A method for preparing a solar cell, a solar cell and a photovoltaic module
By using IrO2-PbO-BeO system glass material and laser enhancement optimization contact technology, a metal-silicon hybrid structure is formed, which solves the problems of light loss and burn-through caused by excessive thickness of doped polysilicon layer, and achieves efficient passivation of solar cells. and electrical performance improvements.
Patent Information
- Application Number
- CN202311742432.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-12-15
AI Technical Summary
The thickness of the doped polysilicon layer in existing passivated contact solar cells is too thick, resulting in increased light loss, and when the thickness is reduced, burn-through is prone to occur, affecting the passivation effect and electrical performance.
Using the printing paste of IrO2-PbO-BeO system glass material and laser-enhanced optimized contact technology, a metal-silicon hybrid structure is formed, which suppresses the lateral growth of metal microcrystals, reduces damage to the doped polysilicon layer, and maintains the passivation effect.
When the thickness of the doped polysilicon layer becomes thinner, light loss is reduced and good passivation effect is maintained, the electrical performance of the solar cell is improved, and the sintering temperature and corrosion area are reduced.
Smart Images

Figure CN117790622B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to a method for preparing a solar cell, a solar cell and a photovoltaic module. Background Art
[0002] A passivated contact solar cell refers to a cell in which a tunnel oxide layer is prepared on the back side of the cell, and then a doped silicon film is deposited on the tunnel oxide layer. The tunnel oxide layer and the doped silicon film constitute a passivated contact structure.
[0003] Since the doped polysilicon layer will enhance the parasitic absorption of light by the cell, resulting in increased light loss, and the degree of light loss is proportional to the thickness of the doped polysilicon layer, thinning the doped polysilicon layer is beneficial to reducing light loss. However, reducing the thickness of the doped polysilicon layer will easily lead to a decrease in the passivation effect of the cell, and the opening voltage will be affected to a certain extent. In addition, after the thickness of the doped polysilicon layer is reduced, silver paste burn-through is likely to occur during the sintering process, which will affect the contact performance of the material and further reduce the passivation effect of the material, and the electrical performance of the battery will be damaged. Summary of the invention
[0004] In order to solve the above technical problems, the present application discloses a method for preparing a solar cell, a solar cell and a photovoltaic module. The slurry used in the sintering process of the preparation method contains a glass material of IrO2-PbO-BeO system glass. The above slurry is combined with laser enhanced optimized contact technology to form a specific contact structure, namely a metal-silicon hybrid structure. The contact structure can inhibit the lateral growth of metal microcrystals generated by the slurry after reaching the tunneling layer, thereby reducing the damage to the doped polysilicon layer.
[0005] In a first aspect, an embodiment of the present application provides a method for preparing a solar cell, comprising:
[0006] Depositing a tunneling layer on the light-receiving side or the backlight side of the silicon wafer;
[0007] A doped polysilicon layer is prepared on a side of the tunneling layer facing away from the silicon wafer; wherein the thickness of the doped polysilicon layer is 50 nm to 100 nm;
[0008] Depositing a first functional layer on a side of the doped polysilicon layer away from the tunneling layer;
[0009] Printing a paste on a side of the first functional layer away from the doped polysilicon layer; wherein the paste contains a glass material of IrO2-PbO-BeO system glass;
[0010] Sintering the slurry to form a first metal electrode; wherein the first metal electrode penetrates the first functional layer to form an ohmic contact with the doped polysilicon layer;
[0011] The area where the first metal electrode is located is processed using laser enhanced optimized contact technology.
[0012] Optionally, the glass material includes the following raw materials in percentage by mass:
[0013] 20% to 35% IrO2;
[0014] 60% to 70% PbO;
[0015] 5% to 15% BeO.
[0016] Optionally, the slurry includes the following raw materials in percentage by mass:
[0017] 81.5% to 89.0% silver powder;
[0018] 1.0% to 5.0% of glass material, wherein the glass material is glass powder with a D50 particle size of ≤3.5 μm;
[0019] 7.5% to 12.5% organic carrier;
[0020] 1.0% to 2.5% additives.
[0021] Optionally, the step of preparing a doped polysilicon layer on a side of the tunneling layer facing away from the silicon wafer comprises:
[0022] Preparing a plurality of doped amorphous silicon layers stacked in sequence away from the silicon wafer, and preparing a blocking and passivation layer between two of the doped amorphous silicon layers; wherein the doping concentration of the plurality of doped amorphous silicon layers increases in a direction away from the silicon wafer;
[0023] The doped polysilicon layer is obtained by annealing and crystallization at 850° C. to 900° C.
[0024] Optionally, the step of preparing a plurality of doped amorphous silicon layers stacked in sequence away from the silicon wafer, and preparing a barrier and passivation layer between two of the doped amorphous silicon layers, comprises:
[0025] SiH4 and PH3 with a flow rate of Q1 are introduced for a reaction time of t1 to obtain the first doped amorphous silicon layer;
[0026] SiH4 and PH3 with a flow rate of Q2 are introduced for a reaction time of t2 to obtain the second doped amorphous silicon layer;
[0027] Passing an oxygen source to obtain the blocking and passivation layers made of silicon oxide;
[0028] SiH4 and PH3 with a flow rate of Q3 are introduced for a reaction time of t3 to obtain the third doped amorphous silicon layer; wherein t3>t2>t1, Q3>Q2>Q1.
[0029] Optionally, the step of preparing a doped polysilicon layer on a side of the tunneling layer facing away from the silicon wafer comprises:
[0030] Preparing a plurality of doped amorphous silicon layers stacked in sequence away from the silicon wafer, and annealing and crystallizing at 850° C. to 900° C. to obtain the doped polycrystalline silicon layer; wherein the doping concentration of the plurality of doped amorphous silicon layers increases in a direction away from the silicon wafer;
[0031] Or, preparing an intrinsic amorphous silicon layer and a plurality of doped amorphous silicon layers stacked in sequence away from the silicon wafer, and annealing and crystallizing them at 850° C. to 900° C. to obtain the doped polycrystalline silicon layer; wherein the doping concentration of the plurality of doped amorphous silicon layers increases in a direction away from the silicon wafer;
[0032] Alternatively, an intrinsic amorphous silicon layer and a plurality of doped amorphous silicon layers are prepared, which are stacked in sequence away from the silicon wafer, and a blocking and passivation layer is prepared between two of the doped amorphous silicon layers, and the doped polycrystalline silicon layer is obtained by annealing and crystallizing at 850°C to 900°C; wherein the doping concentration of the plurality of doped amorphous silicon layers increases in a direction away from the silicon wafer.
[0033] Optionally, in the step of using laser enhanced optimized contact technology to process the area where the first metal electrode is located, the laser wavelength is 590nm~880nm, the laser frequency is 30Mhz~60Mhz, the laser scanning speed is 60mm / s~190mm / s, and the laser scanning battery cell rate is 0.6 seconds / piece to 3.7 seconds / piece.
