A method for non-destructive testing of soldering depth of lead-acid battery terminals

By creating pre-drilled holes in the sidewall of the lead pipe and combining them with pressure testing, the problem of low efficiency and poor reliability in the existing lead-acid battery terminal welding depth detection has been solved. This achieves efficient and low-cost non-destructive testing, improving battery quality and safety.

CN117825141BActive Publication Date: 2026-11-17FENGFAN
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311662878.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-06
Publication Date
2026-11-17
Estimated Expiration
2043-12-06

AI Technical Summary

Technical Problem

Existing methods for detecting the welding depth of lead-acid battery terminals are inefficient, unreliable, costly, and difficult to operate, making them unsuitable for full product inspection requirements and affecting battery reliability and safety.

Method used

A pre-drilled hole is made laterally on the side wall of the lead pipe. After the lead pipe and the battery cover are injection molded, they are welded together. A metal probe is heated and pressed into the lead pipe and the terminal post. The pressure change is monitored by pressure testing to determine whether the welding depth meets the requirements.

Benefits of technology

This technology enables non-destructive testing of the welding depth of lead-acid battery terminals, improving testing efficiency and reliability, reducing testing costs, making it suitable for full product inspection, and enhancing battery quality and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117825141B_ABST
    Figure CN117825141B_ABST
Patent Text Reader

Abstract

This invention provides a method for non-destructive testing of the welding depth of lead-acid battery terminals, belonging to the field of battery testing technology. The method includes the following steps: S1: Pre-drilling holes in the side wall of a lead pipe; S2: Injection molding of the lead pipe and battery cover in an injection mold; S3: Passing the terminal post through the lead pipe from bottom to top; S4: Heating and pressing a metal probe into the interior of the lead pipe and terminal post to form the welded battery terminals; S5: Performing a pressure test on the individual cells containing the terminals on both sides of the battery to monitor pressure changes. This invention provides a method for non-destructive testing of the welding depth of lead-acid battery terminals. By improving the lead pipe structure and adjusting the welding process, and by using a pressure test to detect the welding depth, it overcomes the problems of low efficiency, poor reliability, high testing cost, and difficult operation of existing testing methods, thereby improving product quality and service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery testing technology, and more specifically, relates to a method for non-destructive testing of the welding depth of lead-acid battery terminals. Background Technology

[0002] Automotive lead-acid batteries are electrical energy output and storage devices in vehicles. The battery is connected to the vehicle through positive and negative terminals on the battery and positive and negative terminals on the vehicle to transfer electrical energy. The quality of the terminals affects the battery's charging and discharging performance, as well as the safety of the vehicle and its occupants.

[0003] Lead-acid battery terminals are made by fusing lead tubes and terminal posts made of lead-based alloy material through high-temperature welding (acetylene + oxygen + high-temperature metal probe). The welding depth of the terminal is a critical dimension. If it does not meet the requirements, the connection between the terminal and the top of the car terminal clamp will be weak. When the clamp is tightened, it will damage the terminal and cause cracks, resulting in sulfuric acid leakage from the battery, corrosion of vehicle parts, and in severe cases, threats to personal safety.

[0004] Currently, there are two main types of methods for detecting the soldering depth of terminals:

[0005] The first type involves destructive dissection and testing using punch cutting or wire cutting methods, which is inefficient, unreliable, and results in a large amount of battery waste.

[0006] The second category is ultrasonic flaw detection technology. Although it does not damage the battery, the technology is not mature, and the equipment and testing costs are high. It is also difficult to operate and is not suitable for the requirement of full product inspection. Summary of the Invention

[0007] The purpose of this invention is to provide a method for non-destructive testing of the welding depth of lead-acid battery terminals, aiming to solve the problems of low efficiency, poor reliability, high testing cost, high operation difficulty, and unsuitability for full product inspection requirements in existing online terminal welding depth testing, thereby improving battery reliability and safety.

