Multi-element Bianstone Ceramic Glaze

By adjusting the formula and firing process of multi-element Bianstone ceramic glaze, the problem of the difference in expansion coefficient between Bianstone and white glaze was solved, resulting in Bianstone ceramic glaze vessels with high yield and health benefits.

CN117819939BActive Publication Date: 2026-11-17冯琪茗 +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310622628.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2026-11-17
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

The application of Bian stone in ceramic glazes in the existing technology has problems such as low yield, deformation caused by the difference in expansion coefficient between Bian stone and white glaze, high fluidity of Bian stone glaze and insufficient function.

Method used

A multi-element Bianstone ceramic glaze formula, including jade clay, white glaze, and Bianstone ceramic glaze, was adopted. By adjusting the formula and introducing zirconium silicate as a stabilizer, combined with a reasonable firing process, the problem of the difference in expansion coefficient between Bianstone and white glaze was solved, and a good fusion of Bianstone and other ceramic raw materials was achieved.

Benefits of technology

It improves the yield of ceramic products, and the application of Bian stone glaze enables the vessels to change the water quality when holding drinking water, and the trace elements produced after drinking have health benefits.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a multi-element Bianstone ceramic glaze. By selecting a scientifically proportioned formula of jade clay, white glaze, and Bianstone ceramic glaze, and adding zirconium silicate as a stabilizer to the Bianstone ceramic glaze formula, the expansion coefficients of the white glaze and the Bianstone ceramic glaze are made to be basically the same, which greatly improves the yield of the multi-element Bianstone ceramic glaze. At the same time, by combining the three formulas and the glaze firing temperature curve, Bianstone is completely and well integrated with other ceramic raw materials, perfectly bringing out the medicinal value of Bianstone. When drinking water is stored in vessels made of natural Bianstone ceramic glaze, it can soften the water and change its quality. The trace elements produced after drinking the water can play a health care role.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a multi-element Bianstone ceramic glaze, belonging to the field of ceramic materials technology. Background Technology

[0002] Bian stone is a very unique stone. It is a meteorite from outer space. Both the "Huangdi Neijing" and "Compendium of Materia Medica" record the use of Bian stone to treat diseases. Adding Bian stone to ceramic glazes allows its multi-element content to achieve health benefits.

[0003] Currently, there are few reports on how to ideally apply Bian stone to ceramics. This is partly because Bian stone is a non-renewable resource and is expensive. The outer glaze uses conventional white glaze, while the inner glaze (the area in contact with drinking water and food) uses Bian stone ceramic glaze. The expansion coefficients of the two glazes are completely different, making them prone to deformation when fired at a high temperature of 1300 degrees Celsius, resulting in an extremely low yield. On the other hand, the main chemical component of Bian stone is calcium carbonate, with a calcium carbonate content as high as 85.3%. When the amount of calcium carbonate in the glaze is too high, the glaze becomes too fluid under high temperature, making it impossible to produce a product. Excessive introduction of alumina will lead to unevenness on the glaze surface. If the amount of calcium carbonate in the glaze is too low, the product's function will not meet the requirements. Summary of the Invention

[0004] The purpose of this invention is to provide a multi-element Bianstone ceramic glaze.

[0005] To solve the above-mentioned technical problems, the technical solution adopted by the present invention includes the following steps: A multi-element Bianstone ceramic glaze, composed of the following three components: Jade clay: Composed of high-quality kaolin, high-quality white calcined kaolin, feldspar, calcined talc and quartz; White glaze: composed of high-quality feldspar, quartz, calcined talc, zinc oxide, Bian stone, and high-quality kaolin; Bianstone ceramic glaze: composed of natural high-quality Bianstone, high-quality kaolin, zirconium silicate, zinc oxide, and calcined talc.

