A smelting method for increasing the scrap ratio in converters
By adding carbon source and scrap steel into the converter, carbon dioxide reacts with the carbon source to generate carbon monoxide, which then burns with oxygen to release heat. This solves the problem of low scrap steel ratio in the converter, achieves efficient scrap steel preheating, and reduces smelting costs and environmental pollution.
Patent Information
- Application Number
- CN202311873458.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-30
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-30
AI Technical Summary
The low scrap ratio in existing converters leads to high smelting costs, severe environmental pollution, and high energy consumption, and also makes equipment modification difficult.
Carbon source and scrap steel are added into the converter. Carbon dioxide is blown from the bottom and oxygen is blown from the top to preheat the scrap steel. The carbon source reacts with carbon dioxide to generate carbon monoxide, which then burns with oxygen to release heat and increase the temperature of the scrap steel.
Without increasing equipment investment, scrap steel preheating was achieved through process adjustments, which increased the scrap steel ratio, reduced smelting costs and environmental pollution, and saved space.
Smart Images

Figure CN117821690B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of converter steelmaking technology, specifically relating to a smelting method for increasing the scrap ratio in converters. Background Technology
[0002] Converter smelting uses molten iron, scrap steel, and ferroalloys as main raw materials. Without the aid of external energy, it relies on the physical heat of the molten iron itself and the heat generated by chemical reactions between its components to complete the steelmaking process in the converter. With the increase in my country's steel reserves, the supply of scrap steel for converter smelting has been increasing year by year. Increasing the amount of scrap steel added to the converter can reduce CO2 emissions per ton of steel, lower converter smelting costs, and significantly reduce environmental pollution and overall energy consumption per ton of steel. Therefore, researchers have begun to study how to increase the scrap steel ratio in converter smelting.
[0003] In related technologies, the main method to increase the scrap steel ratio in converter smelting is to use existing production lines to install simple equipment for scrap steel preheating. For example, before the scrap steel is added to the converter, it is first baked by baking equipment for a specified time and then sent into the converter by the scrap steel hopper. The equipment modification is difficult and requires a large area. Summary of the Invention
[0004] To address the current technical problem of low scrap ratio in converters, this application provides a smelting method for increasing the scrap ratio in converters.
[0005] In a first aspect of this application, a smelting method for increasing the scrap ratio in a converter is provided, comprising the following steps:
[0006] Carbon source and scrap steel are added into the converter, followed by bottom blowing of carbon dioxide and top blowing of oxygen to preheat the scrap steel and obtain heated scrap steel.
[0007] Molten iron is added to a converter containing the heated scrap steel for blowing to increase the scrap steel ratio.
[0008] In some embodiments, the amount of carbon source added is 2-8% of the nominal capacity of the converter.
[0009] In some embodiments, the particle size of the carbon source is 10 mm to 20 mm.
[0010] In some embodiments, the amount of scrap steel added is 40% to 60% of the nominal capacity of the converter.
[0011] In some embodiments, the maximum length of the scrap steel is ≤2m and the thickness of the scrap steel is ≤30mm.
[0012] In some embodiments, when the nominal capacity of the converter is 200t to 300t, the amount of scrap steel added is 80t to 120t, and the amount of carbon source added is 5t to 15t.
[0013] In some embodiments, the top-blown oxygen intensity when the scrap steel preheating time t ≤ 3 min is less than the top-blown oxygen intensity when the scrap steel preheating time t > 3 min; and the bottom-blown carbon dioxide intensity when the scrap steel preheating time t ≤ 3 min is less than the bottom-blown carbon dioxide intensity when the scrap steel preheating time t > 3 min.
[0014] In some embodiments, the top-blown oxygen intensity is 1.5–2.0 Nm³ when the scrap steel preheating time t ≤ 3 min. 3 / min / t, the top-blown oxygen intensity when the preheating time t of the scrap steel is greater than 3 min is 2.0~2.5 Nm. 3 / min / t.