[0034] Optionally, the tunneling layer is a silicon oxide layer;
[0035] And / or, the thickness of the tunneling layer is 1.25 nm to 1.45 nm;
[0036] And / or, the sheet resistance of the doped polysilicon layer is 15Ω / sq to 25Ω / sq;
[0037] And / or, the surface doping concentration of the doped polysilicon layer is 5×10 19 .cm -3 ~7×10 20 .cm -3 ;
[0038] And / or, the first functional layer is a silicon nitride layer;
[0039] And / or, the thickness of the first functional layer is 70nm-80nm.
[0040] In a second aspect, an embodiment of the present application provides a solar cell, which is prepared by the method for preparing a solar cell as described in the first aspect; the solar cell comprises:
[0041] A silicon wafer, the silicon wafer having a first surface and a second surface opposite to the first surface, wherein one of the first surface and the second surface is a light-receiving surface and the other is a backlight surface;
[0042] a tunneling layer, wherein the tunneling layer is disposed on the first surface;
[0043] A doped polysilicon layer, wherein the doped polysilicon layer is disposed on a side of the tunneling layer away from the silicon wafer; the thickness of the doped polysilicon layer is 50 nm to 100 nm;
[0044] A first functional layer, the first functional layer being disposed on a side of the doped polysilicon layer away from the tunneling layer; and
[0045] A first metal electrode, wherein the first metal electrode penetrates the first functional layer and forms an ohmic contact with the doped polysilicon layer; a forked metal-silicon hybrid structure is formed at the contact point between the first metal electrode and the doped polysilicon layer.
[0046] Optionally, the solar cell further comprises:
[0047] a doped layer, the doped layer being arranged on the second surface; the doped layer having a first conductivity type, the silicon wafer and the doped polysilicon layer having a second conductivity type, one of the first conductivity types being an N type and the other being a P type;
[0048] a second functional layer, the second functional layer being disposed on a side of the doped layer facing away from the silicon wafer; and
[0049] A second metal electrode is formed to form an ohmic contact with the doping layer after the second metal electrode penetrates the second functional layer.
[0050] Optionally, the doped polysilicon layer includes a barrier and a passivation layer.
[0051] Optionally, the metal-silicon hybrid structure is a silver-silicon hybrid structure;
[0052] And / or, the tunneling layer is a silicon oxide layer;
[0053] And / or, the thickness of the tunneling layer is 1.25 nm to 1.45 nm;
[0054] And / or, the sheet resistance of the doped polysilicon layer is 15Ω / sq to 25Ω / sq;
[0055] And / or, the surface doping concentration of the doped polysilicon layer is 5×10 19 pcs.cm-3~7×10 20 .cm -3 ;
[0056] And / or, the first functional layer is a silicon nitride layer;
[0057] And / or, the thickness of the first functional layer is 70nm to 80nm;
[0058] And / or, the blocking and passivation layer is a silicon oxide layer.
[0059] In a third aspect, an embodiment of the present application provides a photovoltaic module, comprising the solar cell as described in the second aspect.
[0060] Compared with the prior art, the present invention has the following beneficial effects:
[0061] An embodiment of the present application provides a method for preparing a solar cell, by preparing a doped polysilicon layer with a thinner thickness level of 50nm to 100nm, so as to reduce the parasitic absorption of light by the solar cell and thus reduce light loss; at the same time, a first metal electrode is produced by combining a printing paste with a specific glass material and laser enhanced optimization technology, so that a good passivation effect is still maintained when the thickness of the doped polysilicon layer becomes thinner.
[0062] Specifically, the slurry used in the sintering process of the preparation method contains a glass material of the IrO2-PbO-BeO system glass. IrO2 has a low thermal expansion coefficient, which can effectively improve the stability of the glass system structure, alleviate the corrosion of PbO on the first functional layer and the lateral flow of glass to a certain extent, and reduce the corrosion area of the first functional layer after sintering; and BeO has the effect of lowering the glass transition temperature, so that it still has good wettability at a lower sintering temperature and can effectively etch the first functional layer.
[0063] Furthermore, the preparation method adopts laser enhanced optimized contact technology in combination with a low-corrosion slurry and a reduced sintering temperature to reduce the damage to the thin doped polysilicon layer and the tunneling layer during the sintering process, thereby protecting the excellent passivation effect of the doped polysilicon layer and the tunneling layer; and on this basis, the laser enhanced optimized contact technology forms a specific contact structure, namely a metal-silicon hybrid structure, which can inhibit the lateral growth of metal microcrystals generated by the slurry after reaching the tunneling layer, reduce the damage to the doped polysilicon layer, and is beneficial to maintaining the passivation effect of the doped polysilicon layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0065] Figure 1 is a schematic diagram of the structure of a solar cell according to an embodiment of the present application;
[0066] Figure 2 is a method flow chart of a method for preparing a solar cell in Example 1;
[0067] Figure 3 This is a partial SEM image of the solar cell of Example 1.
[0068] Description of Figure Numbers:
[0069] 100, solar cell; 110, silicon wafer; 120, tunneling layer; 130, doped polysilicon layer; 131, blocking and passivation layer; 140, first functional layer; 150, first metal electrode; 151, metal-silicon hybrid structure; 160, doping layer; 170, second functional layer; 180, second metal electrode. DETAILED DESCRIPTION
[0070] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0071] The thickness of the doped polysilicon layer of the passivated contact solar cell in the related art is relatively thick, ranging from 160nm to 200nm. However, the doped polysilicon layer of the above thickness will cause the cell to have strong parasitic absorption of light and large light loss. In addition, every 10nm increase in the thickness of the doped polysilicon layer can cause a loss of 10mA short-circuit current. Depositing a doped polysilicon layer of the above thickness obviously requires the introduction of more reaction gases and a longer reaction time, resulting in high manufacturing costs for solar cells. Therefore, in order to achieve cost reduction and efficiency improvement of the battery, it is necessary to reduce the thickness of the doped polysilicon layer.
[0072] However, reducing the thickness of the doped polysilicon layer will lead to a series of problems, as follows: the solar cell forms the first metal electrode after sintering the slurry. During the slurry sintering process, the first functional layer covering the doped polysilicon layer is first burned through, and then after reaching the doped polysilicon layer, it continues to burn through a certain depth so that the first metal electrode forms an ohmic contact with the doped polysilicon layer. If the thickness of the doped polysilicon layer is too thin, the doped polysilicon layer will be burned through during the sintering process, which will affect the contact performance and further reduce the passivation effect, and the electrical performance of the solar cell will be damaged.
[0073] In the related art, the burn-through phenomenon is reduced by lowering the sintering temperature. However, simply lowering the sintering temperature may result in the silver paste on the back side being unable to fully etch through the silicon nitride layer, thereby reducing its contact performance with the doped polysilicon layer, increasing the series resistance of the battery, and reducing the electrical performance.
[0074] On the other hand, due to the presence of free electrons in the doped polysilicon layer, the metal microcrystals formed during the sintering process tend to grow laterally after reaching the tunneling layer, that is, grow along the plane direction on the plane where the doped polysilicon layer is located, thereby destroying the doped polysilicon layer, resulting in an increase in the dark saturation current density (J0, metal) and contact resistance. The related art has not studied how to suppress the lateral growth of metal crystals.
