A vacuum consumable electrode for 300M steel and its refining method
Through the short process of electric furnace smelting, LF refining and VD vacuum degassing, combined with pre-deoxidation, diffusion deoxidation and calcium treatment steps, the problem of impurity control in 300M steel smelting has been solved, and the production of 300M steel materials with high strength and excellent fatigue properties has been achieved. , reducing production costs.
Patent Information
- Application Number
- CN202311704786.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-13
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-12-13
AI Technical Summary
The double vacuum smelting process of 300M steel is high in cost and low in efficiency, and it is difficult to effectively control the impurity elements and gas content in single vacuum smelting, which affects the fatigue and stress corrosion properties of the steel.
The short-process process of electric furnace smelting, LF refining and VD vacuum degassing is adopted. The aluminum and oxygen content in the vacuum consumable electrode is strictly controlled through pre-deoxidation, diffusion deoxidation and calcium treatment steps to reduce the generation of alumina B-type inclusions.
It achieves the high strength, excellent plastic toughness and long low-cycle fatigue life of 300M steel, reduces production costs, and improves the stability and purity of the smelting process.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of alloy steel, and in particular to a vacuum consumable electrode for 300M steel and a refining method thereof. Background Art
[0002] As a low-alloy ultra-high strength steel, 300M steel has become the world's highest strength, best comprehensive performance, most widely used and best reputation steel for landing gear. 300M steel is usually smelted in vacuum to obtain a higher purity, which can significantly improve the plasticity, toughness, fatigue and stress corrosion properties of the steel. At present, the smelting method of 300M steel is a double vacuum process of "vacuum induction + vacuum self-consumption", which has high production costs and low efficiency.
[0003] Therefore, in order to alleviate the current situation of high cost, small scale and tight production capacity of vacuum induction melting, it is urgently needed to develop a short process of "electric furnace + LF refining + VD vacuum treatment".
[0004] The development of a short-process process for 300M steel to replace the mature double vacuum smelting process will inevitably bring about the problem of controlling the impurity content. The main difference between double vacuum melting and single vacuum melting lies in the source of the consumable remelting electrode. In the double vacuum process, the consumable electrode is prepared by vacuum induction, while in the single vacuum process, the electrode comes from the electric arc furnace + refining and casting outside the furnace. Single vacuum melting only undergoes vacuum arc remelting once, which is a strict vacuum melting. However, in order to achieve the purity that meets the standard requirements, especially when civil aircraft have high fracture toughness and fatigue performance requirements for landing gear materials, it is necessary to strictly control the content of impurity elements and gases such as S, P, O, and N in 300M steel to achieve the stability of performance indicators.
[0005] Analyzing the types of fracture inclusions in fatigue fracture of single vacuum 300M steel, most of the cracking sources are alumina inclusions or calcium aluminate inclusions, and the average life and minimum life of high-cycle fatigue of 300M steel show a downward trend with the increase of Al content in steel. Al is a strong deoxidizing element and the most common deoxidizer in steel. The type B alumina inclusions formed by its deoxidation products are the main factors affecting the purity of steel, especially the coarse type B alumina brittle inclusions exceeding 5µm have a great influence on the fatigue properties of steel. Therefore, it is very important to control the end oxygen and end aluminum content for alumina type B inclusions during the smelting process. Summary of the invention
[0006] In order to control the end-point oxygen and end-point aluminum contents during the smelting process and reduce the aluminum oxide B-type inclusions in the finished 300M steel product, the present application provides a vacuum consumable electrode for 300M steel and a refining method thereof.
