A nanocellulose-based photocurable resin and preparation method thereof

By mercapto-modifying nanocellulose and combining it with multi-component organic compounds, nanocellulose-based photocurable resin is prepared, which solves the problem of low natural cellulose modification reaction activity and realizes the preparation of high-performance coatings and environmentally friendly processes. Improved film-forming strength and water resistance of coatings.

CN117866201BActive Publication Date: 2024-10-22广东睿鹏材料科学有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311593120.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-27
Publication Date
2024-10-22
Estimated Expiration
2043-11-27

AI Technical Summary

Technical Problem

The existing technology has low reactivity and low grafting rate when modifying natural cellulose, making it difficult to prepare high-performance renewable and environmentally friendly coatings.

Method used

Nanocellulose is used as raw material, and after mercapto modification treatment, it is combined with polyvalent double bond organic compounds, polyvalent mercapto organic compounds, and initiators to prepare nanocellulose-based photocurable resin. Water is used as the solvent and combined with the photoinitiator. and thermal initiators to improve the efficiency of polymerization reactions.

Benefits of technology

It improves the film-forming strength of photo-cured resin, reduces VOC emissions, enhances the efficiency of polymerization reaction, reduces external energy input, and the prepared coating has good water resistance and low volatility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention belongs to the cross-field of high value-added utilization of biomass resources and photocurable resin coating technology, and specifically discloses a nanocellulose-based photocurable resin and a preparation method thereof. The nanocellulose-based photocurable resin is prepared from the following raw materials by weight: 20-90 parts of thiol-modified nanocellulose, 60-90 parts of polyvalent double-bond organic compounds, polyvalent thiol organic compounds, 20-30 parts of trimethylolpropane triacrylate, 0.1-1 parts of initiator, 1-5 parts of emulsifier, 0.2-0.4 parts of defoamer and 80-120 parts of deionized water. The nanocellulose-based photocurable resin produced by the present invention has the advantages of low production cost, green environmental protection, high atomic utilization rate and high strength after film formation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the cross-technical field of high value-added utilization of biomass resources and photocurable resins, and in particular relates to a nano-cellulose-based photocurable resin and a preparation method thereof. Background Art

[0002] With the continuous development of human production and life, the global oil and gas resources are decreasing sharply. It is estimated that the oil resources on the earth will be exhausted within 100 years. Green and renewable bio-based materials have become the most ideal alternative resources for oil, and are also important new materials for the development of polymer chemical industry technology. In the field of coating applications, bio-based materials, especially vegetable oils, have been widely used to prepare new green and environmentally friendly coatings. This is because vegetable oils have the characteristics of non-toxicity, low volatility, biodegradability, and abundant and easy-to-obtain raw materials. Since the 19th century, people have carried out a series of studies on vegetable oil-based polymers. For example, triglycerides in vegetable oils are hydrolyzed with glycerol to obtain monoglycerides for the preparation of alkyd resins; drying oils or fatty acids are first maleic anhydride-treated and then esterified with epoxy prepolymers to prepare fatty acid-modified epoxy coatings; soybean oil is epoxidized and then combined with acrylates to prepare epoxidized soybean oil acrylate resins; monoglyceride is also a polyol that can react with diisocyanates to prepare polyurethanes. The vegetable oils used to prepare water-based polyurethanes include sunflower oil, castor oil, rapeseed oil, soybean oil, etc.; tung oil is thermally cross-linked and polymerized to directly form a biodegradable coating.

[0003] Cellulose is the oldest and most abundant natural polymer on earth. It is an inexhaustible and most precious natural renewable resource for mankind. Cellulose chemistry and industry began more than 160 years ago and was the main research object during the birth and development of polymer chemistry. Cellulose is a macromolecular polysaccharide composed of glucose. The molecular chain contains abundant hydroxyl groups. Generally, cellulose modification is mainly carried out by chemical methods to introduce new groups into the hydroxyl groups of the cellulose molecular chain. However, modification of natural cellulose often has disadvantages such as low reactivity and low grafting rate.

