel cells.

[0003] In order to solve the problems of poor stability and low ion conductivity of AEMs in alkaline environments, researchers have adopted many strategies to improve the performance of membranes. Side chain modification is currently the most widely used modification strategy for AEMs. Compared with modification strategies such as cross-linking and block, side chain modification is simple to operate and easy to control. It can also improve the ion conductivity and alkali resistance of the membrane by designing the molecular configuration and optimizing the microphase structure in the membrane to form a continuous and complete ion transmission channel. Chu et al. synthesized two different side chain AEMs to explore the effects of side chain length and whether it contains triazole groups on the performance of side chain AEMs. The results show that the large triazole groups in the side chains can provide more transport sites for water, thereby improving the ion conductivity of the membrane, and the length of the side chains also affects the structural stability of the membrane. Long side chains can effectively alleviate the degradation of polymer membranes, but too long side chains can also lead to a decrease in membrane performance (X.Chu, J.Liu, S.Miao, et al., Crucial role of side-chain functionality in anion exchange membranes: Properties and alkaline fuel cell performance [J]. Journal of Membrane Science. 2021.625119172.). In addition, the researchers found that when the presence of benzyl structures is avoided, the alkaline stability and conductivity of the membrane are improved, and the presence of large-volume geometric structures in the side chains can alleviate OH by providing greater steric hindrance. -In summary, the present invention studies and designs a side chain type AEMs with a large rigid structure, and avoids the unstable benzyl structure through ether bonds, trying to solve the OH group that restricts the development of AEMs. - Problems of low conductivity and poor alkali resistance. Summary of the invention

[0004] The present invention adopts polyphenylene ether (PPO) as the polymer main chain. Compared with the full carbon main chain without ether oxygen bond, PPO is insufficient in alkali resistance and stability, but the reasonable structural design of the side chain can effectively alleviate the OH - The attack on the main chain ether oxygen bond, and PPO as a common commercial polymer, its source is wide, has multiple reactive sites, and has excellent film-forming properties. Connecting the bulky benzene ring structure through ether bonds can use the steric hindrance effect of the benzene ring to hinder the OH - attack on AEMs, on the other hand, the ether bonds connected to the benzene ring as electron-donating groups can further improve the alkali resistance of the membrane.

[0005] The present invention provides a benzyl side chain-free polyphenylene ether anion exchange membrane, characterized in that the general formula of the anion exchange membrane is:

[0006]

[0007] Where R is selected from X>1.

[0008] The present invention also provides a method for preparing a benzyl side chain-free polyphenylene ether anion exchange membrane, which comprises the following steps:

[0009] S1: Synthesis of brominated polyphenylene ether (BPPO);

[0010] S2: quaternizing 4-hydroxyphenethyl bromide with a quaternizing agent to obtain HO-Ph-R;

[0011] S3: subjecting the brominated polyphenylene ether prepared in step S1 to a Williamson etherification reaction with the HO-Ph-R prepared in step S2 to graft HO-Ph-R onto BPPO to form a PPO-O-Ph-R precursor;

[0012] S4: using the PPO-O-Ph-R precursor prepared in step S3 as a membrane-forming matrix to prepare an anion exchange membrane.

[0013] Preferably, the quaternizing agent is trimethylamine, 1-methylpiperidine or 1-methylimidazole.

[0014] Preferably, the grafting rate of BPPO in step S1 is 30-60%.

[0015] Preferably, the specific steps of step S1 are: mixing polyphenylene ether and chlorobenzene to form a homogeneous solution, adding azobisisobutyronitrile and N-bromosuccinimide, heating to 120-150° C. and stirring to react for 4-10 hours; after the reaction is completed, pouring the solution into excess ethanol to form a precipitate, and vacuum drying the precipitate to obtain brominated polyphenylene ether.

[0016] Preferably, after the precipitate is formed in step S1, the precipitate is redissolved in chloroform to remove residual impurities, and excess ethanol is introduced again for re-precipitation.

