A sodium ferrous sulfate positive electrode material and its preparation method and application
By processing ferrous sulfate and sodium sulfate in a high-temperature and high-pressure environment with a micro-liquid environment of low-melting-point molten salt, the problem of insufficient reaction of sodium ferrous sulfate cathode material during low-temperature sintering is solved, and the yield and quality are improved. The preparation of high-capacity sodium ferrous sulfate battery cathode materials was achieved.
Patent Information
- Application Number
- CN202311751845.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-12-19
AI Technical Summary
The existing sodium ferrous sulfate cathode material for sodium ion batteries does not react sufficiently during the calcination process at low temperature and high temperature, resulting in low yield and high impurities, which cannot be effectively solved.
The micro-liquid environment provided by low-melting-point molten salt in a high-temperature and high-pressure environment is used to uniformly mix ferrous sulfate, sodium sulfate and carbon-based coating materials and then perform heat treatment to improve the tightness and thermal diffusion performance between raw material particles. A high-capacity sodium ferrous sulfate cathode material was prepared.
The yield and quality of sodium ferrous sulfate cathode materials are improved, the atomic diffusion energy barrier is reduced, the reaction efficiency of the material during low-temperature sintering is enhanced, and the preparation of high-capacity sodium ferrous sulfate battery cathode materials is achieved.
Smart Images

Figure CN117776269B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a sodium ferrous sulfate positive electrode material and a preparation method and application thereof. Background Art
[0002] The energy storage market has risen in recent years and will usher in a leapfrog development. It is estimated that the scale of energy storage will exceed 150GWh and exceed 660GWh in 2030. The main growth comes from the power generation side. The centralized renewable energy power generation supporting energy storage power stations have maintained high growth for ten years, with a compound annual growth rate of 170%. In addition, the global energy storage market will usher in an accelerated growth stage in the next decade. By 2030, the new market demand for energy storage will reach 1361.1GWh. Considering the price reduction of lithium iron phosphate, the industry scale will exceed US$1 billion, with a compound growth rate of 142%.
[0003] Technical advantages of sodium electricity: Compared with pumped storage, electrochemical energy storage has the advantages of being less affected by geographical location, short construction period and continuously decreasing costs. Currently, lithium-ion batteries occupy a dominant position of more than 90% in electrochemical energy storage. The leading advantage of lithium-ion batteries in the field of electrochemical energy storage has given the green light to the industrial development of sodium-ion batteries with similar models. Sodium-ion batteries with higher cost performance are expected to replace lithium-ion batteries in the field of electrochemical energy storage, and the low-temperature safety and other characteristics of sodium-ion batteries have further broadened the application scenarios of supporting energy storage. With the rapid expansion of the energy storage market, it is expected to drive the industrialization process of sodium-ion batteries.
[0004] Promoting the scale and low cost of sodium-ion batteries, improving their comprehensive performance, and promoting the industrialization of sodium-ion batteries will play an important role in promoting sodium-ion batteries in the energy storage market.
[0005] At present, the main positive electrode materials of sodium ion batteries are layered oxides, polyanions, and Prussian blue. Polyanion materials are considered to be the most likely technology route for large-scale energy storage due to their naturally excellent structural stability and very low and abundant raw material costs. At present, during the preparation process of the positive electrode material of sodium ferrous sulfate battery, due to the particularity of the material, it cannot be calcined at high temperature. At low temperatures, ferrous sulfate and sodium sulfate cannot fully react, resulting in low yield and a large number of impurities. These problems have not been effectively solved. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a sodium ferrous sulfate positive electrode material and a preparation method and application thereof.
[0007] The first object of the present invention is to provide a method for preparing a sodium ferrous sulfate positive electrode material, comprising the following steps:
[0008] S1. Fully crushing and evenly mixing ferrous sulfate, sodium sulfate, carbon-based coating material and molten salt to obtain a mixed powder;
[0009] S2. Under a protective atmosphere, heat-treating the mixed powder described in S1 to obtain the sodium ferrous sulfate positive electrode material.
[0010] In one embodiment of the present invention, the melting point of the molten salt is below the heat treatment temperature, and the boiling point is above the heat treatment temperature.
[0011] In one embodiment of the present invention, in S1, the molten salt is selected from sodium nitrate and / or sodium nitrite.
[0012] In one embodiment of the present invention, in S1, the carbon-based coating material is selected from one or more of carbon nanotubes, carbon black, graphite, nanographite, graphene and carbon fiber.
