Oxyhalide solid electrolyte and preparation method thereof, and battery
By preparing an oxyhalide solid electrolyte and utilizing the synergistic effect of a specific ratio of metal halide and lithium oxide, the problem of insufficient moisture resistance of the solid electrolyte is solved and the stability and high performance of ionic conductivity in a humid environment are achieved.
Patent Information
- Application Number
- CN202311867172.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-12-29
AI Technical Summary
Existing solid electrolytes have poor moisture resistance, resulting in a large decrease in ionic conductivity in a humid environment, affecting the performance of lithium-ion batteries.
The general formula of using oxyhalide solid electrolyte is Li2a+bMbOaX'cX”d, where M is selected from Ta, In or Zr, and , to prepare an oxyhalide solid electrolyte with good moisture resistance.
In a humid environment, the ionic conductivity of the oxyhalide solid electrolyte decreases very little and maintains a high ionic conductivity, improving the stability and performance of lithium-ion batteries.
Smart Images

Figure CN117878390B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrolyte technology, and in particular to an oxyhalide solid electrolyte, a preparation method thereof, and a battery. Background Art
[0002] Lithium-ion batteries have been extensively researched and developed over the past few decades. Lithium-ion batteries are mainly composed of positive electrodes, negative electrodes, electrolytes and separators. Among them, the electrolyte is one of the important components of lithium-ion batteries. It is a substance that establishes ion conduction channels between the positive and negative electrodes inside the battery while blocking electronic conduction. Therefore, the electrochemical performance of the battery is closely related to the properties of the electrolyte.
[0003] Solid-state electrolyte (SSE) is a solid ion conductor electrolyte with the characteristics of high safety, no leakage of toxic organic liquid, low flammability, non-volatility, high mechanical stability, high thermal stability, easy processing, and low self-discharge rate. It is used to replace liquid electrolytes in lithium-ion batteries.
[0004] However, the moisture resistance of existing solid electrolytes is poor and needs to be further improved. Summary of the invention
[0005] In view of this, the present application provides an oxyhalide solid electrolyte, aiming to improve the problem of poor moisture resistance of existing solid electrolytes.
[0006] The embodiment of the present application is implemented as follows: an oxyhalide solid electrolyte, the general formula of which is Li 2a+b M b O a X' c X” d , wherein M is selected from Ta, In or Zr, X is selected from halogen, wherein 0.5≤a≤1.6, 1≤b≤1.5, 5≤c+d≤7.5, c and d are both numbers greater than 0; X' and X" are each independently selected from halogen, and X' and X" are different.
[0007] Optionally, in some embodiments, the halogen includes one or more of F, Cl, and Br.
[0008] Optionally, in some embodiments, the range of a is 0.5≤a≤0.8; and / or
[0009] The range of b is 1≤b≤1.2; and / or
[0010] The range of c+d is 5≤c+d≤6.8.
[0011] Optionally, in some embodiments, the general formula of the oxyhalide solid electrolyte is Li 2.5 Ta1.1 O 0.7 Cl 6.1 F 0.5 、Li2TaO 0.5 Cl 5.6 F 0.4 , Li 3.2 Zr 1.2 One or more of OCl5Br, Li4Zr2OCl8F2.
[0012] Optionally, in some embodiments, the ionic conductivity of the oxyhalide solid electrolyte at a relative humidity of 0% is in the range of 10.7 to 11.8 mS / cm; and / or
[0013] The ionic conductivity of the oxyhalide solid electrolyte is in the range of 9.1 to 10.9 mS / cm at a relative humidity of 5%; and / or
[0014] The ionic conductivity of the oxyhalide solid electrolyte is in the range of 10.5 to 10.7 mS / cm at a relative humidity of 10%; and / or
[0015] The ionic conductivity of the oxyhalide solid electrolyte is in the range of 8.0 to 10.1 mS / cm at a relative humidity of 15%; and / or
[0016] The ionic conductivity of the oxyhalide solid electrolyte is in the range of 7.1 to 10.0 mS / cm at a relative humidity of 20%; and / or
[0017] The ionic conductivity of the oxyhalide solid electrolyte is in the range of 5.9-7.5 mS / cm when the relative humidity is 30%.