[0017] Preferably, the specific steps of step S2 are: dissolving 4-hydroxyphenethyl bromide in N-methylpyrrolidone, adding a quaternary ammonium agent dropwise, and stirring the reaction for 8-20 hours; after the reaction is completed, pouring the solution into excess ethyl acetate to obtain a precipitate; washing, filtering, and drying the precipitate to form HO-Ph-R.

[0018] Preferably, the specific steps of step S3 are: dissolving NaH and tetrabutylammonium bromide in N-methylpyrrolidone, stirring under a nitrogen atmosphere, dropping the HO-Ph-R solution dissolved in N-methylpyrrolidone, and stirring and reacting at 30-60° C. for 1-4 hours; after the reaction is completed, continue to drop the brominated polyphenylene ether solution dissolved in N-methylpyrrolidone, continue to stir and react at 30-60° C. and N2 for 12-24 hours, centrifuge the reactant, take the supernatant and continue to pour it into acetone to generate a precipitate, filter, wash, and vacuum dry to obtain a PPO-O-Ph-R precursor.

[0019] Preferably, the specific steps of step S4 are: dissolving PPO-O-Ph-R in a solvent, filtering, and standing to degas to form a casting solution; pouring the casting solution on a glass plate, pre-evaporating the solvent for 0.2-1h, and then vacuum drying at 60-100°C, and after the solvent is completely evaporated, soaking the glass plate in deionized water to remove the obtained membrane from the glass plate; finally, soaking the membrane in a 0.5-2M NaOH solution for 12-24h to replace Br- with OH-, and repeatedly rinsing with deionized water to obtain an anion exchange membrane.

[0020] The specific synthetic route of the present invention is:

[0021]

[0022] The benzyl side chain-free polyphenylene ether anion exchange membrane prepared by the invention can be used in anion exchange membrane fuel cells.

[0023] The present invention selects commercially available polyphenylene ether as the polymer main chain, utilizes bromomethylation and Williamson etherification reaction, grafts 4-hydroxyphenylethyl bromide onto the polyphenylene ether main chain, and then quaternizes it to prepare side chain polyphenylene ether-based AEMs. Compared with the prior art, the present invention has the following effects.

[0024] (1) Through the Williamson etherification reaction, 4-hydroxyphenylethyl bromide containing a large rigid structure is grafted onto the main chain of polyphenylene ether, and the conventional N-bonded benzyl structure is avoided by ether bond connection to alleviate OH - The attack on the main chain. The steric hindrance effect provided by the bulky benzene ring further improves the alkali resistance of the membrane. The rigid benzene ring structure improves the membrane's anti-swelling performance.

[0025] (2) The best performance of AEMs was obtained by adjusting the grafting rate. When the grafting rate of the membrane was 46%, the performance of the membrane was the best. - Conductivity can reach 50.9mS·cm -1 , maintaining good dimensional stability while having a certain water absorption rate.

[0026] (3) The membrane quaternized with piperidine showed the highest ionic conductivity, with OH - The conductivity can reach 69.8mS·cm at 80℃ -1 The piperidine-type AEMs not only exhibit excellent ionic conductivity but also have certain mechanical strength. In the wet state, the elongation at break can reach 17.6%, and it still retains 64% of the initial conductivity after being immersed in 1M NaOH solution for 480h. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Contact angles of different films of Examples 1-3;

[0028] Figure 2 Examples 1-3 Ionic conductivity of different membranes;

[0029] Figure 3 Thermogravimetric curves of different films of Examples 1-3;

[0030] Figure 4 Example 1-3 (a) Alkali resistance test, (b) Battery performance test. DETAILED DESCRIPTION

[0031] Example 1

[0032] (1) Synthesis of brominated polyphenylene ether

[0033] The specific steps of the synthesis of BPPO are as follows: add 6g of commercially available PPO and 60mL of chlorobenzene to a two-necked round-bottom flask equipped with a condensing device, stir and dissolve at 80°C, and after it is completely dissolved to form a homogeneous solution, add 0.3g of azobisisobutyronitrile (AIBN) and 3.6g of N-bromosuccinimide (NBS), heat to 135°C, stir and react for 8h, and after the reaction is completed, stir and pour the homogeneous solution into excess ethanol to precipitate to form a light brown precipitate of BPPO. The precipitated product BPPO is redissolved in 60mL of chloroform to remove residual impurities. After BPPO is completely dissolved, it is poured into excess ethanol for reprecipitation. The precipitated product is moved into a 60°C vacuum drying oven and dried for 48h to obtain BPPO. The degree of bromination is controlled by adjusting the amount of NBS, and the degree of bromination is calculated by nuclear magnetic resonance hydrogen spectrum.