[0075] Based on the above analysis, the present application provides a method for preparing solar cells, wherein the slurry used in the sintering process of the preparation method comprises a glass material of IrO2-PbO-BeO system glass, and the slurry has the characteristics of low glass transition temperature, good wettability and low corrosion area, and can be sintered at a lower sintering temperature, and effectively etch the first functional layer, and the corrosion area of the first functional layer is smaller. Furthermore, the above slurry is combined with laser enhanced optimized contact technology to form a specific contact structure, namely a metal-silicon hybrid structure, which can inhibit the lateral growth of metal microcrystals generated by the slurry after reaching the tunneling layer, reduce the damage to the doped polysilicon layer, and is conducive to maintaining the passivation effect of the doped polysilicon layer.
[0076] The technical solution of the present invention will be described below in conjunction with embodiments and drawings.
[0077] In a first aspect, an embodiment of the present application provides a method for preparing a solar cell, comprising:
[0078] Depositing a tunneling layer on the light-receiving side or the backlight side of the silicon wafer;
[0079] A doped polysilicon layer is prepared on the side of the tunneling layer facing away from the silicon wafer; wherein the thickness of the doped polysilicon layer is 50nm to 100nm;
[0080] Depositing a first functional layer on a side of the doped polysilicon layer away from the tunneling layer;
[0081] Printing a paste on a side of the first functional layer away from the doped polysilicon layer; wherein the paste contains a glass material of IrO2-PbO-BeO system glass;
[0082] Sintering the slurry to form a first metal electrode; wherein the first metal electrode penetrates the first functional layer to form an ohmic contact with the doped polysilicon layer;
[0083] The area where the first metal electrode is located is processed using laser enhanced contact optimization technology.
[0084] The thickness of the doped polysilicon layer 130 prepared by the preparation method of the solar cell is only 50nm to 100nm, and the doped polysilicon layer 130 and the tunneling layer 120 constitute a passivation contact structure. The inventors have found that when the thickness of the doped polysilicon layer 130 is greater than 50nm, the solar cell 100 can have a better passivation effect, indicating that the thinner doped polysilicon layer 130 in the present application does not have a significant loss of passivation effect. By preparing a thinner doped polysilicon layer 130, the parasitic absorption of light by the solar cell 100 is reduced, thereby reducing light loss.
[0085] The first functional layer 140 is generally a passivation layer, an anti-reflection layer, or a passivation and anti-reflection layer. Specifically, during the sintering process of the slurry, as the temperature increases, the glass material in the slurry begins to soften and flow, contacts the first functional layer and corrodes the first functional layer, and the metal exists in the glass material in the form of metal ions. The above metal specifically refers to the metal material used as a conductor in the slurry, such as silver. In the cooling stage, the above metal is deposited in the doped polysilicon layer 130 to form metal crystallites, thereby forming the first metal electrode 150. By laser processing the area where the first metal electrode 150 is located, the temperature at the laser irradiation point increases, the metal crystallites will continue to grow, the laser induces the metal crystallites and silicon to diffuse with each other, and after cooling, a forked metal-silicon hybrid structure is formed. The forked metal-silicon hybrid structure can increase the contact area between the first metal electrode 150 and the doped polysilicon layer 130, and the resistance of the ohmic contact decreases with the increase of the contact area, so the metal-silicon hybrid structure can improve the ohmic contact.
[0086] In order to avoid a series of problems in the sintering process of the thin doped polysilicon layer 130, firstly, the slurry used in the sintering process of the preparation method contains a glass material of the IrO2-PbO-BeO system glass. IrO2 has a low thermal expansion coefficient. 4+ The outermost electron structure of Ir has more lone pairs and empty orbitals, which makes it have greater polarization. 4+ With Pb 2+ They have similar electron layer structures and are easily polarized. Since charges of the same kind repel each other, Ir 4+ With Pb2+ After polarization, the positive charge can be effectively shielded. The positive charge here refers to the silver ions formed by the sintering of the slurry, which promotes the uniform distribution of the silver ions in the contact area and improves the contact performance of the area. In addition, the addition of IrO2 can alleviate the corrosion of PbO on the first functional layer and the lateral flow of the glass to a certain extent, reduce the corrosion area of the first functional layer 140 after sintering, and effectively improve the structural stability of the glass system.
[0087] The Be produced by BeO 2+ The radius is small and stable enough, and the probability of entering the IrO2-PbO system and reacting with the substances in the system is extremely small, that is, BeO mainly plays a filling role. BeO has the effect of lowering the glass transition temperature, making the glass transition temperature of the slurry drop to 360℃~370℃, so that it still has good wettability at a lower sintering temperature and can effectively etch the first functional layer.
[0088] In general, the slurry used to make the first metal electrode 150 can be sintered at a lower sintering temperature. Exemplarily, the sintering temperature is 650°C to 720°C. Since the probability of the slurry burn-through is positively correlated with the sintering temperature, that is, the probability of the slurry burn-through is lower, reducing the occurrence of the doped polysilicon layer burn-through phenomenon. Even if low-temperature sintering is adopted, the slurry can still fully etch through the first functional layer, and the corrosion area is small, and the damage to the first functional layer 140 and the doped polysilicon layer 130 is smaller. In addition, even if low-temperature sintering cannot form good contact during the sintering process, the present application can still process the area where the first metal electrode 150 is located through laser enhanced optimized contact technology, thereby forming a metal-silicon hybrid structure that can improve contact.
[0089] Finally, the preparation method adopts laser enhanced optimized contact technology and the above slurry and reduced sintering temperature to reduce the damage to the thin doped polysilicon layer 130 and the tunneling layer 120 during the sintering process, and protect the excellent passivation effect of the doped polysilicon layer 130 and the tunneling layer 120. Different from the metal grains formed by the current slurry sintering method, which form a large contact area with the tunneling layer after reaching the tunneling layer, the above bifurcated metal-silicon hybrid structure has a very small contact area with the tunneling layer after reaching the tunneling layer. This is because the bifurcated metal-silicon hybrid structure is of submicron size level, and the term "submicron size level" refers to 0.1μm to 1μm. Therefore, the metal-silicon hybrid structure can inhibit the lateral growth of metal crystallites generated by the slurry after reaching the tunneling layer 120, reduce the damage to the doped polysilicon layer 130, and is conducive to maintaining the passivation effect of the doped polysilicon layer 130.
[0090] Furthermore, the glass material includes the following raw materials in percentage by mass:
[0091] 20% to 35% IrO2;
[0092] 60% to 70% PbO;
[0093] 5% to 15% BeO.
[0094] The PbO in the glass material is used to give the glass powder the ability to corrode the first functional layer. If the mass percentage of PbO is less than 60%, it is easy to cause the corrosion ability to be too small, so that the corrosion ability of the glass material is weak, the first functional layer cannot be penetrated, and then an effective ohmic contact cannot be formed. If the mass percentage of PbO is greater than 70%, the corrosion ability is too strong, and it will continue to damage the silicon wafer after corroding the first functional layer. In addition, if the mass percentage of PbO is too large, the mass percentage of the other two components IrO2 and BeO will be too small, making it difficult to effectively reduce the glass transition temperature and reduce the corrosion area after sintering. If the mass percentage of IrO2 is less than 20%, it will cause uneven distribution of silver ions in the contact area, resulting in poor contact performance of the battery cell. If the mass percentage of IrO2 is greater than 35%, the mass percentage of PbO or BeO will be too small, which will cause phenomena such as insufficient corrosion ability and excessively high glass transition temperature. If the mass percentage of BeO is less than 5%, the glass transition temperature of the slurry cannot be effectively reduced, and the corrosion effect on the first functional layer is not ideal. If the mass percentage of BeO is greater than 15%, the mass percentage of PbO or IrO2 will be too small, which will lead to phenomena such as insufficient corrosion ability, poor lateral flow improvement effect, and a large corrosion area.