[0015] In some embodiments, the bottom-blown carbon dioxide intensity is 0.08–0.12 Nm when the scrap steel preheating time t ≤ 3 min. 3 / min / t, the intensity of bottom-blown carbon dioxide when the preheating time t of the scrap steel is greater than 3 min is 0.12~0.20 Nm. 3 / min / t.
[0016] In some embodiments, the preheating time of the scrap steel is 8 min to 12 min.
[0017] A smelting method for increasing the scrap ratio in a converter, according to an embodiment of this application, includes the following steps: carbon source and scrap steel are sequentially added to the converter; then, carbon dioxide is blown from the bottom and oxygen from the top to preheat the scrap steel, obtaining heated scrap steel; molten iron is added to the converter containing the heated scrap steel for smelting, thereby increasing the scrap ratio. This application, without increasing equipment investment, adds the carbon source and scrap steel to the converter before adding molten iron. The carbon dioxide gas blown from the bottom of the converter reacts chemically with the carbon in the carbon source to form carbon monoxide, which has a volume twice that of carbon dioxide. This CO gas can fully fill the gaps between the scrap steel pieces added to the converter, thoroughly enveloping the scrap steel. The oxygen blown from the top of the converter reacts with the carbon monoxide surrounding the scrap steel, releasing heat through combustion, and also directly burns with the carbon source, releasing heat, thus uniformly preheating the scrap steel to form heated scrap steel. The high temperature of the heated scrap steel allows it to fully melt and form molten steel during the smelting process.
[0018] Compared with existing technologies, this application increases the proportion of scrap steel produced in the converter by adding a carbon source into the converter and bottom-blowing carbon dioxide and top-blowing oxygen. The bottom-blown carbon dioxide reacts with the carbon source to form carbon monoxide, and the top-blown oxygen reacts with the carbon monoxide, releasing heat to preheat the scrap steel. This application only requires process adjustments, without modifying the converter equipment, saving costs and requiring no additional space. Attached Figure Description
[0019] Figure 1The diagram illustrates the process steps of a smelting method for increasing the scrap ratio in a converter, according to one or more embodiments of this application. Detailed Implementation
[0020] To enable those skilled in the art to more clearly understand this application, the technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0021] This application provides a smelting method for increasing the scrap ratio in a converter. This smelting method increases the scrap ratio in the converter by preheating the scrap steel through process adjustment, without requiring equipment modification, saving costs, and without occupying additional space.
[0022] Figure 1 A process flow diagram illustrating the smelting method for increasing the scrap ratio in converters is shown. Please refer to [link / reference needed]. Figure 1 The smelting method for increasing the scrap ratio in converters provided in this application includes the following steps:
[0023] S1. Carbon source and scrap steel are added into the converter in sequence, followed by bottom blowing of carbon dioxide and top blowing of oxygen to preheat the scrap steel and obtain heated scrap steel.
[0024] S2. Add molten iron to a converter containing the heated scrap steel and blow it to increase the scrap steel ratio.
[0025] A carbon source is a material with carbon as its main component, such as carbon powder, coal powder, graphite powder, coke, or coke powder. The carbon in the carbon source reacts chemically with the carbon dioxide blown in from the bottom of the converter to produce carbon monoxide, which has twice the volume of carbon dioxide. This CO gas can fully fill the gaps between the scrap steel pieces added to the converter, thoroughly encapsulating the scrap steel. It then reacts with the oxygen blown in from the top of the converter in a combustion reaction, releasing heat and improving the uniformity of scrap steel preheating. Because the volume of carbon monoxide is larger than that of the bottom-blown carbon dioxide, the heat released in the combustion reaction is greater, resulting in better scrap steel preheating. The carbon source can also directly react with the top-blown oxygen in a combustion reaction, further improving the scrap steel preheating efficiency.