[0034] (2) Synthesis of small molecule HO-Ph-QA

[0035] The commercially available 4-hydroxyethyl bromide was pre-quaternized for the next reaction. The synthesis steps of HO-Ph-QA are as follows: 10 mL of DMF solution was dissolved in 1 g of 4-hydroxyethyl bromide, the solution was stirred at 40 ° C, 3 mL of trimethylamine solution was slowly dripped into the stirred 4-hydroxyethyl bromide, the solution was stirred for 12 hours, after the reaction, the solution was poured into excess ethyl acetate to obtain a white precipitate, and the product was washed with ether two to three times. The precipitated product was filtered through a Buchner funnel, and the filtered product was moved to a 60 ° C vacuum drying oven for vacuum drying for 24 hours to remove the residual solvent, and the product was named HO-Ph-QA.

[0036] (3) Preparation of PPO-O-Ph-QA by Williamson etherification reaction

[0037] HO-Ph-QA was grafted on the polymer main chain BPPO with a grafting rate of 46% by Williamson etherification reaction. The specific experimental operation is as follows: 10mL NMP solution was used to dissolve 0.42g HO-Ph-QA, and it was transferred to a dropping funnel for use. 0.1g NaH and 0.1g tetrabutylammonium bromide were added to a three-necked flask, and 8mL NMP solution was added to dissolve. Then nitrogen (N2) was introduced and stirred. When NaH was evenly dispersed in the solution, the dropping funnel was opened and the HO-Ph-QA solution was slowly added dropwise. The reaction was stirred at 40°C and N2 atmosphere for 2h. Subsequently, 1g BPPO polymer was dissolved in 20mL NMP until it was completely dissolved, and then slowly added dropwise to the stirring HO-Ph-QA solution, and the reaction was stirred overnight at 40°C and N2 conditions. After reacting overnight, the insoluble precipitate was removed by centrifugation, the supernatant was poured into acetone to generate a precipitate, which was filtered and washed with ethanol to remove the residual HO-Ph-QA small molecules. The product was then transferred to a 60°C vacuum drying oven and dried for 24 hours to obtain a product named PPO-O-Ph-QA.

[0038] (4) Preparation of anion exchange membrane

[0039] Dissolve 1g PPO-O-Ph-QA in 19mL NMP solution and stir with a mechanical stirring device. After the polymer is completely dissolved, filter the casting solution with a filter cloth to remove a small amount of insoluble impurities, and then let it stand for 12 hours to eliminate the damage of bubbles to the membrane structure. After the casting solution is degassed, cast the casting solution on a clean glass plate that has been heated in advance, pre-evaporate the solvent for 0.5h, and further remove the residual solvent under vacuum at 80°C to obtain a transparent and flexible film. Soak the glass plate in deionized water to remove the obtained film from the glass plate. Finally, soak the membrane in 1M NaOH solution for 24h to remove Br - Replaced by OH - The AEMs were then rinsed repeatedly with deionized water.

[0040] Example 2

[0041] (1) Synthesis of brominated polyphenylene ether (BPPO)

[0042] Add 6g of commercially available PPO and 60mL of chlorobenzene to a flask equipped with a condensing device, stir and dissolve at 80°C, and after forming a homogeneous solution, add 0.9g of AIBN and 10.8g of NBS, raise the temperature to 135°C, stir and react for 8h, and then pour the homogeneous solution into excess ethanol to precipitate a light brown precipitate of BPPO. Then dissolve BPPO in 60mL of chloroform, and after it is completely dissolved, re-precipitate it in ethanol. Move the precipitated product into a 60°C vacuum drying oven and dry it for 48h to obtain BPPO.