[0095] Further, the slurry includes the following raw materials by mass percentage:
[0096] 81.5% to 89.0% silver powder;
[0097] 1.0% to 5.0% of glass material, wherein the glass material is glass powder with a D50 particle size of ≤3.5 μm;
[0098] 7.5% to 12.5% organic carrier;
[0099] 1.0% to 2.5% additives.
[0100] The organic carrier includes resin, organic solvent and additive. The resin can be one or both of pine alcohol and dodecanol, the organic solvent can be one or both of epoxy resin and cellulose resin, and the additive can be one or both of polyether, polyamide and diethylene glycol. The additive can be functional additives such as thickener, surfactant and coupling agent.
[0101] In the related art, silver-aluminum slurry is generally used to make the first metal electrode, and its metal components include silver powder and aluminum powder. The aluminum-containing slurry can form silver-aluminum spikes to improve ohmic contact, but it will also increase the carrier recombination rate at the contact interface between the first metal electrode and the doped layer, resulting in a decrease in the opening voltage of the solar cell and an increase in contact resistance. In order to make the first metal electrode form a good ohmic contact with the silicon wafer, a high-temperature sintering method is often used to embed the first metal electrode into the doped layer on the surface of the silicon wafer. In addition, the silver-aluminum alloy deposited on the surface of the silicon wafer grows downward as the temperature rises to form silver-aluminum spikes. However, the higher sintering temperature is likely to cause a certain degree of damage to the surface of the silicon wafer, aggravating the recombination rate of carriers at the interface, and reducing the opening voltage and efficiency of the material.
[0102] In contrast, the present application improves the ohmic contact by forming a silver-silicon hybrid structure without forming silver-aluminum spikes, and thus no longer requires high-temperature sintering to grow and generate silver-aluminum spikes. The first functional layer is burned through by low-temperature sintering, which causes less damage to the silicon wafer, thereby reducing the recombination rate, and the opening voltage and efficiency are increased to a certain extent, as follows:
[0103] The present application uses laser enhanced optimized contact technology to generate a heating area at the contact interface between the first metal electrode and the doped polysilicon layer to form a bifurcated silver-silicon hybrid structure. The bifurcated silver-silicon hybrid structure can increase the contact area between the metal and the semiconductor, and the resistance of the ohmic contact decreases as the contact area increases. Therefore, the silver-silicon hybrid structure can improve the ohmic contact and replace the silver-aluminum spikes used to improve the ohmic contact. The silver-silicon hybrid structure will not accelerate the carrier recombination rate on the surface of the material while reducing the contact resistance, and the solar cell opening voltage and efficiency are both increased to a certain extent.
[0104] Furthermore, the present application no longer requires high-temperature sintering to grow silver-aluminum spikes, and no aluminum powder component needs to be added to the slurry to form silver-aluminum spikes, so that BeO can be added to the slurry to lower the glass transition temperature to lower the sintering temperature. The addition of BeO enables the slurry to effectively burn through the first functional layer.
[0105] Optionally, the step of preparing a doped polysilicon layer on a side of the tunneling layer facing away from the silicon wafer includes:
[0106] A plurality of doped amorphous silicon layers are prepared and stacked in sequence away from the silicon wafer, and a blocking and passivation layer is prepared between two of the doped amorphous silicon layers; wherein the doping concentration of the plurality of doped amorphous silicon layers increases in a direction away from the silicon wafer;
[0107] The doped polysilicon layer is obtained by annealing and crystallization at 850°C to 900°C.
[0108] As can be seen from the above, the doped polysilicon layer obtained by the preparation method includes a plurality of doped amorphous silicon layers stacked in sequence away from the silicon wafer. The doping concentration of the plurality of doped amorphous silicon layers increases in the direction away from the silicon wafer, that is, the doping concentration of the doped amorphous silicon layer closer to the silicon wafer is lower, which can effectively reduce the concentration of doping elements reaching the surface of the silicon wafer, and the lower the concentration of doping elements on the surface of the silicon wafer, the lower the probability of the occurrence of the Auger recombination phenomenon, thereby improving the passivation performance. In addition, the increase in doping concentration can increase the crystallization rate of the doped polysilicon layer, and the increase in crystallization rate helps to reduce the resistivity of the doped polysilicon layer.
[0109] Furthermore, a blocking and passivation layer is provided between two of the doped amorphous silicon layers. Exemplarily, the doped polycrystalline silicon layer includes a first doped amorphous silicon layer, a second doped amorphous silicon layer, a blocking and passivation layer, and a third doped amorphous silicon layer stacked in sequence away from the silicon wafer. The blocking and passivation layer serves to block the doping elements in the third doped amorphous silicon layer with a higher doping concentration from diffusing toward the silicon wafer, thereby further effectively reducing the concentration of doping elements reaching the surface of the silicon wafer, alleviating the occurrence of Auger recombination, and improving the passivation performance. In addition, the blocking and passivation layer also serves to enhance the passivation effect. Exemplarily, the blocking and passivation layer can be a silicon oxide layer.
[0110] Furthermore, the step of preparing a plurality of doped amorphous silicon layers stacked in sequence away from the silicon wafer, and preparing a barrier and passivation layer between two of the doped amorphous silicon layers, comprises:
[0111] SiH4 and PH3 with a flow rate of Q1 are introduced for a reaction time of t1 to obtain a first doped amorphous silicon layer;
[0112] SiH4 and PH3 with a flow rate of Q2 are introduced for a reaction time of t2 to obtain a second doped amorphous silicon layer;
[0113] An oxygen source is introduced to obtain a barrier and passivation layer made of silicon oxide;
[0114] SiH4 and PH3 with a flow rate of Q3 are introduced for a reaction time of t3 to obtain a third doped amorphous silicon layer; wherein t3>t2>t1, Q3>Q2>Q1.
[0115] In the preparation process of the doped polysilicon layer of the present application, without introducing a new process, a doped polysilicon layer with a thinner thickness and an increasing doping concentration in a direction away from the silicon wafer can be obtained by simply adjusting the reaction time, PH3 flow rate and annealing temperature.
[0116] Optionally, the step of preparing a doped polysilicon layer on a side of the tunneling layer facing away from the silicon wafer includes:
[0117] A plurality of doped amorphous silicon layers stacked in sequence away from the silicon wafer are prepared, and annealed and crystallized at 850° C. to 900° C. to obtain a doped polycrystalline silicon layer; wherein the doping concentration of the plurality of doped amorphous silicon layers increases in a direction away from the silicon wafer.