[0008] To achieve the above objectives, the technical solution adopted by the present invention is: to provide a method for non-destructive testing of the welding depth of lead-acid battery terminals, comprising the following steps:

[0009] S1: A pre-drilled hole is made horizontally at a distance X from the top of the lead pipe sidewall. The number of pre-drilled holes is at least two, and the interval between adjacent pre-drilled holes is 360° / number of holes.

[0010] S2: The lead pipe and the battery cover are injection molded in an injection mold. The battery cover wraps around the lower part of the lead pipe to form an integral part. The upper part of the lead pipe with pre-made holes is exposed above the battery cover.

[0011] S3: Use a heat sealer to weld the battery cover onto the battery case. The lead pipes of the two pole groups inside the battery case pass through the battery cover from bottom to top.

[0012] S4: The battery enters the terminal welding station. The terminal welding machine heats the metal probe with an acetylene flame. The metal probe is pressed down into the interior of the lead pipe and the terminal post to fuse the upper area of ​​the lead pipe and the terminal post to form the welded battery terminal.

[0013] S5: Perform a pressure test on the individual cells containing the terminals on both sides of the battery and monitor the pressure changes.

[0014] In one possible implementation, in step S5, a pressure test is performed on the individual cells where the terminals on both sides of the battery are located, with a pressure of 40kPa-50kPa and a holding time of 5s.

[0015] If the pressure difference change is ≤0.2kPa, the terminal welding depth meets the requirements, and the welding depth is ≥X;

[0016] If the pressure difference change is greater than 0.2 kPa, the terminal welding depth does not meet the requirements, and the welding depth is less than X.

[0017] If the pressure difference change is greater than 0.2 kPa and multiple batteries fail to meet the welding depth requirements, observe the appearance of the terminals at the pre-drilled holes. If the terminals are smooth and full, it indicates that the pressure testing equipment is malfunctioning. After adjusting the pressure testing equipment, perform the pressure test again.

[0018] In one possible implementation, X = 5mm-8mm, and the diameter of the pre-drilled hole is ≥1mm.

[0019] The beneficial effects of the non-destructive testing method for the welding depth of lead-acid battery terminals provided by this invention are as follows: Compared with the prior art, a pre-drilled hole is horizontally opened at a distance X from the top of the lead pipe sidewall, with at least two pre-drilled holes and an interval angle of 360° / number of holes between adjacent pre-drilled holes; the lead pipe and the battery cover are injection molded in an injection mold, with the battery cover wrapping around the lower part of the lead pipe to form an integral whole, and the upper part of the lead pipe with the pre-drilled hole exposed above the battery cover; the battery cover is welded to the battery cell using a heat sealing machine, and the terminal posts of the two electrode groups inside the battery cell pass through the lead pipe of the battery cover from bottom to top; the battery enters the terminal welding station, and the terminal welding machine heats the metal probe with an acetylene flame, pressing the metal probe down into the interior of the lead pipe and the terminal posts to fuse the upper areas of the lead pipe and the terminal posts to form the welded battery terminals; a pressure test is performed on the cell where the terminals on both sides of the battery are located, and the pressure change is monitored. This invention provides a method for non-destructive testing of the welding depth of lead-acid battery terminals. By improving the lead pipe structure and adjusting the welding process, and by using a pressure test method to detect the welding depth of the terminals, this method overcomes the problems of low efficiency, poor reliability, high testing cost, and high operation difficulty of the original testing methods, thereby improving product quality and service life. Attached Figure Description

[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 This is a schematic diagram of the structure of the metal probe, lead pipe and terminal electrode being heated by an acetylene flame in the initial state, as provided by the present invention.

[0022] Figure 2 A schematic diagram of the structure provided by the present invention, showing the metal probe being pressed into the lead pipe and the end electrode post;

[0023] Figure 3 This is a schematic diagram of the lead pipe structure provided by the present invention;

[0024] Figure 4 The state of the lead melt and the final terminal when the welding depth meets the requirements;

[0025] Figure 5 This shows the state of the lead melt and the final terminal when the soldering depth is insufficient.

