Preparation method and application of a self-cleaning nano-optical radiation refrigeration coating
By combining the design of the bottom refrigeration layer and the upper self-cleaning layer, the problem of insufficient performance and susceptibility to contamination of the existing refrigeration coating is solved, a nano-optical radiation refrigeration coating with high reflectivity and self-cleaning function is achieved, and the coating is improved. performance and durability.
Patent Information
- Application Number
- CN202311792081.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-25
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-12-25
AI Technical Summary
While the existing refrigeration coating improves the reflectivity, the filler volume concentration is too large, resulting in insufficient coating performance, and it is susceptible to contamination when exposed to the atmospheric environment for a long time, affecting performance.
A self-cleaning nano-optical radiation refrigeration coating is used, which is composed of a bottom refrigeration layer and an upper self-cleaning layer. The bottom refrigeration layer is composed of water, hydrophilic materials, polyvinylidene fluoride resin powder, fillers, etc., and the upper self-cleaning layer is composed of water, grate, etc. It is composed of sesame oil, mica powder, vermiculite powder, etc., and through specific stirring steps and temperature control, a coating with high reflectivity and self-cleaning function is formed.
It achieves high reflectivity and good cooling effect, and also has a self-cleaning function, which can effectively resist external impurities and stains and improve the wear resistance and service life of the coating.
Smart Images

Figure BDA0004626658070000061 
Figure BDA0004626658070000062 
Figure BDA0004626658070000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of architectural coatings, and in particular relates to a preparation method and application of a self-cleaning nano-optical radiation refrigeration coating. Background Art
[0002] Radiative cooling refers to a method of making a high-temperature object radiate energy to the outside world to lower its temperature. Radiative cooling uses the principle that objects that are not in contact with each other in a vacuum environment exchange heat with each other due to differences in temperature to cool high-temperature objects. In traditional coatings, inorganic fillers are used to refract light and reflect sunlight to achieve the purpose of cooling.
[0003] However, existing materials have some defects. For example, inorganic fillers have a large oil absorption capacity. If you want to obtain a higher reflectivity, you need to increase the content of inorganic fillers in the refrigeration coating. However, the volume concentration of the filler is much greater than the critical volume concentration of the filler. At this time, although the refrigeration coating has a high reflectivity, other materials are not enough to fill the gaps between the fillers, which causes gaps in the refrigeration coating, resulting in insufficient basic performance of the refrigeration coating, and mechanical properties and weather resistance cannot meet daily use. In addition, the existing refrigeration coating is attached to the outer surface of the object, giving the object a cooling and beautifying decorative effect, but the coating is exposed to the atmospheric environment for a long time and is easily affected by impurities, rain and snow in the air, causing stains on the coating surface, affecting the performance of the refrigeration coating. Therefore, based on the existing problems, it is necessary to meet the refrigeration requirements while making it have a self-cleaning function. Summary of the invention
[0004] In view of this, an object of the present invention is to provide an optical radiation refrigeration coating with a self-cleaning function, a preparation method and an application thereof.
[0005] To achieve the above object, the present invention provides the following technical solution: a self-cleaning nano-optical radiation refrigeration coating, the refrigeration coating is composed of a bottom refrigeration layer and an upper self-cleaning layer, and by weight: the bottom refrigeration layer is composed of 120-160 parts of water, 60-80 parts of hydrophilic material, 5-10 parts of film-forming agent, 3-7 parts of color additive, 3-7 parts of waterproofing agent, 20-30 parts of polyvinylidene fluoride resin powder, and 50-70 parts of filler;
[0006] In terms of weight, the upper self-cleaning layer is composed of 20-30 parts of water, 3-5 parts of castor oil, 10-15 parts of mica powder, 3-5 parts of vermiculite powder, 4-6 parts of leveling agent, 2-4 parts of defoaming agent, 2-4 parts of curing agent, 8-15 parts of calcium carbonate, and 5-8 parts of ethyl acetate.