[0018] Accordingly, the present application also provides a method for preparing an oxyhalide solid electrolyte, comprising the following steps:
[0019] A first metal halide, a second metal halide, a third metal halide, and lithium oxide are mixed to obtain a mixture, wherein the chemical formula of the first metal halide is LiX', and the chemical formula of the second metal halide is MX' m , the chemical formula of the third metal halide is MX" n , X' and X" are each independently selected from halogen, and X' and X" are different, M is selected from Ta, In or Zr, and m and n are each independently selected from any integer from 1 to 5;
[0020] ball-milling the mixture to obtain an oxyhalide solid electrolyte precursor;
[0021] The oxyhalide solid electrolyte precursor is annealed to obtain an oxyhalide solid electrolyte.
[0022] Optionally, in some embodiments, the molar ratio of the lithium oxide, the first metal halide, the second metal halide, and the third metal halide is (0.01-2):(0.01-2):(0.1-1.5):(0.1-1.5); and / or
[0023] The mass ratio of the ball milling beads to the mixture is in the range of (8-20):1; and / or
[0024] The halogen includes F, Cl or Br.
[0025] Optionally, in some embodiments, the ball milling device is a planetary ball mill; and / or
[0026] The ball milling speed is 500-700 rpm; and / or
[0027] The effective ball milling time is 70 to 200 hours; and / or
[0028] The ratio of the rest time of the ball milling to the ball milling time is (0.1-1):1; and / or
[0029] The annealing temperature is 100-300° C., and the annealing time is 30-180 minutes.
[0030] Optionally, in some embodiments, the mixing is performed under a protective atmosphere, and the gas in the protective atmosphere includes one or more of nitrogen, helium, neon, argon, krypton, and xenon.
[0031] Correspondingly, the present application also provides a battery, comprising the oxyhalide solid electrolyte.
[0032] The oxyhalide solid electrolyte described in the present application has good moisture resistance due to the synergistic effect of the elements and element ratios in the oxyhalide solid electrolyte. In this way, the ionic conductivity of the oxyhalide solid electrolyte in a humid environment decreases very little compared to that in a dry environment, while still having good ionic conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0034] Figure 1 It is a flow chart of a method for preparing an oxyhalide solid electrolyte provided in an embodiment of the present application;
[0035] Figure 2 This is an electrochemical impedance spectrum of a battery prepared using the oxyhalide solid electrolyte of Example 1 of the present application;
[0036] Figure 3 is an electrochemical impedance spectrum of a battery prepared with the oxyhalide solid electrolyte of Example 8 of the present application;
[0037] Figure 4 is an electrochemical impedance spectrum of a battery prepared with the oxyhalide solid electrolyte of Example 10 of the present application;
[0038] Figure 5 This is the electrochemical impedance spectrum of the battery prepared by the oxyhalide solid electrolyte of Comparative Example 1 of the present application;
[0039] Figure 6 This is the electrochemical impedance spectrum of the battery prepared by the oxyhalide solid electrolyte of Comparative Example 2 of the present application
[0040] Figure 7 This is the electrochemical impedance spectrum of the battery prepared by the oxyhalide solid electrolyte of Comparative Example 8 of the present application;
[0041] Figure 8 This is the XRD diagram of the oxyhalide solid electrolyte of Example 1 of the present application. DETAILED DESCRIPTION
[0042] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.
[0043] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.
[0044] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.
[0045] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0046] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0047] Existing solid electrolytes include oxide solid electrolytes, sulfide solid electrolytes and halide solid electrolytes. Among them, oxide solid electrolytes have extremely high ionic conductivity and electrochemical window, but it is difficult to take into account mechanical properties. In the actual process of preparing batteries, it is easy to produce unexpected adverse interfacial reactions due to high-temperature sintering. Sulfide solid electrolytes also have extremely high ionic conductivity, but their extremely poor air stability and environmental toxicological behavior limit their rapid development and application, and sulfide solid electrolytes are difficult to pair with the currently popular high-voltage oxide positive electrode materials alone. The halide solid electrolytes that have attracted renewed attention have high ionic conductivity, excellent mechanical properties and good interfacial stability to ternary materials, making it possible to further participate in high-energy density and high-safety solid-state lithium batteries. However, the existing halide solid electrolytes have poor moisture resistance, and the ionic conductivity decreases significantly in a humid environment. In addition, the production process of halide solid electrolytes generally relies on high-energy ball milling and annealing processes. However, in order to achieve ideal physicochemical properties, the ball milling equipment that provides mechanochemical reactions is often extremely expensive, and non-specific phase halides are often unstable after annealing, showing lower ionic conductivity and repeatability.