[0043] (2) Synthesis of small molecule HO-Ph-Pi

[0044] The commercially available 4-hydroxyethyl bromide was quaternized for the next reaction. The synthesis steps of HO-Ph-Pi are as follows: 10 mL of DMF solution was used to dissolve 1 g of 4-hydroxyethyl bromide, the solution was stirred at 40 ° C, 730 μL of 1-methylpiperidine solution was slowly dripped into the stirred 4-hydroxyethyl bromide, the solution was stirred for 12 hours, after the reaction was completed, the solution was poured into excess ethyl acetate to obtain a white precipitate, and the product was washed with ether two to three times. The precipitated product was filtered through a Buchner funnel, and the filtered product was moved to a 60 ° C vacuum drying oven for vacuum drying for 24 hours to remove the residual solvent, and the product was named HO-Ph-Pi.

[0045] (3) Synthesis of the precursor PPO-O-Ph-Pi

[0046] HO-Ph-Pi was grafted on the polymer main chain BPPO with a grafting rate of 46% by Williamson etherification reaction. The specific experimental operation is as follows: 10mL NMP solution was taken to dissolve 0.52g HO-Ph-Pi. After complete dissolution, it was transferred to a dropping funnel. 0.1g NaH and 0.1g tetrabutylammonium bromide were added to a three-necked flask, and NMP solution was added to dissolve. Stir under nitrogen (N2) atmosphere. When NaH is evenly dispersed in the solution, open the dropping funnel and slowly drop HO-Ph-Pi solution. The reaction was stirred at 40°C and N2 atmosphere for 2h to terminate the dehydrogenation reaction. Subsequently, 20mL NMP solution in which 1g BPPO polymer was dissolved was slowly added dropwise to the stirring HO-Ph-Pi solution, and the reaction was stirred overnight at 40°C and N2 conditions. After reacting overnight, the insoluble precipitate was removed by centrifugation, the supernatant was poured into acetone to generate a precipitate, which was filtered and washed with ethanol to remove the residual HO-Ph-Pi small molecules. The product was then transferred to a 60°C vacuum drying oven and dried for 24 hours to obtain a product named PPO-O-Ph-Pi.

[0047] (4) Preparation of anion exchange membrane

[0048] 1g PPO-O-Ph-Pi was dissolved in 19mL NMP solution and stirred by mechanical device. After PPO-O-Ph-Pi was dissolved, the casting solution was filtered with filter cloth to remove a small amount of insoluble impurities and allowed to stand for 12 hours to remove the damage of bubbles to the membrane structure. After the casting solution was degassed, the casting solution was cast on a clean glass plate that had been heated in advance, the solvent was pre-evaporated for 0.5 hours, and the residual solvent was further removed under vacuum at 80°C to obtain a transparent and flexible membrane. The glass plate was soaked in deionized water to remove the obtained membrane from the glass plate. Finally, the membrane was soaked in 1M NaOH solution for 24 hours to replace Br- with OH-, and then the AEMs were repeatedly rinsed with deionized water.

[0049] Example 3

[0050] (1) Synthesis of brominated polyphenylene ether (BPPO)

[0051] Add 6g of commercially available PPO and 60mL of chlorobenzene to a flask equipped with a condensing device, stir and dissolve at 80°C, and after forming a homogeneous solution, add 0.9g of AIBN and 10.8g of NBS, raise the temperature to 135°C, stir and react for 8h, and then pour the homogeneous solution into excess ethanol to precipitate a light brown precipitate of BPPO. Then dissolve BPPO in 60mL of chloroform, and after it is completely dissolved, re-precipitate it in ethanol. Move the precipitated product into a 60°C vacuum drying oven and dry it for 48h to obtain BPPO.

[0052] (2) Synthesis of small molecule HO-Ph-Mi

[0053] The commercially available 4-hydroxyethyl bromide was quaternized for the next reaction. The synthesis steps of HO-Ph-Mi are as follows: 10 mL of DMF solution was used to dissolve 1 g of 4-hydroxyethyl bromide, and the solution was stirred at 40 ° C. 475 μL of 1-methylimidazole solution was slowly dripped into the stirred 4-hydroxyethyl bromide. The solution was stirred for 12 hours. After the reaction, the solution was poured into excess ethyl acetate to obtain a white precipitate, and the product was washed with ether two to three times. The precipitated product was filtered through a Buchner funnel, and the filtered product was moved to a 60 ° C vacuum drying oven for vacuum drying for 24 hours to remove the residual solvent. The product was named HO-Ph-Mi.