[0006] The composition ratio of the jade clay is as follows: Aluminum oxide 20.8%~22.9%, silicon dioxide 65.3%~66.65%, iron oxide 0.13%~0.17%, calcium oxide 0.18%~0.22%, potassium oxide 4.8%~5.8%, sodium oxide 1.55%~1.95%, magnesium oxide 0.09%, titanium dioxide 0.03%, zirconium dioxide <0.01%, barium oxide 0.05%, phosphorus pentoxide <0.01%, nickel monoxide <0.01%, cobalt monoxide <0.01%, copper oxide <0.01%, rubidium oxide 0.03%, sulfur trioxide <0.01%, lithium oxide <0.01%, lead monoxide <0.01%, zinc oxide <0.01%, cadmium oxide <0.01%, strontium oxide <0.01%, manganese monoxide <0.01%, chromium trioxide <0.01%.

[0007] The composition ratio of the white glaze is as follows: Aluminum oxide 11.1%~12.4%, silicon dioxide 62.25%~63.65%, ferric oxide 0.1%~0.14%, calcium oxide 5.15%~5.8%, magnesium oxide 2.4%~4.5%, sodium oxide 0.75%~1.55%, titanium dioxide 0.09%, zirconium dioxide 0.07%, barium oxide 0.05%, phosphorus pentoxide <0.05%, lithium oxide <0.01%, lead monoxide <0.01%, zinc oxide 1.00%, cadmium oxide <0.01%, strontium oxide <0.01%, manganese monoxide <0.01%, rubidium oxide 0.02%, sulfur trioxide <0.05%, boron trioxide <0.05%, fluorine <0.05%, cesium oxide <0.01%.

[0008] The composition ratio of Bianstone ceramic glaze is as follows: Aluminum oxide 9.4%~13.2%, silicon dioxide 47.1%~55.1%, iron oxide 0.2%~0.8%, calcium oxide 14.5%~17.4%, magnesium oxide 0.8%~3.4%, potassium oxide 0.6%~0.65%, zirconium dioxide 0.1%~2.8%, zinc oxide 0.15%~1.5%, sodium oxide <0.01%, barium oxide <0.02%, phosphorus pentoxide 0.11%, yttrium oxide 0.02%, strontium oxide 0.006%, manganese monoxide 0.03%, chromium oxide <0.005%, nickel monoxide <0.002%, copper oxide 0.02%, sulfur trioxide 0.04%, chlorine 0.10%.

[0009] Preferably, the component ratio of jade clay, white glaze, and Bian stone ceramic glaze is as follows: Jade Clay: Aluminum oxide 21.66%, Silicon dioxide 66.59%, Iron oxide 0.15%, Calcium oxide 0.19%, Magnesium oxide 0.09%, Potassium oxide 5.12%, Sodium oxide 1.80%, Titanium dioxide 0.03%, Zirconium dioxide <0.01%, Barium oxide 0.05%, Phosphorus pentoxide <0.01%, Lithium oxide <0.01%, Lead monoxide <0.01%, Zinc oxide <0.01%, Cadmium oxide <0.01%, Strontium oxide <0.01%, Manganese monoxide <0.01%, Chromium oxide <0.01%, Nickel monoxide <0.01%, Cobalt monoxide <0.01%, Copper oxide <0.01%, Rubidium oxide 0.03%, Sulfur trioxide <0.01%.

[0010] White glaze: Aluminum oxide 11.96, Silicon dioxide 62.30, Ferric oxide 0.12, Calcium oxide 5.32, Magnesium oxide 2.52, Sodium oxide 1.38, Titanium dioxide 0.09, Zirconium dioxide 0.07, Barium oxide <0.05, Phosphorus pentoxide <0.05, Lithium oxide <0.01, Lead monoxide <0.01, Zinc oxide 1.00, Cadmium oxide <0.01, Strontium oxide <0.01, Manganese monoxide <0.01, Chromium oxide <0.05, Nickel monoxide <0.01, Rubidium oxide 0.02, Sulfur trioxide 0.05, Boron trioxide <0.05, Fluorine <0.05, Cesium oxide <0.01.

[0011] Bianstone ceramic glaze: Aluminum oxide 13.18, Silicon dioxide 49.30, Iron oxide 0.65, Calcium oxide 17.00, Magnesium oxide 0.87, Potassium oxide 0.61, Sodium oxide <0.01, Titanium dioxide <0.02, Zirconium dioxide 0.18, Barium oxide <0.02, Phosphorus pentoxide 0.11, Yttrium oxide 0.02, Zinc oxide 0.19, Strontium oxide 0.006, Manganese monoxide 0.03, Chromium oxide <0.05, Nickel monoxide <0.002, Copper oxide 0.02, Sulfur trioxide 0.04, Chlorine 0.10.