[0048] The technical solution of this application is as follows:
[0049] In a first aspect, the present invention provides an oxyhalide solid electrolyte having a general formula of Li 2a+b M b O a X' c X” d , wherein M is selected from Ta, In or Zr, X is selected from halogen, wherein 0.5≤a≤1.6, 1≤b≤1.5, 5≤c+d≤7.5, and c and d are both numbers greater than 0.
[0050] It can be understood that in some embodiments, one of c and d can be 0. In this case, the oxyhalide solid electrolyte includes only one halogen.
[0051] The halogen includes, but is not limited to, one or more of F, Cl, and Br.
[0052] In some embodiments, a may be 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, etc. In at least one preferred embodiment, a is in the range of 0.5≤a≤0.8.
[0053] In some embodiments, b may be 1, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, etc. In at least one preferred embodiment, the range of b is 1≤a≤1.2.
[0054] In some embodiments, the c+d may be 5, 5.2, 5.5, 5.6, 5.8, 6, 6.2, 6.4, 6.5, 6.7, 6.8, 7, 7.2, 7.4, 7.5, etc. In at least one preferred embodiment, the range of c+d is 5≤c+d≤6.8.
[0055] As an example, in some embodiments, the general formula of the oxyhalide solid electrolyte is Li 2.5 Ta 1.1 O 0.7 Cl 6.1 F 0.5 、Li2TaO 0.5 Cl 5.6 F 0.4 , Li 3.2 Zr 1.2 One or more of OCl5Br, Li4Zr2OCl8F2.
[0056] The ionic conductivity of the oxyhalide solid electrolyte is in the range of 10.7-11.8 mS / cm when the relative humidity (RH) is 0%.
[0057] The ionic conductivity of the oxyhalide solid electrolyte at a relative humidity (RH) of 5% ranges from 9.1 to 10.9 mS / cm, for example, 9.1 mS / cm, 8.5 mS / cm, 9.8 mS / cm, 10.0 mS / cm, 10.2 mS / cm, 10.5 mS / cm, 10.9 mS / cm, etc.
[0058] The ionic conductivity of the oxyhalide solid electrolyte at a relative humidity (RH) of 10% is in the range of 10.5 to 10.7 mS / cm, for example, 10.5 mS / cm, 10.6 mS / cm, 10.7 mS / cm, etc.
[0059] The ionic conductivity of the oxyhalide solid electrolyte at a relative humidity (RH) of 15% ranges from 8.0 to 10.1 mS / cm, for example, 8.0 mS / cm, 8.2 mS / cm, 8.5 mS / cm, 8.8 mS / cm, 9.0 mS / cm, 9.2 mS / cm, 9.5 mS / cm, 9.8 mS / cm, 10.0 mS / cm, 10.1 mS / cm, etc.
[0060] The ionic conductivity of the oxyhalide solid electrolyte at a relative humidity (RH) of 20% ranges from 7.1 to 10.0 mS / cm, for example, 7.1 mS / cm, 7.2 mS / cm, 7.5 mS / cm, 7.6 mS / cm, 7.8 mS / cm, 8.0 mS / cm, 8.5 mS / cm, 8.6 mS / cm, 9.0 mS / cm, 9.2 mS / cm, 9.4 mS / cm, 9.6 mS / cm, 9.8 mS / cm, 10.0 mS / cm, etc.
[0061] The ionic conductivity of the oxyhalide solid electrolyte at a relative humidity (RH) of 30% ranges from 5.9 to 7.5 mS / cm, for example, 5.9 mS / cm, 6.0 mS / cm, 6.2 mS / cm, 6.4 mS / cm, 6.5 mS / cm, 6.6 mS / cm, 6.8 mS / cm, 7.0 mS / cm, 7.2 mS / cm, 7.3 mS / cm, 7.5 mS / cm, etc.
[0062] The oxyhalide solid electrolyte described in the present application has good moisture resistance due to the synergistic effect of the elements and element ratios in the oxyhalide solid electrolyte. In this way, the ionic conductivity of the oxyhalide solid electrolyte in a humid environment decreases very little compared to that in a dry environment, while still having good ionic conductivity.