[0054] (3) Synthesis of the precursor PPO-O-Ph-Mi

[0055] HO-Ph-Mi was grafted on the polymer main chain BPPO with a grafting rate of 46% by Williamson etherification reaction. The specific experimental operation is as follows: 10mL NMP solution was taken to dissolve 0.45g HO-Ph-Mi. After complete dissolution, it was transferred to a dropping funnel. 0.1g NaH and 0.1g tetrabutylammonium bromide were added to a three-necked flask, and NMP solution was added to dissolve. Stir under nitrogen (N2) atmosphere. When NaH is evenly dispersed in the solution, open the dropping funnel and slowly drop HO-Ph-Mi solution. The reaction was stirred at 40°C and N2 atmosphere for 2h to terminate the dehydrogenation reaction. Subsequently, 20mL NMP solution in which 1g BPPO polymer was dissolved was slowly added dropwise to the stirring HO-Ph-Mi solution, and the reaction was stirred overnight at 40°C and N2 conditions. After reacting overnight, the insoluble precipitate was removed by centrifugation, the supernatant was poured into acetone to generate a precipitate, which was filtered and washed with ethanol to remove the residual HO-Ph-Mi small molecules. After rotary evaporation, the product was transferred to a 60°C vacuum drying oven and dried for 24 hours to obtain the product, which was named PPO-O-Ph-Mi.

[0056] (4) Preparation of anion exchange membrane

[0057] 1g PPO-O-Ph-Mi was dissolved in 19mL NMP solution and stirred by mechanical device. After PPO-O-Ph-Mi was dissolved, the casting solution was filtered with filter cloth to remove a small amount of insoluble impurities and allowed to stand for 12 hours to remove the damage of bubbles to the membrane structure. After the casting solution was degassed, the casting solution was cast on a clean glass plate that had been heated in advance, the solvent was pre-evaporated for 0.5 hours, and the residual solvent was further removed under vacuum at 80°C to obtain a transparent and flexible membrane. The glass plate was soaked in deionized water to remove the obtained membrane from the glass plate. Finally, the membrane was soaked in 1M NaOH solution for 24 hours to replace Br- with OH-, and then the AEMs were repeatedly rinsed with deionized water.

[0058] Characterization results

[0059] (1) Characterization of water absorption (WU), swelling ratio (SR), and ion exchange capacity (IEC)

[0060] Table 1 shows the IEC values, water absorption and swelling rates of the three membranes of Examples 1-3. It can be seen from the data in the table that the IEC values ​​of the three membranes are similar and close to the theoretical values. The prepared membranes have a certain amount of ion-conducting groups, which is beneficial to OH - In terms of transport, PPO-O-Ph-QA exhibited the highest IEC value, which was due to the fact that trimethylamine had the smallest size compared to other groups and thus had the greatest nucleophilicity, resulting in the membrane having the largest IEC value, while PPO-O-Ph-Pi exhibited the lowest IEC value due to its larger volume structure.

[0061] Table 1 WU, SR, IEC of membranes with different functional groups

[0062]

[0063] (2) Contact angle

[0064] The above conclusions were further confirmed by water contact angle. The water contact angle test results of all membranes are shown in Figure 1 . Compared with the unmodified PPO-O-Ph-Br, the water contact angles of all membranes decreased, among which the decrease of PPO-O-Ph-Pi was the most obvious. The water contact angles of all membranes were less than 90°. The results showed the successful introduction of cationic functional groups and the improvement of membrane hydrophilicity. Among them, piperidine most significantly improved the hydrophilicity of the membrane, with the lowest water contact angle of only 53°. This may be because compared with imidazole and trimethylamine, piperidine has the largest alkalinity and water absorption rate, making it easier to form a hydrogen bond network with water molecules, thereby improving water absorption.