[0012] More preferably, the component ratio of jade clay, white glaze, and Bian stone ceramic glaze is as follows: Jade mud: Aluminum oxide 22.87, Silicon dioxide 65.36, Iron oxide 0.14, Calcium oxide 0.21, Magnesium oxide 0.09, Potassium oxide 5.74, Sodium oxide 1.59, Titanium dioxide 0.03, Zirconium dioxide <0.01, Barium oxide 0.05, Phosphorus pentoxide <0.01, Nickel monoxide <0.01, Cobalt monoxide <0.01, Copper oxide <0.01, Rubidium oxide 0.03, Sulfur trioxide <0.01.

[0013] White glaze: Aluminum oxide 12.36, Silicon dioxide 63.59, Iron oxide 0.11, Calcium oxide 5.76, Magnesium oxide 4.16, Potassium oxide 2.88, Sodium oxide 0.80, Titanium dioxide 0.09, Zirconium dioxide 0.07, Barium oxide 0.05, Phosphorus pentoxide <0.05, Lithium oxide <0.01, Lead monoxide <0.01, Zinc oxide 1.00, Cadmium oxide <0.01, Strontium oxide <0.01, Manganese monoxide <0.01, Rubidium oxide 0.02, Sulfur trioxide <0.05, Boron trioxide <0.05, Fluorine <0.05, Cesium oxide <0.01.

[0014] Bianstone ceramic glaze: Aluminum oxide 9.44%, Silicon dioxide 47.20%, Iron oxide 0.76%, Calcium oxide 17.31%, Magnesium oxide 3.28%, Potassium oxide 0.64%, Sodium oxide <0.01%, Titanium dioxide 0.02%, Zirconium dioxide 2.78%, Barium oxide <0.02%, Phosphorus pentoxide 0.11%, Yttrium oxide 0.02%, Zinc oxide 1.44%, Strontium oxide 0.006%, Manganese monoxide 0.03%, Chromium oxide <0.005%, Nickel monoxide <0.002%, Copper oxide 0.02%, Sulfur trioxide 0.04%, Chlorine 0.10.

[0015] A multi-element Bianstone ceramic glaze, also including a preparation process, the specific steps of which are as follows: (1) Prepare the jade clay, white glaze and Bian stone ceramic glaze according to the proportion of ingredients, and then put them into the upper ball mill for ball milling. Add water of 80%~100% of the mass of the clay and glaze respectively. Ball mill the jade clay for 24 hours, and the white glaze and Bian stone ceramic glaze for 18 hours. After ball milling, the jade clay is passed through a 220-mesh sieve, and the white glaze and Bian stone ceramic glaze are passed through a 260-mesh sieve. Then put them into the lower ball mill for ball milling, and add water of 55%~75% of the mass of the clay and glaze respectively. Ball mill the jade clay for 24 hours, and the white glaze and Bian stone ceramic glaze for 18 hours. After ball milling, remove iron by gravity separation. The jade clay is passed through a 220-mesh sieve, and the white glaze and Bian stone ceramic glaze are passed through a 260-mesh sieve. (2) After sieving, the jade clay is pressed and coarsely refined. Then, it is stored in the warehouse for 6-8 days along with the white glaze and Bian stone ceramic glaze. After aging, the jade clay is refined. Then, the jade clay is sent to be formed by hand-pulling or by slip casting. After the blank dries, it is trimmed to obtain the refined blank. The refined blank is inspected to remove defective products. (3) Place the inspected blanks into the bisque firing kiln and fire them at 780℃ for 5 hours. After cooling, inspect the bisques to pick out the defective ones. Then add water to the bisques, apply white glaze, add water again, and then let the bisques dry naturally for 4 hours. After drying, apply Bian stone ceramic glaze and clear bottom glaze, trim the edges of the bisques, and then blow off the ash to inspect the bisques. (4) Place the bisque fired after the ash blowing inspection into the shuttle kiln, and then start the kiln firing and glaze firing. After the glaze firing is completed, wait for it to cool naturally. Take the finished products out of the kiln to inspect them and pick out the defective products. Grind the bottom of the finished products and then put them into the warehouse.