[0007] Furthermore, the hydrophilic material of the bottom refrigeration layer is composed of aluminum oxide, silicon oxide, zirconium oxide, and quartz; the film-forming agent is an acrylic resin film-forming agent, which is formed by the copolymerization of acrylate, acrylonitrile, and acrylamide; the color additive is composed of one or more of titanium dioxide, nano zinc oxide, red iron oxide, and phthalocyanine blue; the waterproofing agent is a fluorocarbon waterproofing agent; the filler is a metal filler, which is composed of two or more of titanium dioxide, magnesium oxide, and barium sulfate.
[0008] Furthermore, the leveling agent in the upper self-cleaning layer is composed of two or more of polyacrylic acid, carboxymethyl cellulose and silicone oil; the defoaming agent is composed of polyether, silicone oil and ethanol; and the curing agent is ethylenediamine (EDA).
[0009] Furthermore, the particle size of the filler is 7-12 μm; and the particle size of the polyvinylidene fluoride resin powder is 0.5-5 μm.
[0010] Furthermore, the total dry film thickness of the refrigeration layer and the self-cleaning layer when in use is no more than 1.5 mm.
[0011] Furthermore, a method for preparing an optical radiation cooling coating with a self-cleaning function is also included, comprising the following steps:
[0012] S1, adding filler, polyvinylidene fluoride resin powder and pigment additive into water, stirring to obtain the first primary mixture, and letting it stand;
[0013] S2, continue to add water and hydrophilic material to the first primary mixture and stir, and then add waterproofing agent and film-forming agent and stir to obtain a refrigeration film;
[0014] S3, adding mica powder and vermiculite powder to water and mixing, and then adding leveling agent, calcium carbonate and ethyl acetate under stirring to obtain a second primary mixture;
[0015] S4, continue to add castor oil, defoamer and curing agent to the second primary mixture, and after standing, obtain a self-cleaning film;
[0016] S5. After evenly applying the cooling film to the surface of the substrate, a cooling layer is obtained, and then the cooling layer is covered with a self-cleaning film, and after air drying, an optical radiation cooling coating with a self-cleaning function is obtained.
[0017] Furthermore, in step S1, the stirring speed is 50-70 rpm / min, the stirring time is 5-7 minutes, and the stirring temperature is stirring at room temperature; in step S2, the stirring speed is 100-120 rpm / min, the stirring time is 20-30 minutes, and the stirring temperature is 40-50 degrees Celsius.
[0018] Furthermore, in the step S3, the mica powder and the vermiculite powder are first stirred at 50-60 rpm / min for 5-7 minutes at room temperature, and after the leveling agent, calcium carbonate and ethyl acetate are added, they are stirred at 40-45 degrees Celsius at a speed of 100-150 rpm / min for 10-15 minutes; in the step S4, the temperature when the castor oil, the defoamer and the curing agent are added is 50-70 degrees Celsius, the rotation speed is 150-200 rpm / min, and the stirring time is 20-25 minutes.
[0019] Furthermore, an optical radiation cooling coating with a self-cleaning function is used for cooling and self-cleaning the surface of a substrate.
[0020] The beneficial effects of the present invention are:
[0021] 1. The raw materials of the present invention are simple and easy to obtain. Through the method of the present invention, after the substances are combined according to specific components, the stirring method and temperature adopted can reduce the precipitation formed due to agglomeration of the coating during preparation, and maximize the properties of the substances, so that the refrigeration coating and the self-cleaning film prepared by the present invention are combined to achieve the purpose of the present application.
[0022] 2. The acrylic resin used in the present invention has good film-forming properties, strong adhesion, good film flexibility, large ductility, high light transmittance, light resistance and aging resistance; castor oil and the like can make the finished product smooth and crack-free.