[0026] Because scrap steel was added to the converter in the first half of the process, even with preheating from the previous furnace, the furnace temperature was still relatively low. Only a very small portion of the carbon dioxide blown in from the bottom reacted with the carbon source; at this stage, the carbon dioxide mainly served to agitate the carbon source, facilitating its combustion and exothermic reaction with the oxygen blown in from above. As the exothermic oxidation reaction between the carbon source and oxygen progressed, the furnace temperature rose in the second half of the process. The carbon dioxide then reacted with the carbon source to form carbon monoxide, which had twice the volume of carbon dioxide. This carbon monoxide then reacted with oxygen to release a large amount of heat, rapidly preheating the scrap steel in a short time.
[0027] The carbon source is added to the converter first, followed by the scrap steel. This creates a layered structure with the carbon source at the bottom and the scrap steel at the top, allowing the carbon source to react quickly and fully with the carbon dioxide gas blown in from the bottom of the converter. Furthermore, this order of adding the carbon source first, then the scrap steel, ensures that the lighter carbon source is pressed down by the scrap steel, preventing it from scattering and wasting when carbon dioxide is blown in from the bottom, thus avoiding waste and ensuring proper preheating of the scrap steel. Because the carbon source is at the bottom and the scrap steel is at the top, bottom-blown carbon dioxide gas is more conducive to a rapid reaction between the carbon source and carbon dioxide.
[0028] In some embodiments, the amount of carbon source added is 2-8% of the nominal capacity of the converter. Since the nominal capacity of the converter is limited, adding too much carbon source can preheat more scrap steel to some extent, but it will reduce the amount of molten iron charged and lower the final converter temperature. Adding too little carbon source will reduce the scrap steel ratio in the converter to some extent.
[0029] In some embodiments, the particle size of the carbon source is 10mm to 20mm. If the particle size of the carbon source is too large, it will affect the reaction efficiency between the carbon source and carbon dioxide to a certain extent, prolong the preheating time of scrap steel, and affect production efficiency. If the particle size of the carbon source is too small, it is more likely to drift upwards to a certain extent, which will also reduce the reaction efficiency between the carbon source and carbon dioxide and prolong the preheating time of scrap steel.
[0030] In some embodiments, the amount of scrap steel added is 40% to 60% of the nominal capacity of the converter. Adding too much scrap steel will, to some extent, lower the converter's final temperature. Adding too little scrap steel will, to some extent, lower the scrap ratio.
[0031] In some embodiments, the maximum length of the scrap steel is ≤2m, and the thickness of the scrap steel is ≤30mm. Scrap steel is generally steel plate, steel block, etc., and its maximum length generally does not exceed 2m, and its thickness does not exceed 30mm. If the length and thickness of the scrap steel are too large, it will increase the melting difficulty during the smelting process and reduce the final temperature of the converter.
[0032] Generally, the nominal capacity of the converter is 150-300t. In some embodiments, when the nominal capacity of the converter is 200t-300t, the amount of scrap steel added can be 80t-120t, and the amount of carbon source added can be 5t-15t.
[0033] In some embodiments, the top-blown oxygen intensity when the scrap preheating time t ≤ 3 min is less than the top-blown oxygen intensity when the scrap preheating time t > 3 min. That is, the top-blown oxygen intensity in the first half of the scrap preheating process is less than the top-blown oxygen intensity in the second half. This is because the carbon source and scrap temperature are both lower in the first half, requiring a small amount of top-blown oxygen to allow the oxygen to react with the carbon source. Simultaneously, bottom-blown carbon dioxide can disturb the carbon source, allowing it to also react with oxygen. Due to the low temperature inside the converter in the first half, only a very small amount of carbon dioxide reacts with carbon to form carbon dioxide; the main reaction is the exothermic combustion reaction between the carbon source and oxygen. As the combustion reaction between the carbon source and oxygen proceeds, the temperature of the carbon source and scrap steel inside the converter gradually increases. In the latter half of the process, the temperature inside the converter has risen to a certain level. Increasing the intensity of top-blown oxygen can further promote the combustion and exothermic reaction between oxygen and carbon source. Moreover, the high temperature inside the furnace at this time also promotes the reaction between carbon dioxide and carbon source to generate carbon monoxide. The carbon monoxide formed moves upward and surrounds the scrap steel above. The carbon monoxide then reacts with oxygen to generate heat quickly and preheat the scrap steel.