[0016] Further, the firing temperature curve of the kiln glaze in step (4) is as follows: starting from room temperature, the temperature is raised to 600℃ for 2 hours, then raised to 980℃ for 3.5 hours, and held at 980℃ for 0.5 hours, then raised to 1160℃ for 2 hours, while firing the ceramic in a reducing flame, and finally raised to 1300℃ for 2 hours, and held at 1300℃ for 20 minutes.

[0017] The beneficial effects of this invention are as follows: This invention solves the problem of extremely low yield caused by the completely different expansion coefficients between white glaze and Bianstone ceramic glaze by adjusting the formulas of white glaze and Bianstone ceramic glaze and introducing zirconium silicate as a stabilizer into Bianstone ceramic glaze. At the same time, it fully integrates Bianstone with other ceramic raw materials, perfectly bringing out the medicinal value of Bianstone. When drinking water is stored in vessels made with natural Bianstone ceramic glaze, the water quality can be softened, thus changing the water quality. The trace elements produced after drinking the water can have a health-preserving effect. Detailed Implementation

[0018] The present invention will be further described in detail below with reference to the embodiments. Example 1

[0019] The components of jade clay, white glaze, and Bian stone ceramic glaze are formulated in a more optimized ratio.

[0020] The firing temperature curve for the glaze is as follows: starting from room temperature, the temperature is raised to 600℃ in 2 hours, then raised to 980℃ in 3.5 hours and held at 980℃ for 0.5 hours. The temperature is then raised to 1160℃ in 2 hours, while the ceramic is fired in a reducing flame. Finally, the temperature is raised to 1300℃ in 2 hours and held at 1300℃ for 20 minutes.

[0021] (1) Prepare the jade clay, white glaze and Bian stone ceramic glaze according to the proportion of ingredients, and then put them into the upper ball mill for ball milling. Add water equal to 90% of the mass of the clay and glaze. Ball mill the jade clay for 24 hours, and the white glaze and Bian stone ceramic glaze for 18 hours. After ball milling, the jade clay is passed through a 220-mesh sieve, and the white glaze and Bian stone ceramic glaze are passed through a 260-mesh sieve. Then put them into the lower ball mill for ball milling, and add water equal to 65% of the mass of the clay and glaze. Ball mill the jade clay for 24 hours, and the white glaze and Bian stone ceramic glaze for 18 hours. After ball milling, remove iron by gravity separation. The jade clay is passed through a 220-mesh sieve, and the white glaze and Bian stone ceramic glaze are passed through a 260-mesh sieve. (2) After sieving, the jade clay is pressed and coarsely refined. Then, it is stored in the warehouse for 7 days along with the white glaze and Bian stone ceramic glaze. After aging, the jade clay is refined. Then, the jade clay is sent to be formed by hand-pulling or by slip casting. After the blank dries, it is trimmed to obtain the refined blank. The refined blank is inspected to remove defective products. (3) Place the inspected blanks into the bisque firing kiln and fire them at 780℃ for 5 hours. After cooling, inspect the bisques to pick out the defective ones. Then add water to the bisques, apply white glaze, add water again, and then let the bisques dry naturally for 4 hours. After drying, apply Bian stone ceramic glaze and clear bottom glaze, trim the edges of the bisques, and then blow off the ash to inspect the bisques. (4) Place the bisque fired after the ash blowing inspection into the shuttle kiln, and then start the kiln firing and glaze firing. After the glaze firing is completed, wait for it to cool naturally. Take the finished products out of the kiln to inspect them and pick out the defective products. Grind the bottom of the finished products and then put them into the warehouse. Example 2

[0022] The components of jade clay, white glaze, and Bian stone ceramic glaze are formulated in a more optimized ratio.

[0023] The firing temperature curve for the glaze is as follows: starting from room temperature, the temperature is raised to 600℃ in 2 hours, then raised to 980℃ in 3.5 hours and held at 980℃ for 0.5 hours. The temperature is then raised to 1160℃ in 2 hours, while the ceramic is fired in a reducing flame. Finally, the temperature is raised to 1300℃ in 2 hours and held at 1300℃ for 20 minutes.