[0063] Second, see Figure 1The present application also provides a method for preparing an oxyhalide solid electrolyte, comprising the following steps:
[0064] Step S11: Mix a first metal halide, a second metal halide, a third metal halide, and lithium oxide to obtain a mixture, wherein the chemical formula of the first metal halide is LiX', and the chemical formula of the second metal halide is MX' m , the chemical formula of the third metal halide is MX" n , X' and X" are each independently selected from halogen, and X' and X" are different, M is selected from Ta, In or Zr, and m and n are each independently selected from any integer from 1 to 5;
[0065] Step S12, ball-milling the mixture to obtain an oxyhalide solid electrolyte precursor;
[0066] Step S13, annealing the oxyhalide solid electrolyte precursor to obtain an oxyhalide solid electrolyte.
[0067] In the step S11:
[0068] The molar ratio of the lithium oxide, the first metal halide, the second metal halide, and the third metal halide is (0.01-2):(0.01-2):(0.1-1.5):(0.1-1.5). Within the mass ratio range, it is beneficial to prepare an oxyhalide solid electrolyte with good moisture resistance and high ion conductivity.
[0069] The halogen includes, but is not limited to, F, Cl or Br.
[0070] In some embodiments, the mixing is performed under a protective atmosphere, and the gas in the protective atmosphere may be, but is not limited to, one or more of nitrogen, helium, neon, argon, krypton, and xenon.
[0071] In step S12:
[0072] In some embodiments, the equipment used for ball milling is a planetary ball mill, which can effectively reduce the cost of ball milling.
[0073] In some embodiments, the ball milling beads are zirconium oxide.
[0074] In some embodiments, the mass ratio of the ball milling beads to the mixture is in the range of (8-20): 1. When the ball milling ratio is lower than this range, the impact energy is low, the mechanochemical reaction is insufficient, and an ordered crystal-amorphous cannot be formed. When the ball milling ratio is higher than this range, the possibility of excessive crystal transformation will increase, thereby possibly reducing the ionic conductivity of the product, and a too high ball milling ratio will lead to low equipment efficiency.
[0075] In some embodiments, the ball milling speed is 500-700 rpm, such as 500 rpm, 530 rpm, 550, 580 rpm, 600 rpm, 620 rpm, 650 rpm, 670 rpm, 700 rpm, etc., and the effective ball milling time (i.e., the total time of the entire ball milling process minus the rest time) is 70-200 h, such as 70 h, 100 h, 120 h, 130 h, 140 h, 150 h, 160 h, 180 h, 200 h, etc. Within the speed and time range, the efficiency of the mechanochemical reaction can be increased, which is conducive to obtaining an oxyhalide solid electrolyte with good moisture resistance.
[0076] In some embodiments, the ratio of the rest time of the ball mill to the ball milling time is (0.1-1):1, for example, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1.0:1, etc. Within the range, when the rest ratio is lower than this interval, more time will be spent on ball milling, which will cause some particles to stick to the wall, that is, contact and collision are reduced, affecting the ball milling effect; and when the rest ratio is higher than this interval, the effective ball milling time will be short and the ball milling efficiency will be low.
[0077] In step S13:
[0078] The annealing temperature is 100-300°C, for example, 100°C, 120°C, 130°C, 150°C, 160°C, 180°C, 200°C, 220°C, 240°C, 250°C, 260°C, 280°C, 300°C, etc., and the annealing time is 30-180min, for example, 30min, 60min, 80min, 100min, 120min, 150min, 160min, 180min, etc. Within the temperature and time range, the formation of the crystalline segment part of the oxyhalide solid electrolyte can be effectively promoted, and the ionic conductivity and moisture resistance of the oxyhalide solid electrolyte can be increased. Too high or too low will cause the ionic conductivity to drop rapidly in performance, and even the target product cannot be formed.
[0079] The method for preparing the oxyhalide solid electrolyte described in the present application uses a specific ratio of a first metal halide, a second metal halide, a third metal halide, and lithium oxide, and prepares an oxyhalide solid electrolyte with good moisture resistance through ball milling and annealing, so that the prepared oxyhalide solid electrolyte can still have good ionic conductivity in a humid environment.
[0080] In a third aspect, an embodiment of the present application further provides a battery comprising the oxyhalide solid electrolyte described above.
[0081] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.