[0026] Explanation of reference numerals in the attached figures:

[0027] 1. Lead pipe; 2. Pre-drilled hole; 3. Acetylene flame; 4. Metal probe; 5. Terminal welding ring; 6. Terminal post; 7. Lead liquid; 8. Terminal. Detailed Implementation

[0028] To make the technical problems to be solved, the technical solutions, and the beneficial effects of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the present invention and are not intended to limit the present invention.

[0029] Please see Figures 1 to 4 The present invention will now describe a method for non-destructive testing of the welding depth of lead-acid battery terminals. A method for non-destructive testing of the welding depth of lead-acid battery terminals includes the following steps:

[0030] S1: A pre-drilled hole 2 is made laterally on the side wall of the lead pipe 1 at a distance of X from the top. The number of pre-drilled holes 2 is at least two, and the interval angle between adjacent pre-drilled holes 2 is 360° / number of holes.

[0031] S2: The lead pipe 1 and the battery cover are injection molded in an injection mold. The battery cover wraps around the lower part of the lead pipe 1 to form an integral part. The upper part of the lead pipe 1 with pre-made holes 2 is exposed above the battery cover.

[0032] S3: Use a heat sealer to weld the battery cover onto the battery case. The lead pipe 1 of the battery cover passes through the two pole group terminals 6 on both sides of the battery case from bottom to top.

[0033] S4: The battery enters the terminal welding station. The terminal welding machine heats the metal probe 4 with an acetylene flame 3. The metal probe 4 is pressed down into the interior of the lead pipe 1 and the terminal post 6 to fuse the upper area of ​​the lead pipe 1 and the terminal post 6 to form the welded battery terminal 8.

[0034] S5: Perform a pressure test on the cells containing terminals 8 on both sides of the battery. The pressure should be 40kPa-50kPa, and the holding time should be 5s. The pressure difference should be ≤0.2kPa. If the pressure difference is ≤0.2kPa, i.e., the welding depth is ≥x (mm), the welding quality meets the requirements, and there will be no air leakage at the battery terminal 8. If the pressure difference is >0.2kPa, i.e., the welding depth is <x (mm), the welding quality does not meet the requirements, and a passage is formed between the inside and outside of the battery terminal 8, which cannot form a seal and leads to air leakage.

[0035] This invention provides a method for non-destructive testing of the welding depth of lead-acid battery terminals. Compared with the prior art, a pre-drilled hole 2 is horizontally opened at a distance X from the top of the lead pipe 1. The number of pre-drilled holes 2 is at least two, and the interval angle between adjacent pre-drilled holes 2 is 360° / number of holes. The lead pipe 1 and the battery cover are injection molded in an injection mold. The battery cover wraps around the lower part of the lead pipe 1 to form an integral whole, and the upper part of the lead pipe 1 with the pre-drilled hole 2 is exposed above the battery cover. The battery cover is welded to the battery cell using a heat sealing machine. The terminal posts 6 of the two side groups of the battery cell pass through the lead pipe 1 of the battery cover from bottom to top. The battery enters the terminal welding station. The terminal welding machine heats the metal probe 4 with an acetylene flame 3. The metal probe 4 is pressed down into the interior of the lead pipe 1 and the terminal posts 6 to fuse the upper areas of the lead pipe 1 and the terminal posts 6 to form the welded battery terminal 8. A pressure test is performed on the cell where the terminals 8 of the battery are located to monitor the pressure change. This invention provides a method for non-destructive testing of the welding depth of lead-acid battery terminals. By improving the structure of the lead pipe 1 and adjusting the welding process, and by using a pressure test method, the welding depth of the terminals can be detected. This method overcomes the problems of low efficiency, poor reliability, high testing cost, and high operation difficulty of the original testing method, thereby improving product quality and service life.

[0036] The pre-drilled hole 2 can be any structure, such as a round hole or a square hole. The temperature of the metal probe 4 during the welding process of terminal 8 can be adjusted according to the size, height, and number of the pre-drilled holes 2 in the lead pipe 1 to meet the welding depth and appearance requirements of terminal 8. The temperature of the metal probe 4 during the welding process of terminal 8 can also be adjusted according to the structure, wall thickness, and alloy composition of the lead pipe 1 to meet the welding depth and appearance requirements of terminal 8.