[0024] (1) Prepare the jade clay, white glaze and Bian stone ceramic glaze according to the proportion of ingredients, and then put them into the upper ball mill for ball milling. Add water equal to 80% of the mass of the clay and glaze. Ball mill the jade clay for 24 hours, and the white glaze and Bian stone ceramic glaze for 18 hours. After ball milling, the jade clay is passed through a 220-mesh sieve, and the white glaze and Bian stone ceramic glaze are passed through a 260-mesh sieve. Then put them into the lower ball mill for ball milling. Add water equal to 75% of the mass of the clay and glaze. Ball mill the jade clay for 24 hours, and the white glaze and Bian stone ceramic glaze for 18 hours. After ball milling, remove iron by gravity separation. The jade clay is passed through a 220-mesh sieve, and the white glaze and Bian stone ceramic glaze are passed through a 260-mesh sieve. (2) After sieving, the jade clay is pressed and coarsely refined. Then, it is stored in the warehouse for 6 days along with the white glaze and Bian stone ceramic glaze. After aging, the jade clay is refined. Then, the jade clay is sent to be formed by hand-pulling or by slip casting. After the blank dries, it is trimmed to obtain the refined blank. The refined blank is inspected to remove defective products. (3) Place the inspected blanks into the bisque firing kiln and fire them at 780℃ for 5 hours. After cooling, inspect the bisques to pick out the defective ones. Then add water to the bisques, apply white glaze, add water again, and then let the bisques dry naturally for 4 hours. After drying, apply Bian stone ceramic glaze and clear bottom glaze, trim the edges of the bisques, and then blow off the ash to inspect the bisques. (4) Place the bisque fired after the ash blowing inspection into the shuttle kiln, and then start the kiln firing and glaze firing. After the glaze firing is completed, wait for it to cool naturally. Take the finished products out of the kiln to inspect them and pick out the defective products. Grind the bottom of the finished products and then put them into the warehouse. Example 3

[0025] The components of jade clay, white glaze, and Bian stone ceramic glaze are formulated in a more optimized ratio.

[0026] The firing temperature curve for the glaze is as follows: starting from room temperature, the temperature is raised to 600℃ in 2 hours, then raised to 980℃ in 3.5 hours and held at 980℃ for 0.5 hours. The temperature is then raised to 1160℃ in 2 hours, while the ceramic is fired in a reducing flame. Finally, the temperature is raised to 1300℃ in 2 hours and held at 1300℃ for 20 minutes.

[0027] (1) Prepare the jade clay, white glaze and Bian stone ceramic glaze according to the proportion of ingredients, and then put them into the upper ball mill for ball milling. Add water equal to 100% of the mass of the clay and glaze. Ball mill the jade clay for 24 hours, and the white glaze and Bian stone ceramic glaze for 18 hours. After ball milling, the jade clay is passed through a 220-mesh sieve, and the white glaze and Bian stone ceramic glaze are passed through a 260-mesh sieve. Then put them into the lower ball mill for ball milling, and add water equal to 55% of the mass of the clay and glaze. Ball mill the jade clay for 24 hours, and the white glaze and Bian stone ceramic glaze for 18 hours. After ball milling, remove iron by gravity separation. The jade clay is passed through a 220-mesh sieve, and the white glaze and Bian stone ceramic glaze are passed through a 260-mesh sieve. (2) After sieving, the jade clay is pressed and coarsely refined. Then, it is stored in the warehouse for 8 days along with the white glaze and Bian stone ceramic glaze. After aging, the jade clay is refined. Then, the jade clay is sent to be formed by hand-pulling or by slip casting. After the blank dries, it is trimmed to obtain the refined blank. The refined blank is inspected to remove defective products. (3) Place the inspected blanks into the bisque firing kiln and fire them at 780℃ for 5 hours. After cooling, inspect the bisques to pick out the defective ones. Then add water to the bisques, apply white glaze, add water again, and then let the bisques dry naturally for 4 hours. After drying, apply Bian stone ceramic glaze and clear bottom glaze, trim the edges of the bisques, and then blow off the ash to inspect the bisques. (4) Place the bisque fired after the ash blowing inspection into the shuttle kiln, and then start the kiln firing and glaze firing. After the glaze firing is completed, wait for it to cool naturally. Take the finished products out of the kiln to inspect them and pick out the defective products. Grind the bottom of the finished products and then put them into the warehouse. Example 4

[0028] The components of jade clay, white glaze, and Bian stone ceramic glaze are selected in optimal proportions.