[0013] In one embodiment of the present invention, in S1, the amounts of ferrous sulfate and sodium sulfate satisfy the chemical formula Na x Fe y (SO4) z , x+2y=2z, 0.5≤x / y≤2.5; the amount of the carbon-based coating material is 1wt%-10wt% of the sodium sulfate, ferrous sulfate and carbon-based coating material; the amount of the molten salt is 1wt%-5wt% of the ferrous sulfate, sodium sulfate, carbon-based coating material and molten salt.
[0014] In one embodiment of the present invention, in S1, the method of sufficient crushing and uniform mixing is selected from one or more of solid phase ball milling, wet sand milling and spray drying.
[0015] In one embodiment of the present invention, in S2, the heat treatment is performed at a temperature of 300°C-400°C and a pressure of 0.5GPa-2GPa.
[0016] In one embodiment of the present invention, in S2, the protective atmosphere is selected from a nitrogen atmosphere.
[0017] The second object of the present invention is to provide a sodium ferrous sulfate positive electrode material prepared by the method described above.
[0018] The third object of the present invention is to provide a sodium ion battery positive electrode, comprising the sodium ferrous sulfate positive electrode material, a conductive agent and a binder.
[0019] In one embodiment of the present invention, the conductive agent is selected from one or more of carbon nanotubes, acetylene black, conductive carbon black, conductive graphite, carbon fiber and graphene; the binder is selected from one or more of polyolefins, fluorine-containing resins, polypropylene resins and rubber.
[0020] Furthermore, the binder is selected from one or more of polyvinylidene fluoride, styrene rubber, nitrile rubber, styrene butadiene rubber (SBR), polyacrylamide (PAA), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylonitrile (PAN), polyimide (PI), butadiene rubber, modified butadiene rubber, carboxyl-modified styrene butadiene rubber and modified polyorganosiloxane polymers.
[0021] In one embodiment of the present invention, the amount of the conductive agent is ≤10wt%; for example, it can be 0.01wt%-10wt%, 1wt%-10wt%, 2wt%-10wt%, 3wt%-10wt%, 4wt%-10wt%, 5wt%-10wt%, 6wt%-10wt%, 7wt%-10wt%, 8wt%-10wt%, 9wt%-10wt%. 0.01wt%, 0.05wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt%, 10wt%; or any proportion between any two values.
[0022] In one embodiment of the present invention, the amount of the binder is ≤10wt%; for example, it can be 0.01wt%-10wt%, 1wt%-10wt%, 2wt%-10wt%, 3wt%-10wt%, 4wt%-10wt%, 5wt%-10wt%, 6wt%-10wt%, 7wt%-10wt%, 8wt%-10wt%, 9wt%-10wt%. 0.01wt%, 0.05wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt%, 10wt%; or any proportion between any two values.
[0023] A fourth object of the present invention is to provide a sodium ion battery, comprising the sodium ion battery positive electrode.
[0024] The technical solution of the present invention has the following advantages compared with the prior art:
[0025] (1) The preparation method described in the present invention is based on the full mixing of raw materials. It uses the high temperature and high pressure sintering environment and the micro-liquid environment provided by the low melting point molten salt to improve the tightness between the raw material particles and reduce the atomic diffusion energy barrier of the material during the low temperature sintering process, thereby improving the yield of the target product and obtaining a high-capacity sodium ferrous sulfate battery positive electrode material.
[0026] (2) The preparation method described in the present invention provides a micro-liquid environment for the material at a high temperature above 350°C through molten salt, which accelerates the thermal diffusion performance between the raw materials and accelerates the generation of the target product. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:
[0028] Figure 1 The charge and discharge performance diagram of the sodium ferrous sulfate positive electrode material prepared in the embodiment of the present invention and the comparative example 1 in the button cell at 0.2C;
[0029] Figure 2 The charge and discharge performance diagram of the sodium ferrous sulfate positive electrode material prepared in the embodiment of the present invention and the comparative example 2 in a button cell at 0.2C;
[0030] Figure 3 The charge and discharge performance diagram of the sodium ferrous sulfate positive electrode material prepared in the embodiment of the present invention and the comparative example 3 in the button cell at 0.2C;
[0031] Figure 4 This is a graph showing the charge and discharge performance of the sodium ferrous sulfate positive electrode material prepared in the embodiment of the present invention and comparative example 5 in a button cell at 0.2C. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0033] In the present invention, unless otherwise explained, technical and scientific terms used in the present invention have the same meanings as commonly understood by those skilled in the art to which the present invention belongs.
[0034] In the present invention, unless otherwise stated, the term "and / or" used in the present invention includes any and all combinations of one or more of the associated listed items.
[0035] In the present invention, unless otherwise stated, the experimental methods used in the embodiments of the present invention are conventional methods unless otherwise stated, and the materials, reagents, etc. used are all commercially available unless otherwise stated.