[0004] Cellulose and its derivatives can be used as reinforcing fillers for coatings, as well as synthetic raw materials for coating resins or as film-forming substances. Therefore, the study of new renewable and environmentally friendly coatings has far-reaching and important significance for the development of my country's coatings industry. Summary of the invention

[0005] The purpose of the present invention is to provide a nano-cellulose-based photocurable resin and a preparation method thereof, in particular a photocurable resin prepared with biomass material, namely cellulose, as raw material.

[0006] The specific technical solutions are as follows:

[0007] A nanocellulose-based photocurable resin is prepared from the following raw materials in parts by weight: 20-90 parts of mercapto-modified nanocellulose, 60-90 parts of polyvalent double-bond organic compounds, 30-50 parts of polyvalent mercapto organic compounds, 20-30 parts of trimethylolpropane triacrylate, 0.1-1 parts of initiator, 1-5 parts of emulsifier, 0.2-0.4 parts of defoamer and 80-120 parts of deionized water;

[0008] The preparation of the thiol-modified nanocellulose comprises the following steps:

[0009] a. Add 3-10 g of 2,2,6,6-tetramethylpiperidine (TEMPO) to 20-30 g of distilled water, heat to 80-100° C., and stir continuously until TEMPO is completely dissolved to obtain a TEMPO solution;

[0010] b. Add 80-300 g of dry cellulose to 200 mL of distilled water, stir at a stirring speed of 200-500 r / min, then add the TEMPO solution, 10-30 g of sodium bromide and 500-1500 mL of 12 wt % sodium hypochlorite solution in sequence, and adjust the pH value of the mixed solution to between 10 and 10.5 with a 5 wt % sodium hydroxide solution, react at room temperature until the pH value of the mixed solution no longer changes within 3 minutes, and add 20-50 mL of alcohol to terminate the reaction;

[0011] c. Filtering the mixed solution in step b, and washing with distilled water until the filtrate is neutral, removing the filtrate to obtain oxidized micro-nanocellulose, and determining its solid content;

[0012] d. Weigh 1000-2000 g of the micro-nano cellulose obtained in step c, soak it in 1000 mL of a 1-5 M thiolamine compound, react at room temperature for 12-24 hours, then centrifuge to remove the filtrate, and obtain the thiol-modified nanocellulose.

[0013] In some embodiments, the nanocellulose-based photocurable resin is prepared from the following raw materials in parts by weight: 30-90 parts of thiol-modified nanocellulose, 70-90 parts of polyvalent double bond organic compounds, 30-50 parts of polyvalent thiol organic compounds, 20-30 parts of trimethylolpropane triacrylate, 0.1-1 parts of initiator, 1-5 parts of emulsifier, 0.2-0.4 parts of defoamer and 80-120 parts of deionized water.

[0014] In some embodiments, the thiolamine compound in step d can be at least one of mercaptoethylamine, 2-mercaptoethylamine, cysteine, 1,1-dimethyl-2-methylmercaptoethylamine, 1-mercaptopropylamine, and 2-mercaptopropylamine.

[0015] In some embodiments, the polyvalent double bond organic compound includes at least one of oleoylsarcosine, 2-acetylpyrazole, phenylacetoacetamide, acetoacetylbenzylamide, and acetoacetanilide.

[0016] In some embodiments, the polythiol organic compound includes at least one of thiol polyethylene glycol thiol, bis (2-thiol) sulfone, and ethylene glycol dimercaptoacetate.

[0017] In some embodiments, the initiator includes a mixture of a photoinitiator and a thermal initiator, and the molar ratio of the photoinitiator to the thermal initiator is 1:3-1:8; the photoinitiator includes at least one of benzophenone, 2,4-dihydroxybenzophenone, Michler's ketone, aromatic acylphosphine oxide, and bisbenzoylphenylphosphine oxide; the thermal initiator includes at least one of azobisisobutyronitrile and benzoyl peroxide.