[0029] The rest is the same as in Example 1. Example 5

[0030] Zirconium silicate is not introduced as a stabilizer in Bian stone ceramic glaze.

[0031] The rest is the same as in Example 1. Example 6

[0032] The firing temperature curve for the glaze is as follows: starting from room temperature, the temperature is raised to 400℃ in 1 hour, then raised to 800℃ in 2 hours and held at 800℃ for 1 hour, then raised to 1200℃ in 1 hour and held at 1200℃ for 5 hours.

[0033] The rest is the same as in Example 1.

[0034] Boiling water was added to the ceramic glaze vessels prepared in Examples 1 to 6, and then the vessels were left to stand for 1 hour. After standing, the water-soluble ions were measured using ICP-OES and ICP-MS methods. The yield of ceramic glaze vessels in each example was calculated. The specific data are shown in Table 1.

[0035] Table 1. Yield and water-soluble ion content data for each embodiment. Implementation Items Finished product yield of utensils (%) Calcium (mg / L) Iron (mg / L) Potassium (mg / L) Magnesium (mg / L) Example 1 93.3 20.77 0.0589 18.61 0.592 Example 2 92.8 20.83 0.0552 18.55 0.581 Example 3 93.2 20.61 0.0573 18.53 0.574 Example 4 86.2 18.21 0.0434 17.08 0.493 Example 5 42.3 19.65 0.0528 17.92 0.521 Example 6 71.9 15.33 0.0321 13.44 0.362 Table 1 shows that the yield and water-soluble ion content of the vessels in Examples 1 to 3 were at the highest levels. Example 4 changed the composition of jade clay, white glaze, and Bian stone ceramic glaze. This may be because the change in composition resulted in a certain difference in the expansion coefficient between the two glazes, and the change also made it impossible for Bian stone to fully integrate with other ceramic raw materials. Therefore, its yield and water-soluble ion content both decreased. Example 5 did not introduce zirconium silicate into the Bian stone ceramic glaze. Without zirconium silicate as a stabilizer, the yield of the vessels decreased sharply. Example 6 changed the heating curve of the kiln firing glaze. Its yield and water-soluble ion content decreased significantly. This may be because the heating curve was not set properly, which made the ceramic prone to cracking, thus reducing the yield of the vessels. It also made it impossible for Bian stone to integrate with other ceramic materials during the firing process, resulting in a lower water-soluble ion content after adding water.