[0007] The present application provides a refining method for a vacuum consumable electrode for 300M steel, which specifically comprises the following steps: electric furnace smelting, LF refining, VD vacuum degassing, and then casting to obtain the vacuum consumable electrode;
[0008] The LF refining includes pre-deoxidation, diffusion deoxidation, and calcium treatment;
[0009] The pre-deoxidation step: when the tapping amount of LF reaches 20-80wt% in the electric furnace, 1.0-1.5kg of aluminum particles / ton of steel are added for pre-deoxidation, and the argon gas flow rate of the ladle bottom blowing during the tapping process is 0.25-0.45NL / min / ton of steel;
[0010] The diffusion deoxidation step: using 0.05-0.15kg / ton of steel aluminum particles for diffusion deoxidation, and the ladle bottom blowing argon gas flow rate is 0.5-1.0NL / min / ton of steel;
[0011] The calcium treatment step includes: feeding calcium wire or adding calcium-containing ferrosilicon alloy to make the T.Ca content in the molten steel be 0.0005-0.0025% to perform calcium treatment to modify the inclusions, and the ladle soft argon blowing flow rate is 0.2-0.45NL / min / ton of steel;
[0012] Calculated by weight percentage, the impurity element content of LF refined steel meets the requirements of Al≤0.01%, S≤0.002%, P≤0.001%, H≤0.0003%, N≤0.0060%, and TO≤0.0035%.
[0013] In the present application, vacuum consumable electrodes are prepared by the above-mentioned refining method. By designing and optimizing the LF refining process, the vacuum consumable electrodes are produced by adopting the process of "pre-deoxidation, diffusion deoxidation, and calcium treatment". The aluminum content and oxygen content in the vacuum consumable electrodes are strictly controlled, the purity of the steel is improved, and then 300M steel bars / forgings are prepared, so that the steel has high strength, excellent plasticity and toughness, and long low-cycle fatigue life.
[0014] In the early stage of steel tapping alloying to LF treatment, the pre-deoxidation slag forming process is carried out first. At this stage, when the steel tapping volume reaches a certain amount, a certain amount of aluminum particles is added, and combined with the ladle bottom argon blowing process, the slag washing process is used to make the molten steel deoxidized more fully, which can shorten the subsequent diffusion deoxidation time and reduce energy loss.
[0015] After the molten steel has completely reached the LF station, a small amount of aluminum particles is added to diffusely deoxidize the molten steel. This stage is combined with a large-flow bottom argon blowing process to make the slag-liquid interface react violently, promote more complete diffusion deoxidation, and at the same time promote the floating removal of large-sized inclusions, thereby reducing the size of inclusions in the vacuum consumable electrode.
[0016] During the calcium treatment process, feeding calcium wire or adding calcium-containing ferrosilicon alloy helps to modify the inclusions, transforming the Al2O3 inclusions in the molten steel into calcium magnesium aluminate inclusions CaO-Al2O3-MgO; this stage is combined with the bottom blowing argon soft blowing process to promote the floating removal of large-sized inclusions, and at the same time protect the steel slag to avoid large-flow bottom blowing argon breaking the top slag layer, resulting in secondary oxidation of the molten steel.
[0017] By precisely controlling the above-mentioned deoxidation process and calcium treatment process, the chemical composition is fine-tuned during the smelting process, the fluctuation range of each element in the alloy composition is narrow, and the refining processing technology of the vacuum consumable electrode has good stability and good organizational uniformity.
[0018] Preferably, in the steel tapping step of LF during electric furnace smelting: eccentric furnace bottom steel tapping is adopted, a slide plate is used for slag blocking operation, and the slag thickness in the ladle is controlled to be less than 3 cm.
[0019] Preferably, in the pre-deoxidation step: when the steel output reaches 40-60wt%, 1.1-1.4kg of aluminum particles are added per ton of steel, and the argon flow rate of the bottom blowing of the ladle is 0.3-0.4NL / min per ton of steel.
[0020] In a specific embodiment, in the pre-deoxidation step, the steel output can be 20wt%, 40wt%, 50wt%, 60wt%, 80wt%, the amount of aluminum particles added can be 1.0kg / ton steel, 1.1kg / ton steel, 1.2kg / ton steel, 1.4kg / ton steel, 1.5kg / ton steel, and the argon gas flow rate of the bottom blowing of the ladle can be 0.25NL / min / ton steel, 0.3NL / min / ton steel, 0.35NL / min / ton steel, 0.4NL / min / ton steel, 0.45NL / min / ton steel.