[0118] Alternatively, the step of preparing a doped polysilicon layer on a side of the tunneling layer facing away from the silicon wafer comprises:
[0119] An intrinsic amorphous silicon layer and a plurality of doped amorphous silicon layers stacked in sequence away from the silicon wafer are prepared, and annealed and crystallized at 850° C. to 900° C. to obtain a doped polycrystalline silicon layer; wherein the doping concentration of the plurality of doped amorphous silicon layers increases in a direction away from the silicon wafer.
[0120] It can be understood that the intrinsic amorphous silicon layer is located between the tunneling layer and the multiple doped amorphous silicon layers, and plays a role in blocking the diffusion of doped elements toward the silicon wafer.
[0121] Alternatively, the step of preparing a doped polysilicon layer on a side of the tunneling layer facing away from the silicon wafer comprises:
[0122] An intrinsic amorphous silicon layer and a plurality of doped amorphous silicon layers are prepared, which are stacked in sequence away from the silicon wafer, and a blocking and passivation layer is prepared between two of the doped amorphous silicon layers. The doped polycrystalline silicon layer is obtained by annealing and crystallizing at 850°C to 900°C; wherein the doping concentration of the plurality of doped amorphous silicon layers increases in a direction away from the silicon wafer.
[0123] It can be understood that the blocking and passivation layer and the intrinsic amorphous silicon layer cooperate with each other to further block the doped elements in the doped amorphous silicon layer from reaching the surface of the silicon wafer and give the doped polysilicon layer a better passivation effect.
[0124] Optionally, in the step of using laser enhanced optimized contact technology to process the area where the first metal electrode is located, the laser wavelength is 590nm to 880nm, including any value within the wavelength range, such as 590nm, 700nm or 880nm. The frequency of the laser is 30Mhz to 60Mhz, including any value within the frequency range, such as 30Mhz, 50Mhz or 60Mhz. The laser scanning speed is 60mm / s to 190mm / s, including any value within the scanning speed range, such as 60mm / s, 120mm / s or 190mm / s, and the laser scanning battery cell rate is 0.6 seconds / piece to 3.7 seconds / piece, including any value within the rate range, such as 0.6 seconds / piece, 2.0 seconds / piece or 3.7 seconds / piece.
[0125] Optionally, the tunneling layer is a silicon oxide layer;
[0126] and / or, the thickness of the tunneling layer is 1.25 nm to 1.45 nm, including any value within the thickness range, for example, 1.25 nm, 1.30 nm or 1.45 nm;
[0127] And / or, the sheet resistance of the doped polysilicon layer is 15Ω / sq to 25Ω / sq, including any point value within the sheet resistance range, for example, 15Ω / sq, 20Ω / sq or 25Ω / sq;
[0128] and / or, the surface doping concentration of the doped polysilicon layer is 5×10 19 .cm -3 ~7×10 20 .cm -3 Including any point value within the surface doping concentration range, for example, 5×10 19 .cm -3 , 1×10 20 .cm -3 or 7×10 20 .cm -3 ;
[0129] And / or, the first functional layer is a silicon nitride layer;
[0130] And / or, the thickness of the first functional layer is 70 nm to 80 nm, including any value within the thickness range, for example, 70 nm, 75 nm or 80 nm.
[0131] In a second aspect, an embodiment of the present application provides a solar cell, which is prepared by the method for preparing a solar cell as described in the first aspect. Figure 1 As shown, the solar cell 100 includes a silicon wafer 110, a tunneling layer 120, a doped polysilicon layer 130, a first functional layer 140 and a first metal electrode 150. The silicon wafer 110 has a first surface and a second surface opposite to the first surface, one of the first surface and the second surface is a light-receiving surface and the other is a backlight surface. The tunneling layer 120 is arranged on the first surface. The doped polysilicon layer 130 is arranged on the side of the tunneling layer 120 away from the silicon wafer 110; the thickness of the doped polysilicon layer 130 is 50nm to 100nm. The first functional layer 140 is arranged on the side of the doped polysilicon layer 130 away from the tunneling layer 120. The first metal electrode 150 penetrates the first functional layer 140 to form an ohmic contact with the doped polysilicon layer 130; a forked metal-silicon hybrid structure 151 is formed at the contact between the first metal electrode 150 and the doped polysilicon layer 130.
[0132] The thickness of the doped polysilicon layer 130 of the solar cell 100 is only 50nm to 100nm. When the thickness of the doped polysilicon layer 130 is greater than 50nm, the solar cell 100 can have a better passivation effect. In the present application, the thinner doped polysilicon layer 130 does not have a significant loss in passivation effect. By preparing a thinner doped polysilicon layer 130, the parasitic absorption of light by the solar cell 100 is reduced, thereby reducing light loss.
[0133] The forked metal-silicon hybrid structure 151 can increase the contact area between the first metal electrode 150 and the doped polysilicon layer 130, and the resistance of the ohmic contact decreases with the increase of the contact area. Therefore, the metal-silicon hybrid structure can improve the ohmic contact and has the advantage of less composite compared to the silver-aluminum spikes.
[0134] Optionally, the solar cell 100 further includes a doping layer 160, a second functional layer 170 and a second metal electrode 180, wherein the doping layer 160 is disposed on the second surface. The second functional layer 170 is disposed on the side of the doping layer 160 away from the silicon wafer 110, and the second functional layer 170 includes at least one of a passivation layer, an anti-reflection layer, or a passivation and anti-reflection layer, and the second functional layer 170 may be a single-layer structure or a multi-layer structure. The second metal electrode 180 forms an ohmic contact with the doping layer 160 after penetrating the second functional layer 170. The doping layer 160 has a first conductivity type, and the silicon wafer 110 and the doped polysilicon layer 130 have a second conductivity type, wherein one of the first conductivity types is an N type and the other is a P type. Specifically, the doping layer 160 may be a doping layer 160 formed after diffusion, and then forms a PN junction with the silicon wafer 110.
[0135] Optionally, the doped polysilicon layer 130 includes a blocking and passivation layer 131. The blocking and passivation layer 131 blocks the doping elements in the third doped amorphous silicon layer with a higher doping concentration from diffusing toward the silicon wafer 110, thereby further effectively reducing the concentration of the doping elements reaching the surface of the silicon wafer 110, alleviating the occurrence of Auger recombination, and improving the passivation performance.
[0136] Optionally, the metal-silicon hybrid structure 151 is a silver-silicon hybrid structure;
[0137] and / or, the tunneling layer 120 is a silicon oxide layer;
[0138] and / or, the thickness of the tunneling layer 120 is 1.25 nm to 1.45 nm;
[0139] and / or, the sheet resistance of the doped polysilicon layer 130 is 15Ω / sq to 25Ω / sq;
[0140] And / or, the surface doping concentration of the doped polysilicon layer 130 is 5×10 19 .cm -3 ~7×10 20 .cm -3 ;
[0141] and / or, the first functional layer 140 is a silicon nitride layer;
[0142] and / or, the thickness of the first functional layer 140 is 70 nm to 80 nm;
[0143] And / or, the blocking and passivation layer 131 is a silicon oxide layer.
[0144] In a third aspect, an embodiment of the present application provides a photovoltaic module, comprising the solar cell as described in the second aspect.
[0145] The technical solution of the present invention will be described below in conjunction with embodiments and comparative examples.