[0065] (3) Ionic conductivity

[0066] The ionic conductivity and alkali stability of the membrane are always the two most critical parameters of AEMs and are important indicators of whether AEMs have practical value. Figure 2 As shown in the figure, it can be found that the ionic conductivity of all membranes increases with the increase of temperature and reaches the maximum value at 80℃, among which the conductivity of PPO-O-Ph-Pi is as high as 64mS cm at 80℃. -1 Compared with the conductivity of other AEMs, the piperidine-functionalized membrane exhibits the highest ionic conductivity. The ionic conductivity of the membrane is affected by the water absorption rate and IEC value of the membrane. Although the IEC value of the piperidine-functionalized AEM is not the highest, it has the highest water absorption rate and the highest alkalinity. Therefore, it is easier to build a complete and continuous ion transport channel, thus making the membrane have a higher ionic conductivity. This result is similar to the findings of many researchers. [89-91] Similar to the previous article, the apparent activation energies of the three membranes are between 10.96 kJ / mol and 12.37 kJ / mol. - The main driver of this is still water in the environment.

[0067] (4) Thermal stability and mechanical properties

[0068] The thermal properties of AEMs were tested using TGA in a nitrogen atmosphere to evaluate the thermal stability of the membrane in practical applications. Figure 3As shown in the figure, the weight loss of all membranes can be divided into three stages: the first stage is between 30-260℃, where the loss is caused by the water adsorbed by the membrane material and the residual solvent; the second stage between 260-450℃ is caused by the thermal decomposition of the cationic groups in the membrane material; and the third stage after 450℃ is caused by the decomposition of the polymer main chain at high temperature. The test results show that all membranes can meet the practical application of fuel cells.

[0069] The mechanical properties of the membrane were tested using an electronic universal testing machine, and all membranes were tested at room temperature and in a humid state. The test results are shown in Table 2. All membranes showed good elongation at break, which was due to the hydration of the membrane, and PPO-O-Ph-Pi showed the best elongation at break, which was due to the fact that compared with PPO-O-Ph-QA and PPO-O-Ph-Mi, piperidine-functionalized AEMs had the highest water absorption rate, thereby increasing the flexibility of the membrane, while the tensile strength was the best value for PPO-O-Ph-Mi with the lowest water absorption rate, on the one hand because of its lowest water absorption rate, and on the other hand the imidazole five-membered ring further improved the rigidity of the membrane on the basis of the side chain, and the Young's modulus of the three membranes was between 160-448MPa. The test results show that under the same side chain grafting rate, the hydrophilicity of the cationic functional group and the rigidity it provides will affect the mechanical properties of the membrane. It should be avoided that too many cationic groups are grafted to cause the membrane to absorb too much water and swell, or the hydrophobicity of the side chain should be further improved, so that the membrane has a high water absorption rate while ensuring a certain anti-swelling performance. In short, although the mechanical properties of PPO-O-Ph-QA and PPO-O-Ph-Mi are not good, they can still meet the use of fuel cells.

[0070] Table 2 Mechanical strength of different films

[0071]

[0072] (5) Alkali resistance stability

[0073] The alkali stability test in this part of the work is to immerse the three membranes of Examples 1-3 in 1M NaOH solution for 480h (20d) at the same time and test the changes in their ionic conductivity. Figure 4 As can be seen in (a), after being immersed in 1M NaOH solution at 80℃ for 480h, the ionic conductivity of all membranes still retained more than 50% of the initial conductivity, which indicates that the side chain structure membrane is beneficial to improving the alkali resistance of the membrane. Among the three cationic groups, the piperidine functional group has the best alkali resistance, and the conductivity still retains 64% of the original after immersion for 480h, while the imidazole functional group loses 48.1% of the initial conductivity. This is because the imidazole group has the lowest alkalinity compared to other groups. Secondly, the C2 position of the imidazole group has no substituent, which makes it more easily absorbed by OH. -Although the piperidine functional group has better alkali resistance than other functional groups, the performance of alkali resistance in the reported literature is still unsatisfactory, mainly because the piperidine functional group connected by N bond is more easily attacked by OH than the functional group not connected by N bond. - If you want to further improve the alkali resistance of the membrane, you can consider avoiding N-bond connection through etherification or -NH- connection, or alleviate OH by cross-linking or organic-inorganic hybrid modification. - attack.