[0023] 3. The hydrophilic material of the present invention has a certain affinity for metals, and the filler is an inorganic oxide. The two are similar and can be well dispersed in water to prepare a coating. A mixture of silicon dioxide, zinc oxide, barium sulfate, magnesium oxide, calcium carbonate, etc. is added to the coating as a functional filler. While improving the solar reflectance and atmospheric window emissivity of the coating, it can also effectively increase the hardness of the coating, improve the wear resistance of the coating, and further improve the ability of the coating to resist the impact or friction of external particles such as wind, sand, and dust.
[0024] 4. In the present invention, by adding polyvinylidene fluoride resin powder and ethyl acetate, the coating can be closely combined with the substrate during preparation, and the coating and the coating, and the coating and the substrate can have strong adhesion, and it is not easy to fall off during use, thereby improving its service life.
[0025] Other advantages, objectives and features of the present invention will be described in the following description and will be apparent to those skilled in the art to some extent, or those skilled in the art may be taught from the practice of the present invention. The objectives and other advantages of the present invention may be realized and obtained through the following description. DETAILED DESCRIPTION
[0026] A self-cleaning optical radiation cooling coating
[0027] Example 1
[0028] S1, after mixing 20 parts of titanium dioxide, 20 parts of magnesium oxide, and 10 parts of barium sulfate, add them to 80 parts of water, then add 20 parts of polyvinylidene fluoride resin powder, 1 part of titanium dioxide, and 2 parts of nano zinc oxide to the water, stir at 50 rpm / min for 5 minutes, and let stand for 10 minutes to obtain the first primary mixture;
[0029] S2, add 30 parts of aluminum oxide, 30 parts of silicon oxide, and 40 parts of water to the first primary mixture, stir at a rate of 100 rpm / min for 20 minutes, and then add 3 parts of fluorocarbon waterproofing agent and 5 parts of acrylic resin film-forming agent and continue to stir at a rate of 120 rpm / min for 20 minutes, the stirring temperature is 40 degrees Celsius, and a refrigeration film is obtained;
[0030] S3, add 10 parts of mica powder, 3 parts of vermiculite powder to water and mix, stir at a rate of 50rpm / min for 5 minutes, warm to 40 degrees Celsius, continue to add a mixture of 4 parts of polyacrylic acid and carboxymethyl cellulose, 8 parts of calcium carbonate, 5 parts of ethyl acetate under agitation, stir at a rate of 100rpm / min for 10 minutes, and obtain the second initial mixing;
[0031] S4, continue to raise the temperature to 50 degrees Celsius, add 3 parts of castor oil, 2 parts of a mixture of polyether, silicone oil and ethanol, and 2 parts of ethylenediamine (EDA) to the second primary mixture, stir at a rate of 150 rpm / min for 20-25 minutes, and then stand for 60 minutes to obtain a self-cleaning film;
[0032] S5. After evenly applying the cooling film to the surface of the substrate, a cooling layer is obtained. When the cooling layer is 70% dry, a self-cleaning film is continuously applied. After air drying, an optical radiation cooling coating with a self-cleaning function is obtained.
[0033] Example 2
[0034] S1, after mixing 30 parts of titanium dioxide and 30 parts of magnesium oxide, add them to 80 parts of water, then add 30 parts of polyvinylidene fluoride resin powder, 1.5 parts of titanium dioxide, and 1.5 parts of nano zinc oxide to the water, stir at 50 rpm / min for 5 minutes, and let stand for 10 minutes to obtain the first primary mixture;
[0035] S2, add 35 parts of aluminum oxide, 40 parts of silicon oxide, and 60 parts of water to the first primary mixture, stir at a rate of 100 rpm / min for 20 minutes, and then add 5 parts of fluorocarbon waterproofing agent and 8 parts of acrylic resin film-forming agent and continue to stir at a rate of 120 rpm / min for 20 minutes, the stirring temperature is 50 degrees Celsius, and a refrigeration film is obtained;
[0036] S3, add 15 parts of mica powder, 5 parts of vermiculite powder to water and mix, stir at a rate of 50rpm / min for 5 minutes, warm to 40 degrees Celsius, continue to add a mixture of 6 parts of polyacrylic acid and carboxymethyl cellulose, 10 parts of calcium carbonate, 7 parts of ethyl acetate under agitation, stir at a rate of 100rpm / min for 10 minutes, and obtain the second initial mixing;
[0037] S4, continue to raise the temperature to 50 degrees Celsius, add 5 parts of castor oil, 4 parts of a mixture of polyether, silicone oil and ethanol, and 3 parts of ethylenediamine (EDA) to the second primary mixture, stir at a rate of 150 rpm / min for 20-25 minutes, and then stand for 60 minutes to obtain a self-cleaning film;
[0038] S5. After evenly applying the cooling film to the surface of the substrate, a cooling layer is obtained. When the cooling layer is 70% dry, a self-cleaning film is continuously applied. After air drying, an optical radiation cooling coating with a self-cleaning function is obtained.