[0018] In some embodiments, the emulsifier includes at least one of sodium dodecyl sulfosulfate, 2-p-nonylphenoloxy-ethyl ammonium sulfate, 2-acrylamido-methyl-propyl sodium sulfate, and 2-acrylamido-methyl-propyl ammonium sulfate.

[0019] In some embodiments, the defoaming agent includes at least one of a silicone defoaming agent and a polyether defoaming agent.

[0020] The present invention also provides a method for preparing the above-mentioned nanocellulose-based photocurable resin, the preparation method comprising the following steps:

[0021] a. In a multifunctional reaction kettle, the thiol-modified nanocellulose, the polythiol organic compound, trimethylolpropane triacrylate, deionized water, an emulsifier and a defoamer are sequentially added, and then stirred while introducing nitrogen to obtain an emulsion, and then nitrogen is continued to be introduced for 5-10 minutes;

[0022] b. Stop the nitrogen flow, heat to 80-100° C., then add the multi-component double-bond organic compound in the formula amount, and continue stirring for 0.5-1 hour; finally, add the initiator in the formula amount, continue stirring evenly to initiate the polymerization reaction, and keep the temperature for 1-3 hours;

[0023] c. After the heat preservation reaction is completed, the temperature is lowered to 50° C., the mixture is poured out from the multifunctional reactor, deionized water is added to reduce the viscosity, the mixture is dispersed and emulsified in a high-speed disperser, and water is removed by vacuum distillation to obtain the nanocellulose-based photocurable resin.

[0024] In some embodiments, the stirring condition in step a is: stirring at a speed of 500-1000 rpm for 10-30 minutes.

[0025] The present invention has the following advantages:

[0026] (1) Using water as a solvent not only makes the reaction process green and environmentally friendly, but also reduces the emission of VOCs during the subsequent use of photocurable resins;

[0027] (2) The strength of the photocurable resin film can be enhanced by modifying the nanocellulose with thiol groups and using it as a reactant instead of simply using it as a filler;

[0028] (3) The photoinitiator and the thermal initiator are mixed in the formula. The photoinitiator initiates the polymerization reaction under ultraviolet light and releases heat to drive the thermal initiator to further initiate the subsequent polymerization reaction, producing a multi-bonomine effect, making full use of the heat generated by the polymerization reaction and reducing the input of external energy. DETAILED DESCRIPTION

[0029] The following will combine specific embodiments, technical process steps, specific implementation conditions and materials to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] a. Add 5 g of 2,2,6,6-tetramethylpiperidine (TEMPO) to 30 g of distilled water, heat to 90°C, and stir continuously until TEMPO is completely dissolved;

[0032] b. Add 150 g of dry cellulose to 200 mL of distilled water, stir at a stirring speed of 300 r / min, then add the prepared TEMPO solution, 20 g of sodium bromide and 1000 mL of 12 wt % sodium hypochlorite solution in sequence, and adjust the pH value of the mixed solution to between 10 and 10.5 with 5 wt % sodium hydroxide solution, react at room temperature until the pH value of the mixed solution no longer changes within 3 minutes, and add 30 mL of alcohol to terminate the reaction;

[0033] c. Filtering the mixed solution in step b, and washing with distilled water until the filtrate is neutral, removing the filtrate to obtain oxidized micro-nanocellulose, and determining its solid content;

[0034] d. Weigh 2000 g of the micro-nano cellulose obtained in step c, soak it in 1000 mL of 3 M mercaptoethylamine, react at room temperature for 18 hours, then centrifuge to remove the filtrate, and obtain thiol-modified nanocellulose.