[0036] Example
[0037] The sodium ferrous sulfate positive electrode material and the preparation method thereof of the present invention specifically comprise the following steps:
[0038] S1. Take 199.8g of anhydrous sodium sulfate, 303.8g of anhydrous ferrous sulfate, 27.0g of CNTs powder and 5.767g of sodium nitrate, mix and crush them evenly by solid phase ball milling to obtain a mixed powder;
[0039] S2. Place the mixed powder in a hot press flat mold, and fill the closed hot press heating chamber with 99.999% high-purity nitrogen gas at a nitrogen inlet flow rate of 1m 3 / h, after charging for 30min, the gas flow rate was changed to 350mL / min, the nitrogen gas state in the closed environment was maintained, the pressurized heating device was turned on, and heat treatment was carried out under the conditions of sintering temperature of 350℃ and pressure of 1GPa to obtain sodium ferrous sulfate positive electrode material.
[0040] Comparative Example 1
[0041] S1, take 199.8g of anhydrous sodium sulfate, 303.8g of anhydrous ferrous sulfate, 27.0g of CNTs powder and 5.767g of sodium nitrate, mix and crush them evenly by solid phase ball milling to obtain a mixed powder;
[0042] S2. The mixed powder is placed in a tubular furnace and subjected to heat treatment at a sintering temperature of 350° C. in a nitrogen environment to obtain a sodium ferrous sulfate positive electrode material.
[0043] Comparative Example 2
[0044] S1, take 199.8g of anhydrous sodium sulfate, 303.8g of anhydrous ferrous sulfate, 27.0g of CNTs powder and 5.767g of sodium nitrate, mix and crush them evenly by solid phase ball milling to obtain a mixed powder;
[0045] S2. Place the mixed powder in a hot press flat mold, and fill the closed hot press heating chamber with 99.999% high-purity nitrogen gas at a nitrogen inlet flow rate of 1m 3 / h, after charging for 30min, the gas flow rate was changed to 350mL / min, the nitrogen gas state in the closed environment was maintained, the pressurized heating device was turned on, and heat treatment was carried out under the conditions of sintering temperature of 350℃ and pressure of 0.1GPa to obtain sodium ferrous sulfate positive electrode material.
[0046] Comparative Example 3
[0047] S1, take 199.8g of anhydrous sodium sulfate, 303.8g of anhydrous ferrous sulfate, 27.0g of CNTs powder and 5.767g of sodium nitrate, mix and crush them evenly by solid phase ball milling to obtain a mixed powder;
[0048] S2. Place the mixed powder in a hydraulic press flat mold, perform hydraulic treatment under a pressure of 1 GPa, then place the agglomerated material in a tubular furnace, perform heat treatment at a sintering temperature of 350° C. in a nitrogen environment, and obtain a sodium ferrous sulfate positive electrode material.
[0049] Comparative Example 4
[0050] S1, take 199.8g of anhydrous sodium sulfate, 303.8g of anhydrous ferrous sulfate, 27.0g of CNTs powder and 5.767g of sodium nitrate, mix and crush them evenly by solid phase ball milling to obtain a mixed powder;
[0051] S2. Place the mixed powder in a hot press flat mold, turn on the pressurized heating device in a nitrogen-free environment, and perform heat treatment at a sintering temperature of 350° C. and a pressure of 1 GPa to obtain a sodium ferrous sulfate positive electrode material (the material is completely oxidized).
[0052] Comparative Example 5 (without sodium nitrate)
[0053] S1. Take 199.8 g of anhydrous sodium sulfate, 303.8 g of anhydrous ferrous sulfate, and 27.0 g of CNTs powder, mix and crush them evenly by solid phase ball milling to obtain a mixed powder;
[0054] S2. Place the mixed powder in a hot press flat mold, and fill the closed hot press heating chamber with 99.999% high-purity nitrogen gas at a nitrogen inlet flow rate of 1m 3 / h, after charging for 30min, the gas flow rate was changed to 350mL / min, the nitrogen gas state in the closed environment was maintained, the pressurized heating device was turned on, and heat treatment was carried out under the conditions of sintering temperature of 350℃ and pressure of 1GPa to obtain sodium ferrous sulfate positive electrode material.