[0034] In some embodiments, the top-blown oxygen intensity is 1.5–2.0 Nm when the preheating time of the scrap steel is ≤3 min. 3 / min / t, the top-blown oxygen intensity when the preheating time t of the scrap steel is greater than 3 min is 2.0~2.5 Nm. 3 / min / t, meaning the top-blown oxygen intensity in the first half is 1.5–2.0 Nm³. 3 / min / t, the top-blown oxygen intensity in the latter half is 2.0~2.5Nm 3 / min / t.
[0035] In some embodiments, during the preheating of the scrap steel, the intensity of bottom-blown carbon dioxide is 0.1–0.2 Nm. 3 / min / t.
[0036] In some embodiments, the preheating time of the scrap steel is 8 min to 12 min, for example 9 min, 10 min or 11 min.
[0037] Additionally, it needs to be explained that the scrap ratio refers to the ratio of the scrap steel added to the converter to the sum of the scrap steel and molten iron added to the converter, that is, the scrap ratio equals scrap steel / (scrap steel + molten iron).
[0038] The following will describe in detail, with reference to specific embodiments, a smelting method for increasing the scrap ratio in a converter provided in this application.
[0039] Example 1
[0040] Example 1 provides a smelting method for increasing the scrap ratio in a converter. The smelting is carried out in a converter with a nominal capacity of 210t, and the specific smelting steps are as follows:
[0041] (1) After the previous slag splashing protection is completed, 6 tons of coke with a particle size range of 10-20mm are added into the converter, followed by 87 tons of scrap steel. CO2 is blown in from the bottom and oxygen is blown in from the top to start the smelting process for 10 minutes to preheat the scrap steel. The smelting mode is controlled as follows:
[0042] During the first 3 minutes of blowing, the oxygen supply intensity from the top blown oxygen was 1.7 Nm. 3 The bottom-blown CO2 intensity is 0.11 Nm³ / min / t. 3 / min / t; During the 3-10 min blowing time, the bottom-blown CO2 intensity is 0.14 Nm. 3 / min / t, increase the top-blown oxygen supply intensity to 2.3Nm 3 / min / t.
[0043] After blowing for 10 minutes, the temperature of the scrap steel in the converter was measured to be 903℃.
[0044] (2) Add 130t of molten iron and slag-forming material to the converter after the treatment in step 1, and carry out converter blowing. During converter blowing, the bottom-blown gas is Ar gas, and the bottom-blown intensity is 0.13 Nm. 3 / min / t, with oxygen as the top-blown gas, increasing the oxygen supply intensity to 3.6 Nm. 3 / min / t;
[0045] (3) After the composition is qualified, the converter tapping operation is carried out.
[0046] In the smelting method provided in Example 1, the scrap steel ratio in the converter is 40.1%.
[0047] Example 2
[0048] Example 2 provides a smelting method for increasing the scrap ratio in a converter. The smelting is carried out in a converter with a nominal capacity of 300t, and the specific smelting steps are as follows:
[0049] (1) After the previous slag splashing protection is completed, 15 tons of coke with a particle size range of 10-20mm is added to the converter, followed by 120 tons of scrap steel. CO2 is blown in from the bottom and oxygen is blown in from the top to start the smelting process for 10 minutes to preheat the scrap steel. The smelting mode is controlled as follows:
[0050] During the first 3 minutes of blowing, the oxygen supply intensity from the top blown oxygen was 1.8 Nm. 3 / min / t, bottom-blown CO2 intensity is 0.09 Nm 3 / min / t; During the 3-10 min blowing time, the bottom-blown CO2 intensity is 0.17 Nm. 3 / min / t, increase the top-blown oxygen supply intensity to 2.4Nm 3 / min / t.