[0035] Example 2

[0036] a. Add 8 g of 2,2,6,6-tetramethylpiperidine (TEMPO) to 30 g of distilled water, heat to 90°C, and stir continuously until TEMPO is completely dissolved;

[0037] b. Add 240 g of dry cellulose to 200 mL of distilled water, stir at a stirring speed of 500 r / min, then add the prepared TEMPO solution, 30 g of sodium bromide and 1500 mL of 12 wt % sodium hypochlorite solution in sequence, and adjust the pH value of the mixed solution to between 10 and 10.5 with 5 wt % sodium hydroxide solution, react at room temperature until the pH value of the mixed solution no longer changes within 3 minutes, and add 50 mL of alcohol to terminate the reaction;

[0038] c. Filtering the mixed solution in step b, and washing with distilled water until the filtrate is neutral, removing the filtrate to obtain oxidized micro-nanocellulose, and determining its solid content;

[0039] d. Weigh 1000 g of the micro-nano cellulose obtained in step c, soak it in 1000 mL of 5 M 1-mercaptopropylamine, react at room temperature for 24 hours, then centrifuge to remove the filtrate, and obtain thiol-modified nanocellulose.

[0040] Example 3

[0041] Table 1 Raw material ratio of lignin-based acrylic resin film in Example 3

[0042]

[0043] The thiol-modified nanocellulose used in this example is the thiol-modified nanocellulose prepared in Example 1.

[0044] a. In a multifunctional reaction kettle, add thiol-modified nanocellulose, thiol polyethylene glycol thiol, trimethylolpropane triacrylate, deionized water, sodium dodecylsulfonate and polydimethylsiloxane in sequence, then stir at a speed of 500-1000 rpm for 10-30 minutes while introducing nitrogen to obtain an emulsion, and then continue to introduce nitrogen for 5-10 minutes;

[0045] b. Stop the nitrogen flow, heat to 80-100°C, then add the formulated amount of oleoyl sarcosine, and continue stirring for 0.5-1 hour; finally add the formulated amount of a mixture of benzophenone and azobisisobutyronitrile (the mass ratio of the two is 1:3), continue stirring evenly to initiate the polymerization reaction, and keep warm for 2 hours;

[0046] c. After the reaction has been carried out for 2 hours, the temperature is lowered to 50°C, the mixture is poured out from the multifunctional reactor, deionized water is added to reduce the viscosity, the mixture is dispersed and emulsified in a high-speed disperser, and the water is removed by vacuum distillation to obtain a nano-cellulose-based photocurable resin emulsion; the nano-cellulose-based photocurable resin is coated on a glass plate and cured under ultraviolet light to obtain a nano-cellulose-based photocurable resin film.

[0047] According to GB / T6739-1996 "Coating Hardness Pencil Test Method", the strength of the prepared acrylic resin film was tested by manual method. The test results showed that the film strength was > B.

[0048] The VOC of the prepared acrylic resin film was tested according to GB / T23985-2009 “Determination of Volatile Organic Compound (VOC) Content of Paints and Varnishes - Difference Method”, and the result was VOC≤149.

[0049] The water resistance of the prepared acrylic resin film was tested according to GB / T1727-1992. After immersion for 48 hours, the water absorption rate was 10.5%.

[0050] Example 4

[0051] Table 2 Raw material ratio of lignin-based acrylic resin film in Example 4

[0052]

[0053] The thiol-modified nanocellulose used in this example is the thiol-modified nanocellulose prepared in Example 1.

[0054] a. In a multifunctional reactor, add thiol-modified nanocellulose, bis(2-thiol)sulfone, trimethylolpropane triacrylate, deionized water, 2-p-nonylphenoloxy-ethyl ammonium sulfate and GPE type polyoxyethylene (polyoxypropylene) ether in sequence, then stir at a speed of 500-1000 rpm for 10-30 minutes while introducing nitrogen to obtain an emulsion, and then continue to introduce nitrogen for 5-10 minutes;

[0055] b. Stop the nitrogen flow, heat to 80-100°C, then add the formulated amount of phenylacetamide, and continue stirring for 0.5-1 hour; finally, add the formulated amount of a mixture of Michler's ketone and benzoyl peroxide (the mass ratio of the two is 1:5), continue stirring evenly to initiate the polymerization reaction, and keep warm for 2 hours;

[0056] c. After the reaction has been carried out for 2 hours, the temperature is lowered to 50°C, the mixture is poured out from the multifunctional reactor, deionized water is added to reduce the viscosity, the mixture is dispersed and emulsified in a high-speed disperser, and water is removed by vacuum distillation to obtain a nano-cellulose-based photocurable resin emulsion; the nano-cellulose-based photocurable resin is coated on a glass plate and cured to obtain a nano-cellulose-based photocurable resin film.