[0146] Example 1
[0147] like Figure 2 As shown, the preparation method of the solar cell provided in this embodiment comprises the following steps:
[0148] S1. Depositing a tunneling layer on the backlight side of a silicon wafer: A N-type silicon wafer with a light-receiving side that has been textured and boron-expanded is introduced with nitrous oxide for 105 seconds, and a tunneling layer with a thickness of 1.2 nm is formed on the backlight side of the silicon wafer.
[0149] S2. Prepare a doped polysilicon layer on the side of the tunneling layer away from the silicon wafer: introduce PH3 and SiH4, with a PH3 flow rate of 380sccm, a SiH4 flow rate of 2800sccm, and a reaction time of 115s to obtain a first doped amorphous silicon layer; introduce PH3 and SiH4, with a PH3 flow rate of 500sccm, a SiH4 flow rate of 2800sccm, and a reaction time of 245s to obtain a second doped amorphous silicon layer; introduce nitrous oxide with a flow rate of 7500sccm, and a reaction time of 20s to obtain a barrier and passivation layer of silicon oxide material; introduce PH3 and SiH4, with a PH3 flow rate of 700sccm, a SiH4 flow rate of 2800sccm, and a reaction time of 250s to obtain a third doped amorphous silicon layer; anneal and crystallize at 900°C to obtain a doped polysilicon layer.
[0150] S3. Depositing a first functional layer on a side of the doped polysilicon layer away from the tunneling layer: introducing silane and ammonia to obtain a silicon nitride layer, namely, the first functional layer.
[0151] S4. Printing slurry on the side of the first functional layer away from the doped polysilicon layer: printing slurry on the side of the first functional layer away from the doped polysilicon layer by screen printing, the slurry comprising the following raw materials in percentage by mass: 83% silver powder, 3.5% glass powder, 11.5% organic carrier and 2% additives, wherein the glass powder, i.e., the glass material, is IrO2-PbO-BeO system glass, and based on the total mass of the glass powder as 100%, the content of IrO2 in the glass powder is 28%, the content of PbO is 64%, the content of BeO is 8%, and the D50 particle size of the glass powder is ≤3.5μm.
[0152] S5. Sintering the slurry to form a first metal electrode: sintering at 690° C. for 15 seconds to obtain a first metal electrode.
[0153] S6. Use laser enhanced optimized contact technology to process the area where the first metal electrode is located: Use laser to process the first metal electrode on the backlight surface, the laser wavelength is 550nm, the power is 50Mhz, the laser scanning speed is 100mm / s, and the battery cell scanning rate is 2.9 seconds / cell.
[0154] See also Figure 3 In the SEM image of the solar cell, it can be observed that after step S6, the contact area of the doped polysilicon layer 130 forms a metal-silicon hybrid structure 151, that is, a silver-silicon hybrid structure.
[0155] Example 2
[0156] The difference between this embodiment and embodiment 1 is that the barrier and passivation layers are not fabricated in step S2, which is as follows:
[0157] S2. Prepare a doped polysilicon layer on the side of the tunneling layer away from the silicon wafer: introduce PH3 and SiH4, with a PH3 flow rate of 380sccm, a SiH4 flow rate of 2800sccm, and a reaction time of 115s to obtain a first doped amorphous silicon layer; introduce PH3 and SiH4, with a PH3 flow rate of 500sccm, a SiH4 flow rate of 2800sccm, and a reaction time of 245s to obtain a second doped amorphous silicon layer; introduce PH3 and SiH4, with a PH3 flow rate of 700sccm, a SiH4 flow rate of 2800sccm, and a reaction time of 250s to obtain a third doped amorphous silicon layer; anneal and crystallize at 900°C to obtain a doped polysilicon layer.
[0158] Example 3
[0159] The difference between this embodiment and embodiment 1 is that: in step S2, the production of an intrinsic amorphous silicon layer is added, which is specifically as follows:
[0160] Before forming the first doped amorphous silicon layer, 2800 sccm of SiH4 was introduced with a reaction time of 70 seconds to obtain an intrinsic amorphous silicon layer.
[0161] Example 4
[0162] The difference between this embodiment and embodiment 1 is that the slurry in step S4, based on the total mass of the glass powder being 100%, the IrO2 content in the glass powder used is 10%, the PbO content is 82%, and the BeO content is 8%.
[0163] In step S5, the first metal electrode is obtained by sintering at 760° C. for 20 seconds.
[0164] Example 5
[0165] The difference between this embodiment and embodiment 1 is that the slurry in step S4, based on the total mass of the glass powder being 100%, has an IrO2 content of 28%, a PbO content of 71%, and a BeO content of 1%.
[0166] In step S5, the first metal electrode is obtained by sintering at 775° C. for 20 seconds.
[0167] Example 6
[0168] The difference between this embodiment and embodiment 1 is that the slurry in step S4, based on the total mass of the glass powder being 100%, has an IrO2 content of 40%, a PbO content of 52%, and a BeO content of 8%.
[0169] In step S5, sintering is performed at 750° C. for 20 seconds to obtain a first metal electrode.
[0170] Example 7
[0171] The difference between this embodiment and embodiment 1 is that the slurry in step S4, based on the total mass of the glass powder being 100%, has an IrO2 content of 28%, a PbO content of 52%, and a BeO content of 20% in the glass powder used.
[0172] In step S5, the first metal electrode is obtained by sintering at 650° C. for 15 seconds.
[0173] Comparative Example 1
[0174] The difference between this comparative example and Example 1 is that in step S2, PH3 and SiH4 are introduced, the PH3 flow rate is 760sccm, the SiH4 flow rate is 2850sccm, the reaction time is 1050s, and a doped polysilicon layer with a thickness of 200nm is prepared on the side of the tunneling layer away from the silicon wafer.
[0175] Comparative Example 2
[0176] The difference between this comparative example and Example 1 is that the glass powder of the slurry in step S4 contains only PbO, and the sintering temperature in step S5 is 790°C.
[0177] Comparative Example 3
[0178] The only difference between this comparative example and Example 1 is that the glass powder of the slurry in step S4 contains only PbO and IrO2. Taking the total mass of the glass powder as 100%, the content of PbO in the glass powder is 65%, and the content of IrO2 is 35%. The sintering temperature in step S5 is 775°C.
[0179] Comparative Example 4
[0180] The only difference between this comparative example and Example 1 is that the glass powder of the slurry in step S4 contains only BeO and PbO. Taking the total mass of the glass powder as 100%, the content of PbO in the glass powder is 92%, and the content of BeO is 8%. The sintering temperature in step S5 is 782°C.
[0181] Comparative Example 5
[0182] The only difference between this comparative example and Example 1 is that step S6 is not performed, that is, the laser enhanced contact optimization technology is not used to process the area where the first metal electrode is located.
[0183] The electrical properties of the solar cells prepared in Examples 1-7 and Comparative Examples 1-5 were tested. The test results are shown in Table 1.
[0184] Table 1: Electrical performance test results of solar cells prepared in Examples 1-7 and Comparative Examples 1-5
[0185]
[0186]
[0187] The properties of the slurries of Examples 1, 4, 5, 6, 7 and Comparative Examples 2-4 were tested, and the test results are shown in Table 2.
