A flame-retardant modified graphene oxide and its preparation method
By grafting organic molecular chains onto graphene oxide, the problem of poor compatibility between graphene oxide and nylon was solved, enabling the widespread application of flame-retardant modified graphene oxide in the textile field and improving the antistatic, flame-retardant, UV-resistant, and antioxidant properties of nylon.
Patent Information
- Application Number
- CN202410035340.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-10
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-01-10
AI Technical Summary
The poor compatibility of graphene oxide with nylon and the easy precipitation and poor durability of flame retardants limit its application in the textile field.
By grafting organic molecular chains onto graphene oxide to form amide group linkages, its interfacial compatibility with nylon is improved, and the introduction of DOPO structure as a flame retardant enhances its antistatic and flame retardant properties.
It improves the dispersibility and durability of graphene oxide in nylon, enhances the antistatic, flame retardant, UV resistant and antioxidant properties of the material, and strengthens the mechanical properties of nylon.
Smart Images

Figure BDA0004657496460000021 
Figure BDA0004657496460000031 
Figure BDA0004657496460000032
Abstract
Description
Technical Field
[0001] This invention belongs to the field of graphene material technology, specifically, it relates to a flame-retardant modified graphene oxide and its preparation method. Background Technology
[0002] Graphene is a two-dimensional honeycomb-like planar structure composed of a single layer of tightly packed carbon atoms. With a thickness of only 0.34 nm, it is the thinnest material known to date. This unique structural characteristic makes graphene the fundamental building block for constructing other dimensional carbon materials. Graphene possesses outstanding mechanical, electrical, thermal, and barrier properties.
[0003] Graphene oxide (GO) is a derivative of graphene and a novel carbon material. It has carboxylic acid functional groups at its edges and hydroxyl and epoxy groups on its surface. It has good dispersibility, hydrophilicity, and biocompatibility and is considered one of the most promising carbon materials in modern times.
[0004] Polyamide, commonly known as nylon (PA), has seen rapid development in recent years due to its outstanding characteristics such as high tensile strength, strong corrosion resistance, and fatigue resistance. It has wide applications in various industrial fields, including chemical fiber textiles, transportation, electronics, and construction, and is an important component of today's new materials industry. Fabrics made from nylon fibers, in particular, have experienced rapid growth in recent years. However, nylon has poor antistatic properties, easily causing static electricity accidents. Graphene oxide, on the other hand, possesses excellent antistatic properties. Blending it with nylon can significantly improve nylon's antistatic properties. However, graphene oxide is an inorganic material, and its compatibility with nylon is poor when directly blended. Furthermore, because nylon is flammable, traditional methods of directly adding various flame retardants can achieve a certain flame-retardant effect, but these are prone to precipitation and detachment, resulting in poor durability and limiting its application in the textile field. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a flame-retardant modified graphene oxide and its preparation method.
[0006] The objective of this invention can be achieved through the following technical solutions:
[0007] A method for preparing flame-retardant modified graphene oxide includes the following steps:
[0008] S1. In a three-necked flask equipped with a stirring reflux apparatus, p-chlorobenzaldehyde, 4-amino-2,2,6,6-tetramethylpiperidine, condensing agent and methanol are stirred and mixed evenly, and refluxed at 65°C for 2 hours. After the reaction is completed, part of the solvent is removed by rotary evaporation, and then purified by column chromatography (the eluent is a benzene / chloroform mixed solvent with a volume ratio of 1:3). The eluent is removed by rotary evaporation to obtain intermediate 1.
[0009] Under the action of a condensing agent, the aldehyde group on p-chlorobenzaldehyde condenses with the -NH2 group on 4-amino-2,2,6,6-tetramethylpiperidine to form an imine group (C=N Schiff base structure), yielding intermediate 1; the specific reaction process is shown below:
[0010]
[0011] S2. Under nitrogen protection, intermediate 1, DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide), AIBN (azobisisobutyronitrile), and DMF (N,N-dimethylformamide) were mixed in a three-necked flask equipped with a stirrer and reacted at 80°C for 6 hours. After the reaction was completed, the reaction was stopped, and part of the solvent was removed by vacuum distillation. Then, the mixture was purified by column chromatography (the eluent was a benzene / chloroform mixed solvent with a volume ratio of 4:1). The eluent was removed by rotary evaporation to obtain intermediate 2.