[0021] Preferably, in the diffusion deoxidation step: the amount of aluminum particles is 0.07-0.12 kg / ton of steel, and the flow rate of argon gas blown from the bottom of the ladle is 0.6-0.9 NL / min / ton of steel.
[0022] In a specific embodiment, in the diffusion deoxidation step: the amount of aluminum particles can be 0.05kg / ton steel, 0.07kg / ton steel, 0.10kg / ton steel, 0.12kg / ton steel, 0.15kg / ton steel, and the argon gas flow rate of the bottom blowing of the ladle can be 0.5NL / min / ton steel, 0.6NL / min / ton steel, 0.75NL / min / ton steel, 0.9NL / min / ton steel, 1.0NL / min / ton steel.
[0023] Preferably, in the calcium treatment step: the T.Ca content in the molten steel is 0.0010-0.0020%, and the ladle soft argon blowing flow rate is 0.3-0.4NL / min / ton of steel.
[0024] In a specific embodiment, in the calcium treatment step: the T.Ca content in the molten steel can be 0.0005%, 0.0010%, 0.0015%, 0.0020%, 0.0025%, and the soft argon blowing flow rate of the ladle can be 0.2NL / min / ton of steel, 0.3NL / min / ton of steel, 0.35NL / min / ton of steel, 0.4NL / min / ton of steel, 0.45NL / min / ton of steel.
[0025] Through experimental analysis, it can be known that the present application further optimizes the process parameters of pre-deoxidation, diffusion deoxidation and calcium treatment to the above range, which can further reduce the aluminum content and oxygen content in the vacuum consumable electrode, thereby improving the purity of the vacuum consumable electrode for 300M steel.
[0026] Preferably, the pre-deoxidation step also includes: adding 5.0-10.0 kg / ton of steel of lime and 3.0-5.0 kg / ton of steel of high basicity and low melting point refined slag, wherein the high basicity and low melting point refined slag consists of the following components in weight percentage: 5-10% MgO, 5-10% SiO2, 5% CaF2, and the rest are CaO and Al2O3, and the CaO / Al2O3 ratio is 2.0-3.0.
[0027] Preferably, the LF refining also includes: performing a slag removal treatment, adding 0.3-0.5kg / ton of steel quartz and 1.0-2.0kg / ton of steel lime to adjust the slag composition after slag removal to produce high basicity refined white slag, and the white slag refining period is 15-30min; the high basicity refined white slag is composed of the following components in weight percentage: CaO 55-60%, SiO215-20%, Al2O310-15%, MgO15-20%; the tapping temperature is 1650-1720℃, and slag blocking balls are used for slag blocking treatment during the tapping process.
[0028] Preferably, the VD vacuum degassing step includes: the working vacuum degree is ≤67Pa, the bottom blowing argon flow rate in the pre-vacuum stage is 0.2-0.4NL / min / ton of steel, the bottom blowing argon flow rate after entering the vacuum is 0.8-1.0NL / min / ton of steel, and the vacuum treatment time is 20-30min; the steel tapping temperature is 1550-1600℃, and slag blocking balls are used for slag blocking during the steel tapping process; in terms of weight percentage, the impurity element content of the steel tapping satisfies Al≤0.01%, S≤0.001%, P≤0.001%, H≤0.0001%, N≤0.0040%, and TO≤0.0020%.
[0029] In a second aspect, the present application provides a vacuum consumable electrode for 300M steel, which is prepared using the above-mentioned refining method of the vacuum consumable electrode for 300M steel.
[0030] Preferably, the vacuum consumable electrode for 300M steel has the following elemental composition, measured by weight percentage: C 0.39-0.44%, Mn 0.90-1.40%, Si 1.50-1.80%, Cr 0.70-0.95%, Ni 1.65-2.00%, Mo 0.35-0.50%, V 0.05-0.10%, Ca 0.0005-0.0030%, Al≤0.01%, S≤0.001%, P≤0.001%, H≤0.0001%, N≤0.0040%, TO≤0.0020%, and the balance is Fe.