[0057] According to GB / T6739-1996 "Coating Hardness Pencil Test Method", the strength of the prepared acrylic resin film was tested by manual method. The test results showed that the film strength was > B.

[0058] The VOC of the prepared acrylic resin film was tested according to GB / T23985-2009 “Determination of Volatile Organic Compound (VOC) Content of Paints and Varnishes - Difference Method”, and the result was VOC≤143.

[0059] The water resistance of the prepared acrylic resin film was tested according to GB / T1727-1992. After immersion for 48 hours, the water absorption rate was 15.2%.

[0060] Example 5

[0061] Table 3 Raw material ratio of lignin-based acrylic resin film in Example 5

[0062]

[0063] The thiol-modified nanocellulose used in this example is the thiol-modified nanocellulose prepared in Example 2.

[0064] a. In a multifunctional reactor, add thiol-modified nanocellulose, ethylene glycol dimercaptoacetate, trimethylolpropane triacrylate, deionized water, 2-acrylamido-methyl-propyl sodium sulfate and GP-type glycerol polyether in sequence, then stir at a speed of 500-1000 rpm for 10-30 minutes while introducing nitrogen to obtain an emulsion, and then continue to introduce nitrogen for 5-10 minutes;

[0065] b. Stop the nitrogen flow, heat to 80-100°C, then add the formulated amount of acetyl acetyl benzyl amide, and continue stirring for 0.5-1 hour; finally, add the formulated amount of a mixture of bisbenzoylphenyl phosphine oxide and benzoyl peroxide (the mass ratio of the two is 1:4), continue stirring evenly to initiate the polymerization reaction, and keep warm for 2 hours;

[0066] c. After the reaction has been carried out for 2 hours, the temperature is lowered to 50°C, the mixture is poured out from the multifunctional reactor, deionized water is added to reduce the viscosity, the mixture is dispersed and emulsified in a high-speed disperser, and water is removed by vacuum distillation to obtain a nano-cellulose-based photocurable resin emulsion; the nano-cellulose-based photocurable resin is coated on a glass plate and cured to obtain a nano-cellulose-based photocurable resin film.

[0067] According to GB / T6739-1996 "Coating Hardness Pencil Test Method", the strength of the prepared acrylic resin film was tested by manual method. The test results showed that the film strength was > B.

[0068] The VOC of the prepared acrylic resin film was tested according to GB / T23985-2009 “Determination of Volatile Organic Compound (VOC) Content of Paints and Varnishes - Difference Method”, and the result was VOC≤119.

[0069] The water resistance of the prepared acrylic resin film was tested according to GB / T1727-1992. After immersion for 48 hours, the water absorption rate was 16.8%.

[0070] Example 6

[0071] Table 4 Raw material ratio of lignin-based acrylic resin film in Example 6

[0072]

[0073] The thiol-modified nanocellulose used in this example is the thiol-modified nanocellulose prepared in Example 2.

[0074] a. In a multifunctional reactor, thiol-modified nanocellulose, thiol polyethylene glycol thiol, trimethylolpropane triacrylate, deionized water, 2-acrylamido-methyl-propyl ammonium sulfate and ethylene glycol siloxane are added in sequence, and then nitrogen is introduced and stirred at a speed of 500-1000 rpm for 10-30 minutes to obtain an emulsion, and then nitrogen is continued to be introduced for 5-10 minutes;

[0075] b. Stop the nitrogen flow, heat to 80-100°C, then add the formulated amount of 2-acetylpyrazole, and continue stirring for 0.5-1 hour; finally, add the formulated amount of a mixture of benzophenone and benzoyl peroxide (the mass ratio of the two is 1:8), continue stirring evenly to initiate the polymerization reaction, and keep warm for 2 hours;