[0188] Table 2: Performance test results of the slurries of Examples 1, 4, 5, 6, 7 and Comparative Examples 2-4
[0189] Grouping Glass transition temperature(℃) Example 1 365 Example 4 387 Example 5 372 Example 6 379 Example 7 359 Comparative Example 2 405 Comparative Example 3 391 Comparative Example 4 375
[0190] As can be seen from Table 1, the thickness of the doped polysilicon layer of Comparative Example 1 is greater than that of the doped polysilicon layer of Example 1. The reduction in the thickness of the doped polysilicon layer of Example 1 reduces the parasitic absorption of light by the solar cell, reduces light loss, and increases current, further making the conversion efficiency of Example 1 higher than that of Comparative Example 1. On the other hand, the open circuit voltage, fill factor, and minority carrier lifetime of Example 1 are all higher than those of Comparative Example 1, and the use of a thinner doped polysilicon layer thickness in Example 1 does not affect other properties.
[0191] Combining Table 1 and Table 2, it can be seen that the glass powder of Comparative Example 2 contains only PbO, which leads to a high glass transition temperature of up to 405°C. In addition, during the sintering process, the corrosion of PbO on the first functional layer and the lateral flow of glass are more serious, and the passivation performance is reduced. The slurry used in Example 1 contains a glass material of IrO2-PbO-BeO system glass. The addition of IrO2 can alleviate the corrosion of PbO on the first functional layer and the lateral flow of glass to a certain extent, and BeO has the effect of lowering the glass transition temperature, so that it still has good wettability at a lower sintering temperature and can effectively etch the first functional layer. Example 1 using this slurry can be sintered at a lower sintering temperature than Comparative Example 2. After sintering, it can reduce damage to the silicon wafer and the first functional layer, and the corrosion area after sintering is smaller, so that the conversion efficiency, open circuit voltage, fill factor and minority carrier lifetime of Example 1 are all higher than those of Comparative Example 2.
[0192] Although IrO2 is added to the slurry of Comparative Example 3, that is, the glass powder is a glass material of IrO2-PbO system glass, without BeO, its glass transition temperature is still as high as 391°C. BeO is added to Example 1, which has the effect of lowering the glass transition temperature, so that it still has good wettability at a lower sintering temperature and can effectively etch the first functional layer, so that the sintering temperature of Example 1 is 690°C lower than the sintering temperature of Comparative Example 3, 775°C. The lower sintering temperature reduces the damage to the silicon wafer during sintering, so that the conversion efficiency, short-circuit current and fill factor of Example 1 are higher than those of Comparative Example 3.
[0193] In Comparative Example 4, BeO is added to the slurry, which has the effect of lowering the glass transition temperature. However, due to the lack of IrO2, the corrosion of PbO on the first functional layer and the lateral flow of glass are still relatively serious, and the uneven distribution of silver ions in the contact area leads to poor contact performance of the cell. In Example 1, IrO2 is added, and IrO2 has a lower thermal expansion coefficient. 4 + The outermost electron structure of Ir has more lone pairs and empty orbitals, which makes it have greater polarization. 4+ With Pb 2+ They have similar electron layer structures and are easily polarized. Since charges of the same kind repel each other, Ir 4+ With Pb 2+After polarization, it can effectively shield positive charges, where the positive charges refer to the silver ions formed by the sintering of the slurry, which promotes the uniform distribution of silver ions in the contact area and improves the contact performance of the area. The dark saturation current density of Example 1 is lower than that of Comparative Example 4. It is speculated that the addition of IrO2 inhibits the lateral growth of the metal microcrystals formed during the sintering process after reaching the tunneling layer, and the damage to the doped polysilicon layer is smaller, and the dark saturation current density is improved. The smaller the dark saturation current density, the less the recombination, the better the passivation effect, and the higher the open circuit voltage.
[0194] Comparative Example 5 does not use laser enhanced optimized contact technology to process the area where the first metal electrode is located, resulting in poor contact performance. However, Example 1 uses laser enhanced optimized contact technology to generate a heating area at the contact interface between the first metal electrode and the doped polysilicon layer to form a bifurcated silver-silicon hybrid structure. The silver-silicon hybrid structure can improve ohmic contact, reduce contact resistance, and will not accelerate the carrier recombination rate on the material surface, so that the open circuit voltage and conversion efficiency of Example 1 are significantly better than those of Comparative Example 5.
[0195] Example 2 does not provide for the preparation of a blocking and passivation layer, while Example 1 also prepares a blocking and passivation layer in step S2. The blocking and passivation layer serves to block the doping elements in the third doped amorphous silicon layer with a higher doping concentration from diffusing toward the silicon wafer, thereby further effectively reducing the concentration of doping elements reaching the surface of the silicon wafer, alleviating the occurrence of Auger recombination, and improving the passivation performance. The conversion efficiency, open circuit voltage, short circuit current, fill factor and minority carrier lifetime of Example 1 are all higher than those of Example 2.
[0196] Compared with Example 1, Example 3 adds an intrinsic amorphous silicon layer, which further blocks the diffusion of doping elements toward the silicon wafer, thereby further effectively reducing the concentration of doping elements reaching the surface of the silicon wafer and alleviating the occurrence of Auger recombination. It can be seen that the open circuit voltage and minority carrier lifetime of Example 3 are higher than those of Example 1.
[0197] The IrO2 content of Example 4 is lower than that of Example 1. The low IrO2 content leads to uneven distribution of silver ions in the contact area of Example 4, resulting in poor contact performance of the solar cell. However, the conversion efficiency, open circuit voltage, etc. of Example 1 are better than those of Example 4.
[0198] The BeO content of Example 5 is lower than that of Example 1. The low BeO content results in that the glass transition temperature of the slurry cannot be effectively reduced, and the corrosion effect on the first functional layer is not ideal. As can be seen from Table 2, the glass transition temperature of Example 5 is higher than that of Example 1. The sintering process of Example 1 has a better corrosion effect on the first functional layer, so that the contact performance of Example 1 is better, and the conversion efficiency, open circuit voltage and fill factor of Example 1 are all higher than those of Example 5.
[0199] The IrO2 content of the slurry of Example 6 is higher than that of Example 1, so that the PbO in the slurry of Example 6 is lower than that of Example 1. The reduced PbO content leads to insufficient corrosion ability of the slurry, which is not conducive to forming good contact, thereby causing the conversion efficiency, open circuit voltage, short circuit current, fill factor and minority carrier lifetime of Example 6 to be lower than those of Example 1.
[0200] The BeO content of the slurry of Example 7 is higher than that of Example 1, so that the PbO in the slurry of Example 7 is lower than that of Example 1. The reduced PbO content leads to insufficient corrosion ability of the slurry, which is not conducive to forming good contact, thereby causing the conversion efficiency, open circuit voltage, short circuit current, fill factor and minority carrier lifetime of Example 7 to be lower than that of Example 1.
[0201] The above is a detailed introduction to a method for preparing a solar cell, a solar cell and a photovoltaic module disclosed in an embodiment of the present invention. Specific examples are used herein to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method for preparing a solar cell, a solar cell and a photovoltaic module of the present invention and their core ideas. At the same time, for a person skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation modes and application scopes. In summary, the content of this specification should not be understood as a limitation on the present invention.