[0031] In a third aspect, the present application provides a 300M steel obtained by vacuum consumable remelting using the above-mentioned vacuum consumable electrode.
[0032] Compared with the traditional double vacuum process of vacuum induction + vacuum consumable remelting, the vacuum consumable electrode produced by the present application is used as the raw material, and an optimized vacuum consumable remelting process is adopted to prepare 300M steel. This can greatly reduce the process pressure of vacuum smelting and has a fast production cycle, thereby significantly reducing production costs.
[0033] In summary, the technical solution of this application has the following effects:
[0034] The present application optimizes the design of the LF refining process and adopts the process of "pre-deoxidation, diffusion deoxidation, and calcium treatment" to achieve good coordination between the various process parameters to produce a vacuum consumable electrode, strictly control the aluminum content and oxygen content in the vacuum consumable electrode, and precisely control the above-mentioned deoxidation process and calcium treatment process, and fine-tune the chemical composition during the smelting process. The fluctuation range of each element in the alloy composition is narrow, and the refining processing technology of the vacuum consumable electrode is stable and the organizational uniformity is good.
[0035] By using the vacuum consumable electrode obtained by the technical solution provided in this application to prepare 300M steel material, the purity of the steel can be improved, and the steel can obtain high strength, excellent plasticity and toughness, and ultra-long fatigue life. DETAILED DESCRIPTION
[0036] The present application is further described in detail below in conjunction with examples, comparative examples and performance testing experiments. These examples should not be construed as limiting the scope of protection claimed in the present application. Example
[0037] Examples 1-3
[0038] Examples 1-3 respectively provide a method for refining a vacuum consumable electrode for 300M steel.
[0039] The difference between the above embodiments is that the process parameters in the preparation method of the vacuum consumable electrode are different and the element components of the produced electrode are different, as shown in Table 1.
[0040] The specific steps of the method for preparing the vacuum consumable electrode in the above embodiment are:
[0041] (1) Electric furnace smelting
[0042] Ingredients: Use 20-45t of scrap steel, 6-20t of pig iron, 6-20t of ferrovanadium, ferrosilicon, nickel plate, ferrochrome, manganese metal, ferromolybdenum and other raw materials (total amount of 55-60 tons) for electric furnace smelting and fine-tuning of alloy composition;
[0043] Melting: Initially, 20 kg of lime is added per ton of steel to make slag and remove phosphorus, and the bottom blowing oxygen flow rate is 30 Nm 3 / h / ton steel, side blowing oxygen flow rate 800NL / min / ton steel, limestone injection flow rate 100kg / min, foam slag submerged arc smelting;
[0044] At the end of oxidation, slag is removed to prevent phosphorus reversion, and eccentric bottom tapping is adopted;
[0045] Tapping of primary molten steel in electric furnace: control P≤0.0015%, tapping temperature 1620-1720℃.
[0046] (2) LF refining
[0047] (2.1) Steel alloying to LF treatment position pre-deoxidation slag forming process:
[0048] LF treatment preparation period: The end point of electric furnace smelting and the temperature of molten steel at tapping are 1620-1720℃. The flow rate of argon gas at the bottom of the ladle during tapping is controlled at 0.25-0.45NL / min / ton of steel. When the tapping amount is 20-80t, 1.0-1.5kg of aluminum particles / ton of steel are added for pre-deoxidation.
[0049] In the later stage of steelmaking, high-quality lime 5.0-10.0kg / ton steel and high-basicity low-melting-point refined slag (high-basicity low-melting-point refined slag consists of the following weight percentage components: MgO 5-10%, SiO25-10%, CaF25%, the rest is CaO and Al2O3, and the CaO / Al2O3 ratio is 2.0-3.0) 3.0-5.0kg / ton steel are added; the refined slag must be completely liquid at the refining temperature to reduce the viscosity of the refined slag and promote the slag-metal interface reaction;
[0050] The eccentric furnace bottom is used for tapping, and the slag blocking operation is to use a slide plate to control the slag to prevent the oxidized slag from flowing into the ladle, ensuring slag-free tapping and controlling the slag thickness in the ladle to less than 3cm.