[0055] Test Case
[0056] The sodium ferrous sulfate positive electrode material prepared in Example 1 and Comparative Examples 1-3 and 5 was made into a button cell to test the electrical performance, wherein the weight ratio of the electrode components was sodium ferrous sulfate positive electrode material: conductive agent (acetylene black): binder (PVDF) = 90:5:5; the negative electrode used a sodium sheet, and the test temperature of the button cell was 25°C. The charge and discharge performance at 0.2C was as follows: Figure 1-4 As shown. Figure 1It can be seen that in the absence of hydraulic pressure, the capacity of Comparative Example 1 is much lower than that of the embodiment. The addition of CNTs makes the raw material particles too dispersed, greatly increasing the atomic diffusion energy barrier of the material during low-temperature sintering, resulting in a lower yield of the target product sodium ferrous sulfate, resulting in a lower capacity. Figure 2 It can be seen that in the case of insufficient pressure, the capacity of Comparative Example 2 is lower than that of the embodiment. Insufficient pressure causes the external pressure to be unable to completely close the raw material particles together, resulting in poor effect. Figure 3 It can be seen that in the case of separate heating and hydraulic treatment, the capacity of Comparative Example 3 is lower than that of the embodiment. The ferrous sulfate containing bound water in the embodiment is in a molten state at high temperature. Under the action of pressure, it is accelerated to combine with the sodium sulfate particles, so that the ferrous sulfate wraps the sodium sulfate particles to the greatest extent, so that the contact surface area between the sodium sulfate and the ferrous sulfate reaches the maximum, thereby improving the yield of the target product. Figure 4 It can be seen that the capacity obtained in the embodiment with added molten salt is higher than that in the comparative example 5 without added molten salt. The micro-liquid environment provided by the low-melting-point molten salt can help improve the tightness between the raw material particles and reduce the atomic diffusion energy barrier of the material during the low-temperature sintering process, thereby increasing the yield of the target product.
[0057] In summary, the preparation method adopted by the present invention utilizes the micro-liquid environment provided by the high-temperature and high-pressure sintering environment and the low-melting-point molten salt to improve the tightness between the raw material particles and reduce the atomic diffusion energy barrier of the material during the low-temperature sintering process. The ferrous sulfate containing bound water is in a molten state at a high temperature. Under the action of the low-melting-point molten salt and pressure, it is accelerated to combine with the sodium sulfate particles, so that the ferrous sulfate wraps the sodium sulfate particles to the greatest extent, so that the contact surface area of the sodium sulfate and the ferrous sulfate is maximized, thereby improving the yield of the target product. The obtained sodium ferrous sulfate positive electrode material is subjected to a buckle test. After detection and analysis, the operating voltage of the half-cell of the sodium ferrous sulfate positive electrode material is 2.0V-4.4V; the 0.2C charging specific capacity reaches 94.66mAh / g.
[0058] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A method for preparing a sodium ferrous sulfate positive electrode material, characterized in that: The following steps are involved: S1. Fully crushing and uniformly mixing ferrous sulfate, sodium sulfate, carbon-based coating material and molten salt to obtain a mixed powder; the melting point of the molten salt is below the heat treatment temperature, and the boiling point is above the heat treatment temperature; S2. Under a protective atmosphere, heat-treating the mixed powder described in S1 to obtain the sodium ferrous sulfate positive electrode material; the heat treatment temperature is 300° C.-400° C., and the pressure is 0.5 GPa-2 GPa.
2. The method for preparing the sodium ferrous sulfate positive electrode material according to claim 1, characterized in that: In S1, the molten salt is selected from sodium nitrate and / or sodium nitrite.
3. The method for preparing the sodium ferrous sulfate positive electrode material according to claim 1, characterized in that: In S1, the carbon-based coating material is selected from one or more of carbon nanotubes, carbon black, graphite, nanographite, graphene and carbon fiber.
4. The method for preparing the sodium ferrous sulfate positive electrode material according to claim 1, characterized in that: In S1, the amounts of ferrous sulfate and sodium sulfate satisfy the chemical formula Na x Fe y (SO4) z , x+2y=2z, 0.5≤x / y≤2.5; the amount of the carbon-based coating material is 1wt%-10wt% of the sodium sulfate, ferrous sulfate and carbon-based coating material; the amount of the molten salt is 1wt%-5wt% of the ferrous sulfate, sodium sulfate, carbon-based coating material and molten salt.
5. A sodium ferrous sulfate positive electrode material prepared by the method according to any one of claims 1 to 4.
6. A sodium ion battery positive electrode, characterized in that: It comprises the sodium ferrous sulfate positive electrode material as claimed in claim 5, a conductive agent and a binder.
7. The sodium ion battery positive electrode according to claim 6, characterized in that The conductive agent is selected from one or more of carbon nanotubes, acetylene black, conductive carbon black, conductive graphite, carbon fiber and graphene; the binder is selected from one or more of polyolefins, fluorine-containing resins, polypropylene resins and rubbers.
8. A sodium ion battery, characterized in that: Comprising the sodium ion battery positive electrode as described in claim 6 or 7.
Citation Information
Cited By
Modified sodium ferrous sulfate battery positive electrode material and preparation and synthesis method thereof
CN121516916A