[0039] In order to prove the superiority of the present invention, comparative examples 1 to 3 are set up here.
[0040] Comparative Example 1
[0041] S1, after mixing 20 parts of titanium dioxide, 10 parts of magnesium oxide, and 10 parts of barium sulfate, add them to 100 parts of water, then add 45 parts of polyvinylidene fluoride resin powder and 1 part of titanium dioxide to the water, stir at 50 rpm / min for 5 minutes, and let stand for 10 minutes to obtain the first primary mixture;
[0042] S2, add 10 parts of aluminum oxide, 60 parts of silicon oxide, and 100 parts of water to the first primary mixture, stir at a rate of 100 rpm / min for 20 minutes, and then add 10 parts of fluorocarbon waterproofing agent and 3 parts of acrylic resin film-forming agent and continue to stir at a rate of 120 rpm / min for 20 minutes, the stirring temperature is 40 degrees Celsius, and a refrigeration film is obtained;
[0043] S3, add 5 parts of mica powder, 5 parts of vermiculite powder to water and mix, stir at a rate of 50rpm / min for 5 minutes, warm to 40 degrees Celsius, continue to add a mixture of 10 parts of polyacrylic acid and carboxymethyl cellulose, 5 parts of calcium carbonate, 3 parts of ethyl acetate under agitation, stir at a rate of 100rpm / min for 10 minutes, and obtain the second initial mixing;
[0044] S4, continue to raise the temperature to 50 degrees Celsius, continue to add 1 part of castor oil, 10 parts of a mixture of polyether, silicone oil and ethanol, and 6 parts of ethylenediamine (EDA) to the second primary mixture, stir at a rate of 150 rpm / min for 20-25 minutes, and then stand for 60 minutes to obtain a self-cleaning film;
[0045] S5. After evenly applying the cooling film to the surface of the substrate, a cooling layer is obtained. When the cooling layer is 70% dry, a self-cleaning film is continuously applied. After air drying, an optical radiation cooling coating with a self-cleaning function is obtained.
[0046] The raw material ratio of Comparative Example 1 exceeds the ratio within the scope of this application.
[0047] Comparative Example 2
[0048] S1, after mixing 50 parts of titanium dioxide, add it to 80 parts of water, then add 20 parts of polyvinylidene fluoride resin powder, 1 part of titanium dioxide, and 2 parts of nano zinc oxide to the water, stir at 50 rpm / min for 5 minutes, and let it stand for 10 minutes to obtain the first primary mixture;
[0049] S2, adding 10 parts of silicon oxide and 50 parts of water to the first premix, stirring at a rate of 100 rpm / min for 20 minutes, and then adding 5 parts of acrylic resin film-forming agent and continuing to stir at a rate of 120 rpm / min for 20 minutes, the stirring temperature is 40 degrees Celsius, to obtain a refrigeration film;
[0050] S3, add 15 parts of mica powder to the water, mix well, stir at a rate of 50rpm / min for 5 minutes, raise the temperature to 40 degrees Celsius, continue to add 5 parts of polyacrylic acid, 3 parts of calcium carbonate, and 12 parts of ethyl acetate under stirring, stir at a rate of 100rpm / min for 10 minutes to obtain a second primary mixture;
[0051] S4, continue to raise the temperature to 50 degrees Celsius, continue to add 7 parts of castor oil, 5 parts of a mixture of polyether, silicone oil and ethanol, and 10 parts of ethylenediamine (EDA) to the second primary mixture, stir at a rate of 150 rpm / min for 20-25 minutes, and then stand for 60 minutes to obtain a self-cleaning film;
[0052] S5. After evenly applying the cooling film to the surface of the substrate, a cooling layer is obtained. When the cooling layer is 70% dry, a self-cleaning film is continuously applied. After air drying, an optical radiation cooling coating with a self-cleaning function is obtained.