[0074] (6) Battery performance

[0075] The piperidine anion exchange membrane was selected for battery performance testing. -1 NaOH and 2 mol·L -1 The performance of methanol / air (no carbon dioxide) fuel cell at 60°C is as follows: Figure 4 (b) As shown in the figure, the open circuit voltage of the fuel cell is 0.54 V. The limiting current density at 60°C is 26.74 mA cm -2 With 5.42mW·cm -2 The maximum power density.

Claims

1. A benzyl side chain-free polyphenylene ether anion exchange membrane, characterized in that The general formula of the anion exchange membrane is: Where R is selected from , , , X>

1.

2. A method for preparing a benzyl side chain-free polyphenylene ether anion exchange membrane as claimed in claim 1, characterized in that: It includes the following steps: S1: Synthesis of brominated polyphenylene ether; S2: quaternizing 4-hydroxyphenethyl bromide with a quaternizing agent to obtain HO-Ph-R; S3: subjecting the brominated polyphenylene ether prepared in step S1 to a Williamson etherification reaction with the HO-Ph-R prepared in step S2 to graft HO-Ph-R onto BPPO to form a PPO-O-Ph-R precursor; S4: An anion exchange membrane is prepared using the PPO-O-Ph-R precursor prepared in step S3 as a membrane-forming matrix.

3. The preparation method according to claim 2, characterized in that The quaternizing agent is trimethylamine, 1-methylpiperidine or 1-methylimidazole.

4. The preparation method according to claim 2, characterized in that The grafting rate of BPPO in step S1 is 30-60%.

5. The preparation method according to claim 2, characterized in that The specific steps of step S1 are: mixing polyphenylene ether and chlorobenzene to form a homogeneous solution, adding azobisisobutyronitrile and N-bromosuccinimide, heating to 120-150° C. and stirring to react for 4-10 hours; after the reaction is completed, pouring the solution into excess ethanol to form a precipitate, and vacuum drying the precipitate to obtain brominated polyphenylene ether.

6. The preparation method according to claim 5, characterized in that After the precipitate is formed in step S1, the precipitate is redissolved in chloroform to remove residual impurities, and excess ethanol is introduced again for re-precipitation.

7. The preparation method according to claim 2, characterized in that The specific steps of step S2 are: dissolving 4-hydroxyphenethyl bromide in N-methylpyrrolidone, adding a quaternary ammonium agent dropwise, and stirring the reaction for 8-20 hours; after the reaction is completed, pouring the solution into excess ethyl acetate to obtain a precipitate; washing, filtering, and drying the precipitate to form HO-Ph-R.

8. The preparation method according to claim 2, characterized in that The specific steps of step S3 are: dissolving NaH and tetrabutylammonium bromide in N-methylpyrrolidone, stirring under a nitrogen atmosphere, dropping the HO-Ph-R solution dissolved in N-methylpyrrolidone, and stirring the reaction at 30-60° C. for 1-4 hours; after the reaction is completed, continue to drop the brominated polyphenylene ether solution dissolved in N-methylpyrrolidone, continue to stir the reaction at 30-60° C. and N2 for 12-24 hours, centrifuge the reactant, take the supernatant and continue to pour it into acetone to generate a precipitate, filter, wash, and vacuum dry to obtain a PPO-O-Ph-R precursor.

9. The preparation method according to claim 2, characterized in that The specific steps of step S4 are: dissolving PPO-O-Ph-R in a solvent, filtering, and standing to degas to form a casting solution; pouring the casting solution on a glass plate, pre-evaporating the solvent for 0.2-1 h, and then vacuum drying at 60-100°C. After the solvent is completely evaporated, the glass plate is immersed in deionized water to remove the obtained membrane from the glass plate; finally, the membrane is immersed in a 0.5-2M NaOH solution for 12-24 h to replace Br- with OH-, and repeatedly rinsed with deionized water to obtain an anion exchange membrane.

10. Use of the benzyl side chain-free polyphenylene ether anion exchange membrane according to claim 1 in anion exchange membrane fuel cells.