[0051] After blowing for 10 minutes, the temperature of the scrap steel in the converter was measured to be 906℃.
[0052] (2) Add 180t of molten iron and slag-forming material to the converter after the treatment in step 1, and carry out converter blowing. During converter blowing, the bottom-blown gas is Ar gas, and the bottom-blown intensity is 0.14 Nm. 3 / min / t, with oxygen as the top-blown gas, increasing the oxygen supply intensity to 3.7 Nm. 3 / min / t;
[0053] (3) After the composition is qualified, the converter tapping operation is carried out.
[0054] In the smelting method provided in Example 2, the converter scrap ratio is 40.0%.
[0055] Example 3
[0056] Example 3 provides a smelting method for increasing the scrap ratio in a converter. The smelting is carried out in a converter with a nominal capacity of 260t. The specific smelting steps are as follows:
[0057] (1) After the previous slag splashing protection is completed, 16 tons of coke with a particle size range of 10-18mm is added to the converter, followed by 118 tons of scrap steel. CO2 is blown in from the bottom and oxygen is blown in from the top to start the smelting process for 9 minutes to preheat the scrap steel. The smelting mode is controlled as follows:
[0058] During the first 3 minutes of blowing, the oxygen supply intensity from the top blown oxygen was 1.6 Nm. 3 / min / t, bottom-blown CO2 intensity is 0.10 Nm 3 / min / t; During the 3-9 min blowing time, the bottom-blown CO2 intensity is 0.19 Nm. 3 / min / t, increase the top-blown oxygen supply intensity to 2.2Nm 3 / min / t.
[0059] When the blowing process reached 9 minutes, the temperature of the scrap steel in the converter was measured to be 904℃.
[0060] (2) Add 144t of molten iron and slag-forming material to the converter after the treatment in step 1, and carry out converter blowing. During converter blowing, the bottom-blown gas is Ar gas, and the bottom-blown intensity is 0.14 Nm. 3 / min / t, with oxygen as the top-blown gas, increasing the oxygen supply intensity to 3.7 Nm. 3 / min / t;
[0061] (3) After the composition is qualified, the converter tapping operation is carried out.
[0062] Example 4
[0063] Example 4 provides a smelting method to increase the scrap ratio in a converter. The smelting method of Example 3 is used as a reference. The difference between Example 4 and Example 3 is that in step (1), the amount of coke and scrap added, the oxygen supply intensity in the first half stage and the oxygen supply intensity in the second half stage, and the intensity of bottom blowing carbon dioxide are as detailed in Table 1.
[0064] Example 5
[0065] Example 5 provides a smelting method to increase the scrap ratio in a converter. The smelting method of Example 3 is used as a reference. The difference between Example 5 and Example 3 is that in step (1), the amount of coke and scrap added, the oxygen supply intensity in the first half stage and the oxygen supply intensity in the second half stage, the intensity of bottom blowing carbon dioxide, and the scrap preheating time are all specified in Table 1.
[0066] Table 1
[0067] Table 2
[0068] As can be seen from the data in Table 2, the smelting method for increasing the scrap ratio in converters provided in this application has a high preheating temperature of 902-906℃, a preheating time of 8-12 minutes, and high preheating efficiency, increasing the scrap ratio to 40%-51.7%.