[0053] When preparing Comparative Example 2, not all the proportions of the present application were adopted.
[0054] Comparative Example 3
[0055] S1. Mix 50 parts of titanium dioxide and add it to 80 parts of water. Then add 20 parts of polyvinylidene fluoride resin powder, 1 part of titanium dioxide and 2 parts of nano zinc oxide to the water, stir at 20 rpm / min at 40 degrees Celsius for 5 minutes, and let stand for 10 minutes to obtain the first primary mixture.
[0056] S2, adding 10 parts of silicon oxide and 50 parts of water to the first premix, stirring at a rate of 100 rpm / min for 20 minutes, and then adding 5 parts of acrylic resin film-forming agent and continuing to stir at a rate of 120 rpm / min for 20 minutes, the stirring temperature is 70 degrees Celsius, to obtain a refrigeration film;
[0057] S3, add 15 parts of mica powder to water, mix well, stir at a rate of 30rpm / min for 5 minutes, raise the temperature to 70 degrees Celsius, continue to add 5 parts of polyacrylic acid, 3 parts of calcium carbonate, and 12 parts of ethyl acetate under stirring, stir at a rate of 70rpm / min for 10 minutes to obtain a second primary mixture;
[0058] S4, continue to raise the temperature to 100 degrees Celsius, continue to add 7 parts of castor oil, 5 parts of a mixture of polyether, silicone oil and ethanol, and 10 parts of ethylenediamine (EDA) to the second primary mixture, stir at a rate of 80 rpm / min for 20-25 minutes, and then stand for 60 minutes to obtain a self-cleaning film;
[0059] S5. After evenly applying the cooling film to the surface of the substrate, a cooling layer is obtained. When the cooling layer is 70% dry, a self-cleaning film is continuously applied. After air drying, an optical radiation cooling coating with a self-cleaning function is obtained.
[0060] The conditions such as rotation speed, temperature, time, etc. during the preparation of Comparative Example 3 are different from the limited conditions of the present application.
[0061] The self-cleaning refrigeration coatings prepared in Examples 1-2 and Comparative Examples 1-3 were attached to the surface of the substrate under constant sunlight conditions. Three groups were set up and the performance test was carried out after 5 hours. The test results are shown in Tables 1-3 below:
[0062] Table 1
[0063]
[0064] Table 2
[0065]
[0066]
[0067] Table 3
[0068]
[0069] It can be seen from Tables 1 to 3 that the self-cleaning radiation cooling coating prepared by Examples 1 and 2 of the present application has excellent light reflectivity, and can achieve a good cooling effect after being attached to the surface of the substrate. It also has a good self-cleaning effect after rain and dust layer are attached in a simulated natural environment, and basically no marks are left on the surface. When comparative example 1 was prepared, the raw materials were not within the scope of the present application, the raw materials used in comparative example 2 were different from those of the present application, and the parameter conditions used in comparative example 3 were different from those of the present application, so the three could not achieve the effect of the present application.
[0070] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.