[0012] Catalyzed by AIBN, intermediate 1 reacts with DOPO to yield intermediate 2; the specific reaction process is shown below:
[0013]
[0014] S3. At room temperature and under nitrogen protection, intermediate 2, ethylenediamine, triethylamine and tetrahydrofuran were stirred and mixed evenly in a three-necked flask equipped with a stirring and reflux device. The reaction temperature was controlled at 80℃ and the reaction was refluxed for 4 hours. After the reaction was completed, triethylamine hydrochloride was removed by filtration, some solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of benzene and concentrated ammonia solution, with a volume ratio of 3:2). The eluent was removed by rotary evaporation to obtain intermediate 3.
[0015] Intermediate 2 undergoes nucleophilic substitution with ethylenediamine. By controlling the molar ratio of the two to be close to 1:1 and with a slight excess of ethylenediamine, only one amino group on the ethylenediamine participates in the reaction. Triethylamine removes the hydrogen chloride generated in the reaction, accelerating the reaction and yielding intermediate 3. The specific reaction process is shown below:
[0016]
[0017] S4. In a three-necked flask equipped with a stirrer, intermediate 3 was dissolved in DMF, and DCC (dicyclohexylcarbodiimide, dehydrating agent) was added and mixed evenly. Then, the graphene oxide dispersion was slowly added while magnetic stirring was applied. The mixture was ultrasonically treated for 30 minutes to ensure uniform dispersion. The reaction was carried out at 60°C for 6 hours with continuous stirring. After the reaction was completed, the mixture was distilled under reduced pressure, washed, and freeze-dried to obtain flame-retardant modified graphene oxide.
[0018] Under the action of DCC dehydrating agent, the reaction between carboxyl and amino groups can occur without very high conditions. Intermediate 3 is grafted onto graphene oxide to obtain flame-retardant modified graphene oxide; the specific reaction process is shown below:
[0019]
[0020] Furthermore, the condensing agent mentioned in step S1 is one of piperidine and DCC.
[0021] Furthermore, in step S1, the ratio of the amounts of p-chlorobenzaldehyde, 4-amino-2,2,6,6-tetramethylpiperidine, condensing agent, and methanol is 14.1 g: 15.6 g: 9.2 g: 100 mL.
[0022] Furthermore, in step S2, the ratio of intermediate 1, DOPO, AIBN, and DMSO is 27.8g:21.6g:0.5g:100mL.
[0023] Furthermore, in step S3, the ratio of intermediate 2, ethylenediamine, triethylamine, and tetrahydrofuran is 49.4g:10.5g:50mL:150mL.
[0024] Furthermore, in step S4, the ratio of intermediate 3, DMF, DCC, and graphene oxide dispersion is 51.8g:100mL:25.8g:200mL.
[0025] Furthermore, the graphene oxide dispersion in step S4 uses DMF as the dispersion medium and has a concentration of 1 mg / mL.
[0026] Furthermore, the graphene oxide-modified PA fabric is prepared through the following steps:
[0027] After vacuum drying, PA66 is placed in a twin-screw melt spinning machine with flame-retardant modified graphene oxide to obtain modified PA fibers. The modified PA fibers are then twisted to form yarns, which are used as warp yarns and woven into fabric using a circular knitting machine.
[0028] Furthermore, the mass ratio of PA66 to flame-retardant modified graphene oxide is 100:5-15.