[0051] (2.2) Diffusion deoxidation process in LF treatment:
[0052] After the primary molten steel arrives at the station, the molten steel is diffused and deoxidized first, and then soft-blown and stirred to promote the removal of large-sized inclusions and reduce the size of inclusions in 300M steel. The specific steps are:
[0053] When the molten steel reaches the LF temperature of 1580-1650℃, lime is added to make white slag for desulfurization, and the composition is controlled to be CaO / SiO2=3.0. Electrode heating is used to prevent surface crusting.
[0054] In the early stage of LF treatment, the flow rate of argon gas at the bottom of the ladle is controlled to be 0.5-1.0NL / min / ton of steel, and the top is covered with refined slag; 0.05-0.15kg of aluminum particles are added / ton of steel for diffusion deoxidation;
[0055] In the middle stage of LF treatment, a slag removal treatment is carried out. After slag removal, 0.3-0.5kg / ton of quartz and 1.0-2.0kg / ton of lime are added to adjust the slag composition to produce high-basicity refined white slag. The white slag refining period is 15-30min; the high-basicity refined white slag is composed of the following components in weight percentage: CaO 55-60%, SiO215-20%, Al2O310-15%, MgO 15-20%. Under a strong reducing atmosphere, the high-basicity slag can achieve further diffusion desulfurization, deoxidation and terminal aluminum content control.
[0056] (2.3) Calcium treatment process in LF treatment:
[0057] In the middle and late stages of LF treatment, calcium treatment is performed by feeding calcium wire or adding calcium-containing ferrosilicon alloy (calcium content is above 0.1%), which is helpful for inclusion modification; the amount of calcium wire added is to control the T.Ca weight content in the steel to 0.0005-0.0025%, and the inclusions in the steel are modified to CaO-Al2O3-MgO; the ladle soft blowing argon flow rate is 0.2-0.45NL / min / ton steel, and the soft blowing time is 10-15min;
[0058] After refining for 10 minutes, samples are taken to measure the composition. According to the composition results, ferrosilicon, ferromanganese, ferronickel, etc. are added in sequence to adjust the composition of the molten steel; the argon gas flow rate of the ladle bottom blowing is 0.2-0.45NL / min / ton of steel, and the soft blowing time is 15 minutes; the tapping temperature is 1650-1720℃, and slag balls are used for slag treatment during the tapping process; according to the weight percentage, the impurity element content of the tapping steel meets Al≤0.01%, S≤0.002%, P≤0.001%, H≤0.0003%, N≤0.0060%, and TO≤0.0035%.
[0059] (3) VD vacuum degassing treatment
[0060] The main metallurgical functions are degassing (N, H) and inclusion removal, which can meet the requirements of 300M steel for the control of the end point aluminum content. The specific steps are:
[0061] The working vacuum degree is ≤67Pa, the bottom blowing argon flow rate is controlled at 0.2-0.4NL / min / ton of steel in the pre-evacuation stage, and the bottom blowing argon flow rate is controlled at 0.8-1.0NL / min / ton of steel after entering the vacuum; the VD vacuum treatment time is 20-30min, the VD steel-out temperature is 1550-1600℃, and slag-blocking balls are used for slag-blocking treatment during the steel-out process; according to the weight percentage, the impurity element content of the steel-out meets Al≤0.01%, S≤0.001%, P≤0.001%, H≤0.0001%, N≤0.0040%, and TO≤0.0020%.
[0062] (4) Casting
[0063] After VD refining, the electrode is cast into an ingot at a casting temperature of 1570±20°C.
[0064] Table 1 Specific process parameters in Examples 1-3 and Comparative Example 1
[0065]
[0066] Embodiment 4-6
[0067] Examples 4-6 each provide a 300M steel.
[0068] The difference between the above embodiments is that the vacuum consumable electrodes used for producing 300M steel are derived from embodiments 1-3 respectively.