Claims
1. A self-cleaning nano-optical radiation cooling coating, characterized in that: The refrigeration coating is composed of a bottom refrigeration layer and an upper self-cleaning layer, and the bottom refrigeration layer is composed of 120-160 parts of water, 60-80 parts of hydrophilic material, 5-10 parts of film-forming agent, 3-7 parts of color additive, 3-7 parts of waterproofing agent, 20-30 parts of polyvinylidene fluoride resin powder, and 50-70 parts of filler by weight; In parts by weight: the upper self-cleaning layer is composed of 20-30 parts of water, 3-5 parts of castor oil, 10-15 parts of mica powder, 3-5 parts of vermiculite powder, 4-6 parts of leveling agent, 2-4 parts of defoaming agent, 2-4 parts of curing agent, 8-15 parts of calcium carbonate, and 5-8 parts of ethyl acetate; The hydrophilic material of the bottom cooling layer is composed of aluminum oxide, silicon oxide, zirconium oxide, and quartz; the film-forming agent is an acrylic resin film-forming agent, which is a multi-polymer of acrylic ester, acrylonitrile, and acrylamide; the color additive is composed of one or more of titanium dioxide, nano zinc oxide, iron oxide red, and phthalocyanine blue; the waterproofing agent is a fluorocarbon waterproofing agent; the filler is a metal filler, which is composed of two or more of titanium dioxide, magnesium oxide, and barium sulfate; The method for preparing the self-cleaning nano-optical radiation refrigeration coating comprises the following steps: S1, adding filler, polyvinylidene fluoride resin powder and pigment additive into water, stirring to obtain the first primary mixture, and letting it stand; S2, continue to add water and hydrophilic material to the first primary mixture and stir, and then add waterproofing agent and film-forming agent and stir to obtain a refrigeration film; S3, adding mica powder and vermiculite powder to water and mixing, and then adding leveling agent, calcium carbonate and ethyl acetate under stirring to obtain a second primary mixture; S4, continue to add castor oil, defoamer and curing agent to the second primary mixture, and after standing, obtain a self-cleaning film; S5, after evenly applying the refrigeration film on the surface of the substrate, a refrigeration layer is obtained, and then the self-cleaning film is covered on the refrigeration layer, and after air drying, a self-cleaning nano-optical radiation refrigeration coating is obtained; The total dry film thickness of the bottom refrigeration layer and the upper self-cleaning layer when in use is no more than 1.5 mm.
2. The self-cleaning nano-optical radiation cooling coating according to claim 1, characterized in that: The leveling agent in the upper self-cleaning layer is composed of two or more of polyacrylic acid, carboxymethyl cellulose and silicone oil; the defoaming agent is composed of polyether, silicone oil and ethanol; and the curing agent is ethylenediamine (EDA).
3. The self-cleaning nano-optical radiation cooling coating according to claim 1, characterized in that: The particle size of the filler is 7-12 μm; the particle size of the polyvinylidene fluoride resin powder is 0.5-5 μm.
4. The self-cleaning nano-optical radiation cooling coating according to claim 1, characterized in that: The stirring speed in step S1 is 50-70 rpm, the stirring time is 5-7 minutes, and the stirring temperature is room temperature; the stirring speed in step S2 is 100-120 rpm, the stirring time is 20-30 minutes, and the stirring temperature is 40-50 degrees Celsius.
5. The self-cleaning nano-optical radiation cooling coating according to claim 1, characterized in that: In the step S3, the mica powder and the vermiculite powder are first stirred at 50-60 rpm for 5-7 minutes at room temperature, and after the leveling agent, calcium carbonate and ethyl acetate are added, they are stirred at 40-45 degrees Celsius at a speed of 100-150 rpm for 10-15 minutes; in the step S4, the temperature when the castor oil, the defoamer and the curing agent are added is 50-70 degrees Celsius, the rotation speed is 150-200 rpm, and the stirring time is 20-25 minutes.
Citation Information
Patent Citations
Refrigeration film
CN111808312A
Passive radiation refrigeration coating and preparation method and coating structure thereof
CN113292874A