[0037] In addition, the terminal 8 pressure test can be performed using an existing battery airtightness testing machine, or a pressure test device specifically designed for testing terminal 8 can be made.

[0038] If the pressure difference change is greater than 0.2 kPa, and multiple batteries fail to meet the welding depth requirements consecutively, observe the outer port of pre-drilled hole 2. If terminal 8 at the pre-drilled hole 2 appears smooth and full, it indicates an abnormality in the pressure testing equipment. After adjusting the pressure testing equipment, perform the pressure test again. Combining pressure testing with visual observation of the pre-drilled hole 2 not only allows for more accurate confirmation of whether the welding depth meets the requirements but also determines whether the pressure testing equipment is operating normally.

[0039] In addition, multiple pre-drilled holes 2 are provided, and these holes 2 are equally spaced around the upper sidewall of the lead pipe 1 to avoid potential differences in welding depth in different directions. Specifically, X = 5mm-8mm, and the diameter of the pre-drilled hole 2 is ≥1mm to prevent the hole diameter from being too small and affecting the air pressure differential monitoring.

[0040] In step S3, the inner wall of the lead tube 1 and the outer wall of the terminal post 6 are fitted with a clearance. After the upper ends of the lead tube 1 and the terminal post 6 are melted, they form a solid whole to ensure the structural strength of the battery terminal 8.

[0041] In step S4, the metal probe 4 is initially positioned at a distance from the top of the terminal post 6. The metal probe 4 is heated to 550°C by an acetylene flame 3. During the heating process, the acetylene flame 3 pre-melts the top of the lead pipe 1 and the terminal post 6. After 3 seconds, the probe is pressed down into the interior of the lead pipe 1 and the terminal post 6 to achieve deep melting of the lead pipe 1 and the terminal post 6. The depth of the metal probe 4 is not less than X. After 3 seconds, the metal probe 4 is lifted and the top of the lead pipe 1 and the terminal post 6 is cooled. Before heating the metal probe 4, a terminal welding sleeve 5 is first fitted onto the upper part of the lead pipe 1 and the terminal post 6, and the upper end of the metal welding sleeve forms a conical sleeve. After the terminal 8 is welded, cooling water is circulated into the conical sleeve at the end of the terminal welding sleeve 5 to cool the top of the lead pipe 1 and the terminal post 6.

[0042] The present invention provides a method for non-destructive testing of the welding depth of lead-acid battery terminals, which can be implemented through the following embodiments:

[0043] In light of the current after-sales battery issues, pre-drilled holes 2 are installed 6mm below the top of lead pipe 1 (drilling height, the distance from the truncated cone of lead pipe 1 is less than the height of the matching automotive wiring clip). The diameter of pre-drilled holes 2 is 2mm. Four pre-drilled holes 2 are installed, with an interval angle of 90°.

[0044] The lead pipe 1 with pre-drilled hole 2 and the battery cover are injection molded in an injection mold. The battery cover wraps around the lower part of the lead pipe 1 to form an integral part, and the upper part of the lead pipe 1 (including the position of pre-drilled hole 2) is exposed on the battery cover in preparation for welding with the terminal post 6 to form the battery terminal 8. The battery cover is welded to the battery case using a heat sealing machine. At this time, the terminal posts 6 of the electrode groups on both sides of the battery case pass through the lead pipe 1 of the battery cover from bottom to top, and the inner wall of the lead pipe 1 and the terminal post 6 form a clearance fit.