[0082] Example 1
[0083] In an argon atmosphere, lithium oxide Li2O, a first metal halide LiCl, a second metal halide TaCl5 and a third metal chloride LiF are mixed in a molar ratio of 0.7:0.6:1.1:0.5 to obtain a mixture;
[0084] The mixture is added to a ball mill of a planetary ball mill, wherein the mass ratio of the ball milling beads to the mixture is 15:1, and the ball milling beads are zirconium oxide. The ball mill is first completely evacuated, and then the ball mill is placed in air for ball milling. The ball milling speed is 630 rpm, the rest and ball milling time ratio is 1:0.5, and the effective ball milling time is 150 hours; and an oxyhalide solid electrolyte precursor is obtained;
[0085] The oxyhalide solid electrolyte precursor was taken out under the protection of argon atmosphere, and transferred to a muffle furnace equipped in argon atmosphere for high temperature annealing, wherein the annealing temperature was 250° C. and the annealing time was 60 min, to obtain the oxyhalide solid electrolyte.
[0086] The oxyhalide solid electrolyte of this embodiment is Li 2.5 Ta 1.1 O 0.7 Cl 6.1 F 0.5 .
[0087] Example 2
[0088] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the molar ratio of Li2O, LiCl, TaCl5 and LiF is 0.5:0.6:1.0:0.4.
[0089] The oxyhalide solid electrolyte Li2TaO 0.5 Cl 5.6 F 0.4 .
[0090] Example 3
[0091] This embodiment is substantially the same as Embodiment 1, except that in this embodiment, the second metal halide is ZrCl2, and the molar ratio of Li2O, LiCl, ZrCl4 and LiBr in this embodiment is 1.0:0.2:1.2:1.0.
[0092] The oxyhalide solid electrolyte of this embodiment is LiZrOCl4Br.
[0093] Example 4
[0094] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the ball milling speed is 500 rpm.
[0095] Example 5
[0096] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the ball milling speed is 700 rpm.
[0097] Example 6
[0098] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the ball milling time is 70 hours.
[0099] Example 7
[0100] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the ball milling time is 200 hours.
[0101] Example 8
[0102] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the mass ratio of the ball milling beads to the mixture is 8:1.
[0103] Example 9
[0104] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the mass ratio of the ball milling beads to the mixture is 20:1.
[0105] Example 10
[0106] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the annealing temperature is 300°C.
[0107] Embodiment 11
[0108] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the annealing temperature is 100°C.
[0109] Example 12
[0110] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the ratio of rest time to ball milling time is 1:1.
[0111] Embodiment 13
[0112] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the ratio of rest time to ball milling time is 1:0.1.
[0113] Embodiment 14
[0114] This embodiment is basically the same as embodiment 1, except that in this embodiment, the molar ratio of Li2O, LiCl, TaCl5 and LiF is 0.5:0.5:1.0:0.5, and the oxyhalide solid electrolyte in this embodiment is Li2TaO 0.5 Cl 5.5 F 0.5 .
[0115] Embodiment 15
[0116] This embodiment is basically the same as embodiment 1, except that in this embodiment, the molar ratio of Li2O, LiCl, TaCl5 and LiF is 1:0.5:1:0.5, and the oxyhalide solid electrolyte in this embodiment is Li3TaOCl 5.5 F 0.5 .
[0117] Comparative Example 1
[0118] This embodiment is basically the same as embodiment 1, except that in this embodiment, the molar ratio of Li2O, LiCl, TaCl5 and LiF is 0.4:0.1:0.5:0.4, and the oxyhalide solid electrolyte in this embodiment is Li 1.3 Ta 0.5 O 0.4 Cl 2.6 F 0.4 .
[0119] Comparative Example 2
[0120] This embodiment is basically the same as embodiment 1, except that in this embodiment, the molar ratio of Li2O, LiCl, TaCl5 and LiF is 2:1:1.6:0.6, and the oxyhalide solid electrolyte in this embodiment is Li 5.6 Ta 1.6 O2Cl9F 0.6 .
[0121] Comparative Example 3
[0122] This embodiment is basically the same as embodiment 1, except that in this embodiment, the molar ratio of Li2O, LiCl, TaCl5 and LiF is 0.3:0.1:0.7:0.6, and the oxyhalide solid electrolyte in this embodiment is Li 1.3 Ta 0.7 O 0.3 Cl 3.6 F 0.6 .
[0123] Comparative Example 4
[0124] This embodiment is basically the same as embodiment 1, except that in this embodiment, the molar ratio of Li2O, LiCl, TaCl5 and LiF is 1.7:1.0:1.6:0.6, and the oxyhalide solid electrolyte in this embodiment is Li5Ta 1.6 O 1.7 9F 0.6 .