Claims
1. A method for preparing a solar cell, characterized in that: include: Depositing a tunneling layer on the light-receiving side or the backlight side of the silicon wafer; A doped polysilicon layer is prepared on a side of the tunneling layer facing away from the silicon wafer; wherein the thickness of the doped polysilicon layer is 50 nm to 100 nm; Depositing a first functional layer on a side of the doped polysilicon layer away from the tunneling layer; Printing a paste on a side of the first functional layer away from the doped polysilicon layer; wherein the paste contains a glass material of IrO2-PbO-BeO system glass; Sintering the slurry to form a first metal electrode; wherein the first metal electrode penetrates the first functional layer to form an ohmic contact with the doped polysilicon layer; The area where the first metal electrode is located is processed using laser enhanced optimized contact technology.
2. The method for preparing a solar cell according to claim 1, characterized in that: The glass material includes the following raw materials by mass percentage: 20% to 35% IrO2; 60% to 70% PbO; 5% to 15% BeO.
3. The method for preparing a solar cell according to claim 2, characterized in that: The slurry includes the following raw materials by mass percentage: 81.5% to 89.0% silver powder; 1.0% to 5.0% of glass material, wherein the glass material is glass powder with a D50 particle size of ≤3.5 μm; 7.5% to 12.5% organic carrier; 1.0% to 2.5% additives.
4. The method for preparing a solar cell according to claim 1, characterized in that: The step of preparing a doped polysilicon layer on a side of the tunneling layer facing away from the silicon wafer comprises: Preparing a plurality of doped amorphous silicon layers stacked in sequence away from the silicon wafer, and preparing a blocking and passivation layer between two of the doped amorphous silicon layers; wherein the doping concentration of the plurality of doped amorphous silicon layers increases in a direction away from the silicon wafer; The doped polysilicon layer is obtained by annealing and crystallization at 850° C. to 900° C.
5. The method for preparing a solar cell according to claim 4, characterized in that: The step of preparing a plurality of doped amorphous silicon layers stacked in sequence away from the silicon wafer, and preparing a blocking and passivation layer between two of the doped amorphous silicon layers, comprises: SiH4 and PH3 with a flow rate of Q1 are introduced for a reaction time of t1 to obtain the first doped amorphous silicon layer; SiH4 and PH3 with a flow rate of Q2 are introduced for a reaction time of t2 to obtain the second doped amorphous silicon layer; Passing an oxygen source to obtain the blocking and passivation layers made of silicon oxide; SiH4 and PH3 with a flow rate of Q3 are introduced for a reaction time of t3 to obtain the third doped amorphous silicon layer; wherein t3>t2>t1, Q3>Q2>Q1.
6. The method for preparing a solar cell according to claim 1, characterized in that: The step of preparing a doped polysilicon layer on a side of the tunneling layer facing away from the silicon wafer comprises: Preparing a plurality of doped amorphous silicon layers stacked in sequence away from the silicon wafer, and annealing and crystallizing at 850° C. to 900° C. to obtain the doped polycrystalline silicon layer; wherein the doping concentration of the plurality of doped amorphous silicon layers increases in a direction away from the silicon wafer; Or, preparing an intrinsic amorphous silicon layer and a plurality of doped amorphous silicon layers stacked in sequence away from the silicon wafer, and annealing and crystallizing them at 850° C. to 900° C. to obtain the doped polycrystalline silicon layer; wherein the doping concentration of the plurality of doped amorphous silicon layers increases in a direction away from the silicon wafer; Alternatively, an intrinsic amorphous silicon layer and a plurality of doped amorphous silicon layers are prepared, which are stacked in sequence away from the silicon wafer, and a blocking and passivation layer is prepared between two of the doped amorphous silicon layers, and the doped polycrystalline silicon layer is obtained by annealing and crystallizing at 850°C to 900°C; wherein the doping concentration of the plurality of doped amorphous silicon layers increases in a direction away from the silicon wafer.
7. The method for preparing a solar cell according to any one of claims 1 to 6, characterized in that: In the step of using laser enhanced optimized contact technology to process the area where the first metal electrode is located, the laser wavelength is 590nm~880nm, the laser frequency is 30Mhz~60Mhz, the laser scanning speed is 60mm / s~190mm / s, and the laser scanning battery cell rate is 0.6 seconds / piece to 3.7 seconds / piece.
8. The method for preparing a solar cell according to any one of claims 1 to 6, characterized in that: The tunneling layer is a silicon oxide layer; And / or, the thickness of the tunneling layer is 1.25 nm to 1.45 nm; And / or, the sheet resistance of the doped polysilicon layer is 15Ω / sq to 25Ω / sq; And / or, the surface doping concentration of the doped polysilicon layer is 5×10 19 .cm -3 ~7×10 20 .cm -3 ; And / or, the first functional layer is a silicon nitride layer; And / or, the thickness of the first functional layer is 70nm-80nm.
9. A solar cell, characterized in that: The solar cell is prepared by the method for preparing a solar cell according to any one of claims 1 to 8; the solar cell comprises: A silicon wafer, wherein the silicon wafer has a first surface and a second surface opposite to the first surface, wherein one of the first surface and the second surface is a light-receiving surface and the other is a backlight surface; a tunneling layer, wherein the tunneling layer is disposed on the first surface; A doped polysilicon layer, wherein the doped polysilicon layer is disposed on a side of the tunneling layer away from the silicon wafer; the thickness of the doped polysilicon layer is 50 nm to 100 nm; A first functional layer, the first functional layer being disposed on a side of the doped polysilicon layer away from the tunneling layer; and A first metal electrode, wherein the first metal electrode penetrates the first functional layer and forms an ohmic contact with the doped polysilicon layer; a forked metal-silicon hybrid structure is formed at the contact point between the first metal electrode and the doped polysilicon layer.
10. The solar cell according to claim 9, characterized in that: Also includes: a doped layer, the doped layer being arranged on the second surface; the doped layer having a first conductivity type, the silicon wafer and the doped polysilicon layer having a second conductivity type, one of the first conductivity types being an N type and the other being a P type; a second functional layer, the second functional layer being disposed on a side of the doped layer facing away from the silicon wafer; and A second metal electrode is provided, wherein the second metal electrode penetrates the second functional layer and forms an ohmic contact with the doping layer.
11. The solar cell according to claim 9, characterized in that: The doped polysilicon layer has a blocking layer and a passivation layer therein.
12. The solar cell according to claim 11, characterized in that: The metal-silicon mixed structure is a silver-silicon mixed structure; And / or, the tunneling layer is a silicon oxide layer; And / or, the thickness of the tunneling layer is 1.25 nm to 1.45 nm; And / or, the sheet resistance of the doped polysilicon layer is 15Ω / sq to 25Ω / sq; And / or, the surface doping concentration of the doped polysilicon layer is 5×10 19 .cm -3 ~7×10 20 .cm -3 ; And / or, the first functional layer is a silicon nitride layer; And / or, the thickness of the first functional layer is 70nm to 80nm; And / or, the blocking and passivation layer is a silicon oxide layer.
13. A photovoltaic module, characterized in that: Comprising the solar cell according to any one of claims 9 to 12.