[0045] The battery enters the designated position at the terminal welding station. The terminal welding collar 5 descends and contacts the lead pipe 1. The top of the lead pipe 1 and the terminal post 6 in the battery cover section are above the terminal welding collar 5. The terminal welding machine heats the metal probe 4 to about 550°C using an acetylene flame 3. During the heating process, the acetylene flame 3 pre-melts the top of the lead pipe 1 and the terminal post 6. After 3 seconds, the metal probe 4 is pressed down into the lead pipe 1 and the terminal post 6 to achieve deeper melting of the terminal post 6 and the outer wall of the lead pipe 1. The metal probe 4 is pressed down to the bottom of the pre-drilled hole 2 in the lead pipe 1. After 3 seconds, the metal probe 4 is lifted, and cooling water is introduced into the terminal welding collar 5 to cool it down. The lead pipe 1 and the terminal post 6 are fused together to form the battery terminal 8. At this time, the lead liquid 7 at the pre-drilled hole 2 (welding depth) is completely melted and forms a whole with the terminal post and the lead pipe.

[0046] Reference Figure 5 If the probe is pressed down too deeply or other reasons cause the battery lead tube 1 to be positioned too low, the lead liquid 7 near the pre-drilled hole 2 may not be completely melted and filled, resulting in the terminal 8 not being able to form a seal.

[0047] A pressure test was performed on the individual cells at battery terminals 8 on both sides of the aforementioned battery. The pressure was 45 kPa, and the holding time was set to 5 seconds. The change in air pressure difference was monitored.

[0048] If the pressure difference change is ≤0.2kPa, then the welding depth of terminal 8 is ≥6mm, which meets the standard requirements;

[0049] If the pressure difference change is greater than 0.2 kPa, the welding depth of terminal 8 is less than 6 mm, which does not meet the standard requirements. If the number of rejections is significantly abnormal, the appearance of the rejected battery terminal 8 should be inspected. If the appearance of terminal 8 at the pre-drilled hole 2 is smooth and full, it indicates a problem with the testing equipment. After adjusting the equipment, the welding depth can be tested again.

[0050] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method of non-destructively testing the depth of a lead acid battery terminal weld, characterized by, Includes the following steps: S1: A pre-drilled hole (2) is made laterally at a distance X from the top on the side wall of the lead pipe (1). The number of pre-drilled holes (2) is at least two, and the interval angle between adjacent pre-drilled holes (2) is 360° / number of holes. S2: The lead pipe (1) and the battery cover are injection molded in an injection mold. The battery cover wraps around the lower part of the lead pipe (1) to form an integral part. The upper part of the lead pipe (1) with a pre-made hole (2) is exposed above the battery cover. S3: The battery cover is welded to the battery case using a heat sealer. The two pole group terminals (6) inside the battery case pass through the lead pipe (1) of the battery cover from bottom to top. S4: The battery enters the terminal welding station. The terminal welding machine heats the metal probe (4) with an acetylene flame (3). The metal probe (4) is pressed down into the interior of the lead pipe (1) and the terminal post (6) to fuse the upper area of ​​the lead pipe (1) and the terminal post (6) to form the welded battery terminal (8). S5: Perform a pressure test on the cell containing the terminals (8) on both sides of the battery to monitor the pressure change.

2. The method for non-destructive testing of the welding depth of lead-acid battery terminals as described in claim 1, characterized in that, In step S5, a pressure test is performed on the cell where the terminals (8) on both sides of the battery are located. The pressure is 40kPa-50kPa and the holding time is set to 5s. If the pressure difference change is ≤0.2kPa, the terminal welding depth meets the requirements, and the welding depth is ≥X; If the pressure difference change is greater than 0.2 kPa, the terminal welding depth does not meet the requirements, and the welding depth is less than X. If the pressure difference change value is greater than 0.2 kPa and multiple batteries fail to meet the welding depth requirements, observe the appearance of the terminal (8) at the pre-drilled hole (2). If the appearance of the terminal (8) is smooth and full, it indicates that the pressure testing equipment is abnormal. After debugging the pressure testing equipment, perform pressure testing again.

3. The method for non-destructive testing of the welding depth of lead-acid battery terminals as described in claim 1, characterized in that, X = 5mm-8mm, and the diameter of the pre-drilled hole (2) is ≥1mm.

Citation Information

Patent Citations

  • Welding assembly for pseudo soldering detection and equipment and method for detecting pseudo soldering of welding structure

    CN115990729A

  • Terminal welding method of lead-acid battery

    JP2007035307A