[0076] c. After the reaction has been carried out for 2 hours, the temperature is lowered to 50°C, the mixture is poured out from the multifunctional reactor, deionized water is added to reduce the viscosity, the mixture is dispersed and emulsified in a high-speed disperser, and water is removed by vacuum distillation to obtain a nano-cellulose-based photocurable resin emulsion; the nano-cellulose-based photocurable resin is coated on a glass plate and cured to obtain a nano-cellulose-based photocurable resin film.

[0077] According to GB / T6739-1996 "Coating Hardness Pencil Test Method", the strength of the prepared acrylic resin film was tested by manual method. The test results showed that the film strength was > B.

[0078] The VOC of the prepared acrylic resin film was tested according to GB / T23985-2009 “Determination of Volatile Organic Compound (VOC) Content of Paints and Varnishes - Difference Method”, and the result was VOC≤107.

[0079] The water resistance of the prepared acrylic resin film was tested according to GB / T1727-1992. After immersion for 48 hours, the water absorption rate was 13.5%.

[0080] Example 7

[0081] Table 5 Raw material ratio of lignin-based acrylic resin film in Example 7

[0082]

[0083] The thiol-modified nanocellulose used in this example is the thiol-modified nanocellulose prepared in Example 2.

[0084] a. In a multifunctional reactor, add thiol-modified nanocellulose, bis(2-thiol)sulfone, trimethylolpropane triacrylate, deionized water, 2-p-nonylphenoloxy-ethyl ammonium sulfate and ethylene glycol siloxane in sequence, then stir at a speed of 500-1000 rpm for 10-30 minutes while introducing nitrogen to obtain an emulsion, and then continue to introduce nitrogen for 5-10 minutes;

[0085] b. Stop the nitrogen flow, heat to 80-100°C, then add the formulated amount of oleoyl sarcosine, and continue stirring for 0.5-1 hour; finally add the formulated amount of a mixture of Michler's ketone and azobisisobutyronitrile (the mass ratio of the two is 1:5), continue stirring evenly to initiate the polymerization reaction, and keep warm for 2 hours;

[0086] c. After the reaction has been carried out for 2 hours, the temperature is lowered to 50°C, the mixture is poured out from the multifunctional reactor, deionized water is added to reduce the viscosity, the mixture is dispersed and emulsified in a high-speed disperser, and water is removed by vacuum distillation to obtain a nano-cellulose-based photocurable resin emulsion; the nano-cellulose-based photocurable resin is coated on a glass plate and cured to obtain a nano-cellulose-based photocurable resin film.

[0087] According to GB / T6739-1996 "Coating Hardness Pencil Test Method", the strength of the prepared acrylic resin film was tested by manual method. The test results showed that the film strength was > B.

[0088] The VOC of the prepared acrylic resin film was tested according to GB / T23985-2009 “Determination of Volatile Organic Compound (VOC) Content of Paints and Varnishes - Difference Method”, and the result was VOC≤124.

[0089] The water resistance of the prepared acrylic resin film was tested according to GB / T1727-1992. After immersion for 48 hours, the water absorption rate was 10.8%.

[0090] Technical personnel should note that although the present invention has been described according to the above specific implementation methods, the inventive concept of the present invention is not limited to this invention, and any modification using the inventive concept will be included in the scope of protection of this patent.