[0069] The preparation method of 300M steel in the above embodiment specifically includes the following steps:
[0070] The electrodes prepared in Examples 1-3 are sequentially subjected to vacuum consumable remelting, forging, and heat treatment processes to obtain 300M steel products; wherein the specific process parameters are:
[0071] The process parameters of vacuum consumable remelting are: vacuum degree ≤ 0.4Pa, melting rate 6.5kg / min, time 48h;
[0072] The forging process parameters are: holding temperature 1080±20℃, forging after four piers and four draws;
[0073] The process parameters of heat treatment are: quenching at 880±10℃ and tempering at 220±10℃. Comparative Example Comparative Example 1
[0074] This comparative example provides a method for refining a vacuum consumable electrode.
[0075] The difference between this comparative example and Example 2 is that the process parameters in the refining method are specifically shown in Table 1. Comparative Example 2
[0076] This comparative example provides a 300M steel.
[0077] The difference between this comparative example and Example 5 is that the vacuum consumable electrode used to produce 300M steel comes from Comparative Example 1.
[0078] The preparation method of 300M steel in this comparative example is the same as that in Example 5.
[0079] Performance testing
[0080] The chemical composition analysis, mechanical properties, inclusion rating and fatigue performance of the 300M steel products in Examples 4-6 and Comparative Example 2 were tested.
[0081] Determination method and test results: as shown in Table 2.
[0082] Table 2 Chemical composition analysis and performance test results of 300M steel products in Examples 4-6 and Comparative Example 2
[0083]
[0084] Combined with the test results in Table 2, it can be seen that the present application provides a vacuum consumable electrode as a raw material for producing 300M steel. The present application designs and optimizes the LF refining process, adopts the process of "pre-deoxidation, diffusion deoxidation, and calcium treatment", produces a vacuum consumable electrode, strictly controls the aluminum content and oxygen content in the vacuum consumable electrode, improves the purity of the steel, and then prepares 300M steel bars / forgings, so that the steel has high strength, excellent plasticity and toughness, and long low-cycle fatigue life.
[0085] In the process of preparing the vacuum consumable electrode of Comparative Example 1, no pre-deoxidation was carried out when the electric furnace was smelted to the steel tapping of the LF treatment position, and in the subsequent deoxidation process, the process parameters of the argon blowing process, the amount of aluminum added, and the calcium treatment were not designed reasonably, resulting in the aluminum content of the vacuum consumable electrode being 0.072% and the oxygen content being 0.035%, that is, the content of impurity elements in the vacuum consumable electrode was relatively high, and the fatigue performance of the prepared 300M steel bars / forgings was poor.
[0086] By comparing the test results of Examples 1-3, the present application further controls the process parameters of pre-deoxidation as follows: when the steel output reaches 40-60wt%, 1.1-1.4kg of aluminum particles are added per ton of steel, and the argon flow rate of the ladle bottom blowing is 0.3-0.4NL / min / ton of steel. The process parameters of diffusion deoxidation are controlled as follows: the amount of aluminum particles is 0.07-0.12kg / ton of steel, the argon flow rate of the ladle bottom blowing is 0.6-0.9NL / min / ton of steel, and the process parameters of the calcium treatment step are controlled as follows: the T.Ca content in the molten steel is 0.0010-0.0020%, and the ladle soft blowing argon flow rate is 0.3-0.4NL / min / ton of steel, which can further reduce the aluminum content and oxygen content in the vacuum consumable electrode, thereby improving the purity and fatigue performance of the vacuum consumable electrode for 300M steel.