[0069] The smelting method for increasing the scrap ratio in converters provided in this application involves sequentially adding a carbon source and scrap steel into the converter. In the first half of the preheating stage, the primary reaction is an exothermic combustion reaction between oxygen and the carbon source, providing the temperature conditions for the formation of a large amount of carbon monoxide in the second half of the preheating stage. In the second half of the preheating stage, the furnace temperature is higher, and the intensity of bottom-blown carbon dioxide increases. Carbon dioxide reacts extensively with the carbon source to form carbon monoxide, while the intensity of top-blown oxygen also increases. A large amount of oxygen reacts with carbon monoxide in an exothermic oxidation reaction. Due to the high heat release of this reaction, the scrap steel can be rapidly heated, achieving comprehensive and rapid heating of the scrap steel. The scrap steel can be preheated to over 900°C in just a few minutes, increasing the scrap ratio to 40%-51.7%, thus solving the problem of insufficient heat in smelting with a high scrap ratio.
[0070] Compared with existing technologies, this application increases the proportion of scrap steel produced in the converter by adding a carbon source into the converter and bottom-blowing carbon dioxide and top-blowing oxygen. The bottom-blown carbon dioxide reacts with the carbon source to form carbon monoxide, and the top-blown oxygen reacts with the carbon monoxide, releasing heat to preheat the scrap steel. This application only requires process adjustments, without modifying the converter equipment, saving costs and requiring no additional space.
[0071] In this application, unless otherwise expressly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature being directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature being directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.
[0072] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", and "counterclockwise" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.
[0073] In this application, unless otherwise expressly specified and limited, the terms "connection," "fixed," etc., should be interpreted broadly. For example, "fixed" can mean a fixed connection, a detachable connection, or an integral part; it can mean a mechanical connection or an electrical connection; it can mean a direct connection or an indirect connection through an intermediate medium; it can mean the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.
[0074] Furthermore, the use of terms such as "first" and "second" in this application is for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, features defined with "first" or "second" may explicitly or implicitly include one or more features. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.
[0075] Although embodiments of this application have been shown and described, those skilled in the art will understand that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of this application, the scope of which is defined by the claims and their equivalents.
Claims
1. A smelting method for increasing the scrap ratio in a converter, characterized in that, Includes the following steps: Carbon source and scrap steel are sequentially added into the converter, followed by bottom blowing of carbon dioxide and top blowing of oxygen to preheat the scrap steel, obtaining heated scrap steel. The amount of carbon source added is 2-8% of the nominal capacity of the converter; the particle size of the carbon source is 10mm-20mm; the amount of scrap steel added is 40%-60% of the nominal capacity of the converter; the preheating time of the scrap steel is 8min-12min; the top blowing oxygen intensity when the scrap steel preheating time t≤3min is less than the top blowing oxygen intensity when the scrap steel preheating time t>3min; the top blowing oxygen intensity when the scrap steel preheating time t≤3min is 1.5-2.0Nm³. 3 / min / t, the top-blown oxygen intensity when the preheating time t>3min is 2.0~2.5Nm 3 / min / t; the bottom-blown carbon dioxide intensity when the scrap steel preheating time t≤3min is less than the bottom-blown carbon dioxide intensity when the scrap steel preheating time t>3min; the bottom-blown carbon dioxide intensity when the scrap steel preheating time t≤3min is 0.08~0.12Nm 3 / min / t, the intensity of bottom-blown carbon dioxide when the preheating time t of the scrap steel is greater than 3 min is 0.12~0.20 Nm. 3 / min / t; Molten iron is added to a converter containing the heated scrap steel for blowing to increase the scrap steel ratio.
2. The smelting method for increasing the scrap ratio in a converter according to claim 1, characterized in that, The maximum length of the scrap steel is ≤2m, and the thickness of the scrap steel is ≤30mm.
3. The smelting method for increasing the scrap ratio in a converter according to any one of claims 1-2, characterized in that, When the nominal capacity of the converter is 200t~300t, the amount of scrap steel added is 80t~120t, and the amount of carbon source added is 5t~15t.
Citation Information
Patent Citations
Method for preheating waste steel in converter
CN117004790A