[0029] The prepared flame-retardant modified graphene oxide is grafted with organic molecular chains through chemical bonding, forming an organic layer on its surface. This significantly improves the interfacial compatibility between graphene oxide and polycarbonate (PA), thereby promoting the uniform dispersion of modified graphene oxide in PA. Due to its excellent electrical conductivity, uniform dispersion in PA enhances its antistatic effect. Furthermore, as a reinforcing material, graphene oxide improves the impact strength and tensile strength of PA. Additionally, the grafting of organic molecular chains effectively prevents the migration and exudation of organic molecules, ensuring the durability of various properties. Moreover, the organic molecular chains contain DOPO structures, hindered amine structures, and amide groups; among which DOPO is a novel... The flame retardant is halogen-free, non-toxic, non-migrating, and has long-lasting flame retardant properties. It can also promote the dehydration of the material surface to form carbon elastomers, achieving condensed phase flame retardancy. It can endow PA with excellent flame retardancy while maintaining its mechanical properties. In addition, DOPO is a cyclic phosphate ester of phosphorus and phenanthrene, which can also endow PA with certain antioxidant properties. The hindered amine can act as a light stabilizer. In photoprotection, it decomposes hydrogen dioxide to generate stable nitrogen oxide free radicals. These groups can very effectively capture free radicals generated in photo-oxidative degradation, effectively inhibiting the photo-oxidative degradation of PA and giving PA high-efficiency UV resistance. Finally, the amide group improves the compatibility between graphene oxide and PA, allowing the performance of modified graphene oxide to be fully utilized.
[0030] The beneficial effects of this invention are:
[0031] The flame-retardant modified graphene oxide prepared in this invention is obtained by linking organic molecular chains to graphene oxide through amide groups. The organic molecular chains can improve the interfacial effect of graphene oxide, endowing graphene oxide with high flame retardancy, UV resistance and a certain degree of oxidation resistance, thus solving the problem of poor compatibility between graphene oxide and PA. Graphene oxide can effectively prevent the migration and exudation of organic molecules, thereby improving durability. In addition, graphene oxide itself has excellent antistatic properties and can act as a reinforcing material to improve the mechanical properties of PA. Therefore, the obtained flame-retardant modified graphene oxide has important application significance in the textile field. Detailed Implementation
[0032] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0033] Example 1
[0034] Preparation of flame-retardant modified graphene oxide
[0035] S1. In a three-necked flask equipped with a stirring reflux apparatus, 14.1 g of p-chlorobenzaldehyde, 15.6 g of 4-amino-2,2,6,6-tetramethylpiperidine, 9.2 g of piperidine, and 100 mL of methanol were stirred and mixed thoroughly. The mixture was refluxed at 65 °C for 2 h. After the reaction was completed, part of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a benzene / chloroform mixed solvent with a volume ratio of 1:3). The eluent was removed by rotary evaporation to obtain intermediate 1.
[0036] S2. Under nitrogen protection, 27.8 g of intermediate 1, 21.6 g of DOPO, 0.5 g of AIBN and 100 mL of DMF were mixed in a three-necked flask equipped with a stirrer and reacted at 80 °C for 6 h. After the reaction was completed, the reaction was stopped, and part of the solvent was removed by vacuum distillation. Then, the mixture was purified by column chromatography (the eluent was a benzene / chloroform mixed solvent with a volume ratio of 4:1). The eluent was removed by rotary evaporation to obtain intermediate 2.
[0037] S3. At room temperature and under nitrogen protection, 49.4 g of intermediate 2, 10.5 g of ethylenediamine, 50 mL of triethylamine and 150 mL of tetrahydrofuran were stirred and mixed evenly in a three-necked flask equipped with a stirring and reflux device. The reaction temperature was controlled at 80 °C and the mixture was refluxed for 4 h. After the reaction was completed, the triethylamine hydrochloride was removed by filtration, some of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of benzene and concentrated ammonia solution, with a volume ratio of 3:2). The eluent was removed by rotary evaporation to obtain intermediate 3.