Claims

1. A nanocellulose-based photocurable resin, It is characterized in that The nanocellulose is prepared from the following raw materials in parts by weight: 20-90 parts of mercapto-modified nanocellulose, 60-90 parts of polyvalent double-bond organic compounds, 30-50 parts of polyvalent mercapto organic compounds, 20-30 parts of trimethylolpropane triacrylate, 0.1-1 parts of initiator, 1-5 parts of emulsifier, 0.2-0.4 parts of defoamer and 80-120 parts of deionized water; The preparation of the thiol-modified nanocellulose comprises the following steps: a. Add 3-10 g TEMPO to 20-30 g distilled water, heat to 80-100°C, and stir continuously until TEMPO is completely dissolved to obtain a TEMPO solution; b. Add 80-300 g of dry cellulose to 200 mL of distilled water, stir at a stirring speed of 200-500 r / min, then add the TEMPO solution, 10-30 g of sodium bromide and 500-1500 mL of 12 wt % sodium hypochlorite solution in sequence, and adjust the pH value of the mixed solution to between 10 and 10.5 with a 5 wt % sodium hydroxide solution, react at room temperature until the pH value of the mixed solution no longer changes within 3 minutes, and add 20-50 mL of alcohol to terminate the reaction; c. Filtering the mixed solution in step b, and washing with distilled water until the filtrate is neutral, removing the filtrate to obtain oxidized micro-nanocellulose, and determining its solid content; d. Weighing 1000-2000 g of the micro-nano cellulose obtained in step c, soaking it in 1000 mL of a 1-5 M thiolamine compound, reacting it at room temperature for 12-24 hours, and then centrifuging and removing the filtrate to obtain the thiol-modified nanocellulose; The thiolamine compound in step d includes at least one of mercaptoethylamine, 2-mercaptoethylamine, cysteine, 1,1-dimethyl-2-methylmercaptoethylamine, 1-mercaptopropylamine, and 2-mercaptopropylamine; The polyvalent double-bond organic compound comprises at least one of oleoylsarcosine, 2-acetylpyrazole, phenylacetoacetamide, acetoacetylbenzylamide, and acetoacetanilide; The polythiol organic compound comprises at least one of thiol polyethylene glycol thiol, bis(2-thiol) sulfone, and ethylene glycol dimercaptoacetate; The initiator comprises a photoinitiator and a thermal initiator, and the molar ratio of the photoinitiator to the thermal initiator is 1:3-1:8; the photoinitiator comprises at least one of benzophenone, 2,4-dihydroxybenzophenone, Michler's ketone, aromatic acylphosphine oxide, and bisbenzoylphenylphosphine oxide; the thermal initiator comprises at least one of azobisisobutyronitrile and benzoyl peroxide.

2. The nanocellulose-based photocurable resin according to claim 1, It is characterized in that The emulsifier includes at least one of sodium dodecylsulfonate, 2-p-nonylphenoloxy-ethyl ammonium sulfate, 2-acrylamide-methyl-propyl sodium sulfate, and 2-acrylamide-methyl-propyl ammonium sulfate.

3. The nanocellulose-based photocurable resin according to claim 1, It is characterized in that The defoaming agent includes at least one of an organosilicon defoaming agent and a polyether defoaming agent.

4. The method for preparing the nanocellulose-based photocurable resin according to any one of claims 1 to 3, It is characterized in that The steps include: a. In a multifunctional reaction kettle, the thiol-modified nanocellulose, the polythiol organic compound, trimethylolpropane triacrylate, deionized water, an emulsifier and a defoamer are sequentially added, and stirred while introducing nitrogen to obtain an emulsion, and then nitrogen is continuously introduced for 5-10 minutes; b. Stop the nitrogen flow, heat to 80-100° C., then add the multi-component double-bond organic compound in the formula amount, and continue stirring for 0.5-1 hour; finally, add the initiator in the formula amount, continue stirring evenly to initiate the polymerization reaction, and keep the temperature for 1-3 hours; c. After the heat preservation reaction is completed, the temperature is lowered to 50° C., the mixture is poured out from the multifunctional reactor, deionized water is added to reduce the viscosity, the mixture is dispersed and emulsified in a high-speed disperser, and water is removed by vacuum distillation to obtain the nanocellulose-based photocurable resin.

5. The method for preparing the nanocellulose-based photocurable resin according to claim 4, It is characterized in that The stirring condition in step a is: stirring at a speed of 500-1000 rpm for 10-30 minutes.