Claims

1. A multi-element Bianstone ceramic glaze, characterized in that: It consists of the following three components: Jade clay: Composed of high-quality kaolin, high-quality white calcined kaolin, feldspar, calcined talc and quartz; White glaze: composed of high-quality feldspar, quartz, calcined talc, zinc oxide, Bian stone, and high-quality kaolin; Bianstone ceramic glaze: composed of natural high-quality Bianstone, high-quality kaolin, zirconium silicate, zinc oxide, and calcined talc; Jade Clay: Aluminum oxide 20.8%~22.9%, Silicon dioxide 65.3%~66.65%, Ferric oxide 0.13%~0.17%, Calcium oxide 0.18%~0.22%, Potassium oxide 4.8%~5.8%, Sodium oxide 1.55%~1.95%, Magnesium oxide 0.09%, Titanium dioxide 0.03%, Zirconium dioxide <0.01%, Barium oxide 0.05%, Phosphorus pentoxide <0.01%, Nickel monoxide <0.01%, Cobalt monoxide <0.01%, Copper oxide <0.01%, Rubidium oxide 0.03%, Sulfur trioxide <0.01%, Lithium oxide <0.01%, Lead monoxide <0.01%, Zinc oxide <0.01%, Cadmium oxide <0.01%, Strontium oxide <0.01%, Manganese oxide <0.01%, Chromium trioxide <0.01%; White glaze: Aluminum oxide 11.1%~12.4%, Silicon dioxide 62.25%~63.65%, Ferric oxide 0.1%~0.14%, Calcium oxide 5.15%~5.8%, Magnesium oxide 2.4%~4.5%, Sodium oxide 0.75%~1.55%, Titanium dioxide 0.09%, Zirconium dioxide 0.07%, Barium oxide 0.05%, Phosphorus pentoxide <0.05%, Lithium oxide <0.01%, Lead monoxide <0.01%, Zinc oxide 1.00%, Cadmium oxide <0.01%, Strontium oxide <0.01%, Manganese oxide <0.01%, Rubidium oxide 0.02%, Sulfur trioxide <0.05%, Boron trioxide <0.05%, Fluorine <0.05%, Cesium oxide <0.01%; Bianstone ceramic glaze: Aluminum oxide 9.4%~13.2%, silicon dioxide 47.1%~55.1%, ferric oxide 0.2%~0.8%, calcium oxide 14.5%~17.4%, magnesium oxide 0.8%~3.4%, potassium oxide 0.6%~0.65%, zirconium dioxide 0.1%~2.8%, zinc oxide 0.15%~1.5%, sodium oxide <0.01%, barium oxide <0.02%, phosphorus pentoxide 0.11%, yttrium oxide 0.02%, strontium oxide 0.006%, manganese monoxide 0.03%, chromium oxide <0.005%, nickel monoxide <0.002%, copper oxide 0.02%, sulfur trioxide 0.04%, chlorine 0.10%; The specific preparation steps are as follows: (1) Prepare the jade clay, white glaze and Bian stone ceramic glaze according to the proportion of ingredients, and then put them into the upper ball mill for ball milling. Add water of 80%~100% of the mass of the clay and glaze respectively. Ball mill the jade clay for 24 hours, and the white glaze and Bian stone ceramic glaze for 18 hours. After ball milling, the jade clay is passed through a 220-mesh sieve, and the white glaze and Bian stone ceramic glaze are passed through a 260-mesh sieve. Then put them into the lower ball mill for ball milling, and add water of 55%~75% of the mass of the clay and glaze respectively. Ball mill the jade clay for 24 hours, and the white glaze and Bian stone ceramic glaze for 18 hours. After ball milling, remove iron by gravity separation. The jade clay is passed through a 220-mesh sieve, and the white glaze and Bian stone ceramic glaze are passed through a 260-mesh sieve. (2) After sieving, the jade clay is pressed and coarsely refined. Then, it is stored in the warehouse for 6-8 days along with the white glaze and Bian stone ceramic glaze. After aging, the jade clay is refined. Then, the jade clay is sent to be formed by hand-pulling or by slip casting. After the blank dries, it is trimmed to obtain the refined blank. The refined blank is inspected to remove defective products. (3) Place the inspected blanks into the bisque firing kiln and fire them at 780℃ for 5 hours. After cooling, inspect the bisque fired blanks to pick out the defective ones. Then add water to the bisque fired blanks, apply white glaze, add water again, and then let the bisque fired blanks dry naturally for 4 hours. After drying, apply Bian stone ceramic glaze and clear bottom glaze and trim the edges of the glazed blanks. Then blow ash off the glazed blanks for inspection. (4) After the glaze blanks are inspected by blowing off the ash, they are put into the shuttle kiln and then the kiln is fired. After the glaze is fired, wait for it to cool naturally to room temperature. After the finished products are taken out of the kiln, the defective products are picked out and the bottom of the finished products is ground. After the finished products are completed, they can be put into storage. The heating curve for firing the glaze in step (4) is as follows: starting from room temperature, the temperature is raised to 600℃ for 2 hours, then raised to 980℃ for 3.5 hours, and held at 980℃ for 0.5 hours. Then the temperature is raised to 1160℃ for 2 hours, while the ceramic is fired in a reducing flame. Finally, the temperature is raised to 1300℃ for 2 hours, and held at 1300℃ for 20 minutes.

Citation Information

Patent Citations

  • High-transmittance white jade porcelain and production method thereof

    CN108821582A

  • Manufacturing method of soft-light glazed ceramic chip

    CN111875415A