[0038] S4. In a three-necked flask equipped with a stirrer, 51.8 g of intermediate 3 was dissolved in 100 mL of DMF, and 25.8 g of DCC was added and mixed evenly. Then, 200 mL of graphene oxide dispersion (using DMF as the dispersion medium with a concentration of 1 mg / mL) was slowly added while magnetically stirring. The mixture was ultrasonically treated for 30 min to ensure uniform dispersion. The reaction was carried out at 60 °C for 6 h with continuous stirring. After the reaction was completed, the mixture was distilled under reduced pressure, washed, and freeze-dried to obtain flame-retardant modified graphene oxide.
[0039] Example 2
[0040] Preparation of flame-retardant modified graphene oxide
[0041] S1. In a three-necked flask equipped with a stirring reflux apparatus, 28.2 g of p-chlorobenzaldehyde, 31.2 g of 4-amino-2,2,6,6-tetramethylpiperidine, 18.4 g of DCC and 200 mL of methanol were stirred and mixed thoroughly. The mixture was refluxed at 65 °C for 2 h. After the reaction was completed, part of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a benzene / chloroform mixed solvent with a volume ratio of 1:3). The eluent was removed by rotary evaporation to obtain intermediate 1.
[0042] S2. Under nitrogen protection, 55.6 g of intermediate 1, 43.2 g of DOPO, 1 g of AIBN and 200 mL of DMF were mixed in a three-necked flask equipped with a stirrer and reacted at 80 °C for 6 h. After the reaction was completed, the reaction was stopped, and part of the solvent was removed by vacuum distillation. Then, the mixture was purified by column chromatography (the eluent was a benzene / chloroform mixed solvent with a volume ratio of 4:1). The eluent was removed by rotary evaporation to obtain intermediate 2.
[0043] S3. At room temperature and under nitrogen protection, 98.8 g of intermediate 2, 21 g of ethylenediamine, 100 mL of triethylamine and 300 mL of tetrahydrofuran were stirred and mixed evenly in a three-necked flask equipped with a stirring and reflux device. The reaction temperature was controlled at 80 °C and the mixture was refluxed for 4 h. After the reaction was completed, the triethylamine hydrochloride was removed by filtration, some of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of benzene and concentrated ammonia solution, with a volume ratio of 3:2). The eluent was removed by rotary evaporation to obtain intermediate 3.
[0044] S4. In a three-necked flask equipped with a stirrer, 103.6 g of intermediate 3 was dissolved in 200 mL of DMF, and 51.6 g of DCC was added and mixed evenly. Then, 400 mL of graphene oxide dispersion (using DMF as the dispersion medium with a concentration of 1 mg / mL) was slowly added while magnetically stirring. The mixture was ultrasonically treated for 30 min to ensure uniform dispersion. The reaction was carried out at 60 °C for 6 h with continuous stirring. After the reaction was completed, the mixture was distilled under reduced pressure, washed, and freeze-dried to obtain flame-retardant modified graphene oxide.
[0045] Example 3
[0046] 100g of PA66 was vacuum dried and then placed in a twin-screw melt spinning machine with 5g of flame-retardant modified graphene oxide prepared in Example 1 to obtain modified PA fibers. The modified PA fibers were then twisted to form yarns, which were used as warp yarns and woven into fabric using a circular knitting machine.
[0047] Example 4
[0048] 100g of PA66 was vacuum dried and then placed in a twin-screw melt spinning machine with 10g of flame-retardant modified graphene oxide prepared in Example 2 to obtain modified PA fibers. The modified PA fibers were then twisted to form ply yarns, which were used as warp yarns and woven into fabric using a circular knitting machine.
[0049] Example 5
[0050] 100g of PA66 was vacuum dried and then placed in a twin-screw melt spinning machine with 15g of flame-retardant modified graphene oxide prepared in Example 2 to obtain modified PA fibers. The modified PA fibers were then twisted to form yarns, which were used as warp yarns and woven into fabric using a circular knitting machine.