[0125] Comparative Example 5
[0126] This embodiment is basically the same as embodiment 1, except that in this embodiment, the molar ratio of Li2O, LiCl, TaCl5 and LiF is 0.2:0.2:0.6:0.4, and the oxyhalide solid electrolyte in this embodiment is LiTa 0.6 O 0.2 Cl 3.2 F 0.4 .
[0127] Comparative Example 6
[0128] This embodiment is basically the same as embodiment 1, except that in this embodiment, the molar ratio of Li2O, LiCl, TaCl5 and LiF is 2:1:2:1, and the oxyhalide solid electrolyte in this embodiment is Li6Ta2O2Cl 11 F.
[0129] Comparative Example 7
[0130] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the second metal halide TaCl5 and the third metal chloride LiF are not included.
[0131] Comparative Example 8
[0132] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the third metal chloride LiF is not included.
[0133] Comparative Example 9
[0134] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, annealing is not included.
[0135] Comparative Example 10
[0136] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the ratio of rest time to ball milling time is 1:0.01.
[0137] Comparative Example 11
[0138] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the ratio of rest time to ball milling time is 1:0.15.
[0139] The ionic conductivity of the oxyhalide solid electrolytes of Examples 1 to 15 and Comparative Examples 1 to 11 was tested at relative humidity of 0%, 5%, 10%, 15%, 20%, and 30%. The test results are shown in Table 1.
[0140] The test method is: place the powdered electrolyte in an airtight chamber with humidity and gas control, press the powdered electrolyte into a sheet electrolyte to be tested under a pressure of 300MPa, and then expose it to argon gas in a closed chamber with different humidity atmospheres for 12 hours. After loading the mold battery, an electrochemical impedance spectroscopy (EIS) test is performed.
[0141] Table 1:
[0142]
[0143]
[0144] From Table 1 we can see that:
[0145] Compared with the oxyhalide solid electrolytes of Comparative Examples 1 to 8, the oxyhalide solid electrolytes of Examples 1 to 15 have higher ionic conductivity at the same humidity, which shows that the oxyhalide solid electrolytes of the present application have good moisture resistance;
[0146] Compared with the oxyhalide solid electrolyte of Comparative Example 9, the oxyhalide solid electrolytes of Examples 1 to 15 have higher ionic conductivity at the same humidity, which shows that the annealing process can make the prepared oxyhalide solid electrolyte have better moisture resistance;
[0147] Compared with the oxyhalide solid electrolytes of Comparative Examples 10 to 11, the oxyhalide solid electrolytes of Examples 1 to 15 have higher ionic conductivity at the same humidity. It can be seen that within the resting and ball milling time ratio of the present application, the prepared oxyhalide solid electrolytes can have better moisture resistance.
[0148] Battery performance test
[0149] Battery composition: The positive electrode is LiNi8Co1Mn1O2, the electrolyte is the oxyhalide solid electrolyte of Example 1, and the negative electrode is Li 5.4 PS 4.4 Cl 1.6 Modified LiIn anode.
[0150] Test method: The modified negative electrode, 20 mg of the oxyhalide solid electrolyte powder of Examples 1, 8, 10 and Comparative Examples 1, 2, 8, and the positive electrode material are placed in a 10 mm mold battery in sequence, and the cold pressing and feeding process are repeated until the positive electrode is put in and compacted. Finally, an electrochemical impedance spectroscopy (EIS) test is performed at a given pressure of 50 MPa to obtain Figures 2 to 7 The electrochemical impedance spectrum (EIS graph) is shown.
[0151] Depend on Figure 2 , Figure 5 , Figure 6 It can be seen that when a and b are lower than the specified interval, the ionic conductivity of the product powder decreases significantly, while when a and b are higher than the interval, the decrease in ionic conductivity is relatively low.
[0152] Depend on Figure 3 and Figure 4 It can be seen that the ball-to-powder ratio and annealing temperature have a significant effect on the ionic conductivity of the product powder.
[0153] Depend on Figure 7 It can be seen that when the additive does not contain the third metal halide, the ion conductivity decreases extremely significantly, indicating the necessity of adding the third metal halide.
[0154] The oxyhalide solid electrolyte in Example 1 was characterized by X-ray powder diffraction, and the Figure 8 XRD pattern shown.