[0087] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A method for refining a vacuum consumable electrode for 300M steel, characterized in that: The specific steps include: Electric furnace smelting, LF refining, VD vacuum degassing, and then casting to obtain the vacuum consumable electrode; The LF refining includes pre-deoxidation, diffusion deoxidation, and calcium treatment; The pre-deoxidation step: when the tapping amount of LF reaches 20-80wt% in the electric furnace, 1.0-1.5kg of aluminum particles / ton of steel are added for pre-deoxidation, and the argon gas flow rate of the ladle bottom blowing during the tapping process is 0.25-0.45NL / min / ton of steel; The diffusion deoxidation step: using 0.05-0.15kg / ton of steel aluminum particles for diffusion deoxidation, and the ladle bottom blowing argon gas flow rate is 0.5-1.0NL / min / ton of steel; The calcium treatment step includes: feeding calcium wire or adding calcium-containing ferrosilicon alloy to make the T.Ca content in the molten steel be 0.0005-0.0025% to perform calcium treatment to modify the inclusions, and the ladle soft argon blowing flow rate is 0.2-0.45NL / min / ton of steel; According to the percentage by weight, the impurity element content of LF refined steel meets the requirements of Al≤0.01%, S≤0.002%, P≤0.001%, H≤0.0003%, N≤0.0060%, TO≤0.0035%; The pre-deoxidation step further comprises: adding 5.0-10.0 kg lime / ton steel and 3.0-5.0 kg high basicity low melting point refined slag / ton steel, wherein the high basicity low melting point refined slag is composed of the following components in weight percentage: 5-10% MgO, 5-10% SiO2, 5% CaF2, and the rest is CaO and Al2O3, and the CaO / Al2O3 ratio is 2.0-3.0; The LF refining also includes: performing a slag removal treatment, adding quartz 0.3-0.5kg / ton steel and lime 1.0-2.0kg / ton steel to adjust the slag system composition after slag removal, and producing high basicity refined white slag, and the white slag refining period is 15-30min; the high basicity refined white slag is composed of the following weight percentage components: CaO 55-60%, SiO2 15-20%, Al2O3 10-15%, MgO 15-20%; the steel tapping temperature is 1650-1720°C, and the steel tapping process uses slag blocking balls for slag blocking treatment; The VD vacuum degassing step includes: a working vacuum degree of ≤67Pa, a bottom blowing argon flow rate of 0.2-0.4NL / min / ton of steel in the pre-evacuation stage, a bottom blowing argon flow rate of 0.8-1.0NL / min / ton of steel after entering the vacuum, and a vacuum treatment time of 20-30min; a steel tapping temperature of 1550-1600°C, and slag blocking treatment using slag blocking balls during the steel tapping process; and in terms of weight percentage, the content of impurity elements in the steel tapping satisfies Al≤0.01%, S≤0.001%, P≤0.001%, H≤0.0001%, N≤0.0040%, and TO≤0.0020%.
2. The refining method of the vacuum consumable electrode for 300M steel according to claim 1, characterized in that: In the steel tapping step of LF from electric furnace smelting, eccentric furnace bottom steel tapping is adopted, a slide plate is used for slag blocking operation, and the slag thickness in the ladle is controlled to be less than 3 cm.
3. The refining method of the vacuum consumable electrode for 300M steel according to claim 1, characterized in that: In the diffusion deoxidation step, the dosage of aluminum particles is 0.07-0.12 kg / ton of steel, and the flow rate of argon gas blown from the bottom of the ladle is 0.6-0.9 NL / min / ton of steel.
4. The refining method of the vacuum consumable electrode for 300M steel according to claim 1, characterized in that: In the calcium treatment step, the T.Ca content in the molten steel is 0.0010-0.0020%, and the ladle soft blowing argon flow rate is 0.3-0.4NL / min / ton of steel.
5. A vacuum consumable electrode for 300M steel, characterized in that: The steel is prepared by the refining method of the 300M steel vacuum consumable electrode as described in any one of claims 1 to 4.
6. The vacuum consumable electrode for 300M steel according to claim 5, characterized in that: Measured in percentage by weight, the element composition of the vacuum consumable electrode is: C 0.39-0.44%, Mn 0.90-1.40%, Si 1.50-1.80%, Cr 0.70-0.95%, Ni 1.65-2.00%, Mo 0.35-0.50%, V 0.05-0.10%, Ca 0.0005-0.0030%, Al≤0.01%, S≤0.001%, P≤0.001%, H≤0.0001%, N≤0.0040%, TO≤0.0020%, and the balance is Fe.
7. A 300M steel, characterized in that: The vacuum consumable electrode according to any one of claims 5 to 6 is obtained by vacuum consumable remelting.