[0051] Comparative Example
[0052] The flame-retardant modified graphene oxide in Example 5 was replaced with the same mass of ordinary graphene oxide, and the remaining steps were the same as in Example 5.
[0053] Examples 3-5 and the comparative examples were prepared into corresponding test shapes according to different standards, and the following performance tests were conducted:
[0054] The limiting oxygen index of the fabric after 30 washes was determined using the national standard GB / T 5454-1997 "Test for flammability of textiles - Oxygen Index Method".
[0055] The surface charge density was determined according to the national standard GB / T 12703.1-2008 "Evaluation of electrostatic properties of textiles" (the lower the surface charge density, the better the antistatic properties).
[0056] The ultraviolet shielding rate was determined according to the national standard GB / T 18830-2009 "Evaluation of Ultraviolet Protection Performance of Textiles";
[0057] The afterflame time and dripping conditions were determined according to the national standard GB / T 5455-2014 "Determination of vertical damage length, smoldering and afterflame time of textiles".
[0058] Tensile strength was determined according to the national standard GB / T 14337-2008 "Test Method for Tensile Properties of Chemical Fibers (Short Fibers)".
[0059] The measurement results are shown in the table below:
[0060]
[0061] As shown in the table above, the modified PA fabric, due to the addition of flame-retardant modified graphene oxide, exhibits superior properties compared to ordinary graphene oxide. Furthermore, the properties become even more outstanding with increasing amounts of flame-retardant modified graphene oxide. Therefore, the obtained flame-retardant modified graphene oxide has significant application value in the textile industry, especially for nylon modification.
[0062] In the description of this specification, the references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0063] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.
Claims
1. A method for preparing flame-retardant modified graphene oxide, characterized in that, Includes the following steps: S1. Mix p-chlorobenzaldehyde, 4-amino-2,2,6,6-tetramethylpiperidine, condensing agent and methanol evenly, reflux at 65°C for 2 h, evaporate by rotary evaporation, purify by column chromatography, evaporate by rotary evaporation to obtain intermediate 1; Under nitrogen protection, intermediate 1, DOPO, AIBN and DMF were mixed and reacted at 80°C for 6 h. The mixture was then purified by vacuum distillation, column chromatography and rotary evaporation to obtain intermediate 2. S3. At room temperature and under nitrogen protection, intermediate 2, ethylenediamine, triethylamine and tetrahydrofuran were stirred and mixed evenly. The reaction temperature was controlled at 80℃ and the mixture was refluxed for 4 hours. After filtration, rotary evaporation, column chromatography purification and rotary evaporation were performed to obtain intermediate 3. S4. Dissolve intermediate 3 in DMF, add DCC and mix thoroughly; add graphene oxide dispersion while stirring magnetically, sonicate for 30 min, react at 60℃ for 6 h with continuous stirring, distill under reduced pressure, wash, and freeze dry to obtain flame-retardant modified graphene oxide. In step S1, the condensing agent is one of piperidine and DCC; the ratio of p-chlorobenzaldehyde, 4-amino-2,2,6,6-tetramethylpiperidine, condensing agent, and methanol in step S1 is 14.1g:15.6g:9.2g:100mL; the ratio of intermediate 1, DOPO, AIBN, and DMSO in step S2 is 27.8g:21.6g:0.5g:100mL; the ratio of intermediate 2, ethylenediamine, triethylamine, and tetrahydrofuran in step S3 is 49.4g:10.5g:50mL:150mL; and the ratio of intermediate 3, DMF, DCC, and graphene oxide dispersion in step S4 is 51.8g:100mL:25.8g:200mL.
2. The method for preparing flame-retardant modified graphene oxide according to claim 1, characterized in that, The graphene oxide dispersion in step S4 uses DMF as the dispersion medium and has a concentration of 1 mg / mL.
Citation Information
Patent Citations
Preparation method and application of modified graphene nano filling material
CN104804477A
Graphene containing DOPO group and preparation method thereof
CN105001451A