[0155] Depend on Figure 8 It can be seen that the phase structure of the oxyhalide solid electrolyte in Example 1 is a relatively pure single phase, and satisfies the situation that the crystal and amorphous phase exist at the same time. Among them, the crystal phase is mainly formed by mechanochemical reaction and annealing process, and according to previous research conclusions, the crystal phase-amorphous phase mixed phase system can provide better Li ion conductivity, and the appropriate crystal phase ratio can also provide moisture resistance.
[0156] The technical solutions provided by the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for technical personnel in this field, according to the idea of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. An oxyhalide solid electrolyte, characterized in that: The general formula of the oxyhalide solid electrolyte is Li 2a+ b M b O a X' c X” d , wherein M is selected from Ta, In or Zr, X is selected from halogen, 0.5≤a≤1.6, 1≤b≤1.5, 5≤c+d≤7.5, c and d are both numbers greater than 0; X' and X" are each independently selected from halogen, and X' and X" are different.
2. The oxyhalide solid electrolyte according to claim 1, characterized in that The halogen includes one or more of F, Cl, and Br.
3. The oxyhalide solid electrolyte according to claim 1, characterized in that The range of a is 0.5≤a≤0.8; and / or The range of b is 1≤b≤1.2; and / or The range of c+d is 5≤c+d≤6.
8.
4. The oxyhalide solid electrolyte according to claim 1, characterized in that The general formula of the oxyhalide solid electrolyte is Li 2.5 Ta 1.1 O 0.7 Cl 6.1 F 0.5 、Li2TaO 0.5 Cl 5.6 F 0.4 , Li 3.2 Zr 1.2 OCl5Br or more.
5. The oxyhalide solid electrolyte according to claim 1, characterized in that The ionic conductivity of the oxyhalide solid electrolyte is in the range of 10.7 to 11.8 mS / cm at a relative humidity of 0%; and / or The ionic conductivity of the oxyhalide solid electrolyte is in the range of 1.1 to 7.2 mS / cm at a relative humidity of 5%; and / or The ionic conductivity of the oxyhalide solid electrolyte is in the range of 0.28 to 2.2 mS / cm at a relative humidity of 10%; and / or The ionic conductivity of the oxyhalide solid electrolyte is in the range of 0.1 to 2.1 mS / cm at a relative humidity of 15%; and / or The ionic conductivity of the oxyhalide solid electrolyte is in the range of 0.02 to 0.8 mS / cm at a relative humidity of 20%; and / or The ionic conductivity of the oxyhalide solid electrolyte is in the range of 0.01-0.09 mS / cm when the relative humidity is 30%.
6. A method for preparing an oxyhalide solid electrolyte, characterized in that: The steps include: A first metal halide, a second metal halide, a third metal halide, and lithium oxide are mixed to obtain a mixture, wherein the chemical formula of the first metal halide is LiX', and the chemical formula of the second metal halide is MX' m , the chemical formula of the third metal halide is MX" n , X' and X" are each independently selected from halogen, and X' and X" are different, M is selected from Ta, In or Zr, and m and n are each independently selected from any integer from 1 to 5; ball-milling the mixture to obtain an oxyhalide solid electrolyte precursor; The oxyhalide solid electrolyte precursor is annealed to obtain an oxyhalide solid electrolyte.
7. The preparation method according to claim 6, characterized in that: The molar ratio of the lithium oxide, the first metal halide, the second metal halide and the third metal halide is (0.01-2):(0.01-2):(0.1-1.5):(0.1-1.5); and / or The mass ratio of the ball milling beads to the mixture is in the range of (8-20):1; and / or The halogen includes F, Cl or Br.
8. The preparation method according to claim 6, characterized in that: The equipment used for ball milling is a planetary ball mill; and / or The ball milling speed is 500-700 rpm; and / or The effective ball milling time is 70 to 200 hours; and / or The ratio of the rest time of the ball milling to the ball milling time is (0.1-1):1; and / or The annealing temperature is 100-300° C., and the annealing time is 30-180 minutes.
9. The preparation method according to claim 6, characterized in that: The mixing is performed under a protective atmosphere, and the gas in the protective atmosphere includes one or more of nitrogen, helium, neon, argon, krypton, and xenon.
10. A battery, characterized in that: It comprises the oxyhalide solid electrolyte according to any one of claims 1 to 5.
Citation Information
Cited By
A tantalum-doped hafnium-based oxyhalide solid-state electrolyte, a preparation method and applications
CN122992159A