A composite phase change material for thermal regulation of high specific energy battery pack

By combining dual-phase change materials with animal fats and crystalline hydrated salts, using anti-corrosion and toning sterilizers, and dry ice bubbling to form a porous structure, the problem of heat regulation and stability of battery packs in near-space vehicles has been solved, and high ratios have been achieved. It can ensure the excellent cycle performance and long-term reliability of the battery pack.

CN117887426BActive Publication Date: 2024-10-18TIANJIN UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410082307.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-19
Publication Date
2024-10-18
Estimated Expiration
2044-01-19

AI Technical Summary

Technical Problem

In high-specific-energy battery packs of near-space vehicles, there is a lack of effective normal temperature control technology to solve the problems of low temperature gradient and waste heat conversion and utilization. Especially in independent thermal insulation systems, the stability and reliability of traditional phase change materials are limited. .

Method used

It adopts a dual-phase change material combination of inorganic and organic materials, takes advantage of the difference in hydrophilicity and hydrophobicity of animal fats and crystalline hydrated salts, prevents deterioration through antiseptic detergents and toning and sterilizing agents, and combines dry ice bubbles to form a porous structure to achieve Heat regulation and stability improvement.

Benefits of technology

It has improved the heat control capability and stability of high-specific energy battery packs, extended the service life of phase change materials, and ensured the reliability and safety of the battery pack in complex load environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117887426B_ABST
    Figure CN117887426B_ABST
Patent Text Reader

Abstract

The present invention discloses a composite phase change material for thermal regulation of a high-energy-density battery pack; the composite phase change material is composed of 10% to 90% of a first phase change material, 5% to 85% of a second phase change material, and 5% to 40% of a functional additive; the phase change temperature range is 20°C to 60°C. The first phase change material includes animal fat, a preservative and a deteriorating agent, and a color-adjusting sterilizing agent, and the second phase change material is a crystalline hydrate salt. The composite phase change material utilizes the hydrophobicity of animal fat and the hydrophilicity of crystalline hydrates to achieve the common phase change energy storage of organic and inorganic materials, solves the technical problem of performance differences caused by temperature gradients in low-temperature and low-pressure environments in near-space for high-energy-density batteries, prolongs the cycle life of the battery pack, and enhances the effective endurance time provided by all-electric aircraft. The preparation method of the present invention has the characteristics of simple process, safety and reliability, batch stability, and large-scale preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of secondary power sources, and in particular relates to a high-energy-density battery pack thermal regulation composite phase change material. Background Art

[0002] Near-space refers to a space region with an altitude of 20 to 100 km, located at the junction of the atmosphere and space, and is between the flight space of ordinary aircraft and the orbital space of spacecraft. Currently, only high-altitude scientific balloons can operate stably and for a long time here. "Near-space aircraft" equipment refers to aircraft that use near-space to destroy and interfere with space targets (more than 100 km from the ground) and implement communications, telemetry, reconnaissance, transportation, interception and attack on land, sea and air targets. The cost of near-space aircraft is lower than that of satellites, and the working time is longer than that of aircraft. Therefore, in the case of being separated from the ground power supply, it is necessary to develop high-energy-density power supply technology.

[0003] In the working environment of near-space aircraft, the use of thermal insulation measures such as aerogel to isolate heat exchange can effectively prevent heat exchange with the outside world. Low air pressure and high vacuum weaken convection behavior. The absorption and reflection coating on the equipment weakens thermal radiation. How to solve the problem of low temperature gradient and waste heat conversion and utilization of high-energy thermal battery packs in a highly independent insulation system, and help large battery packs maintain the consistency of the working environment and the reliability of electrical performance, lack of efficient normal temperature control technology. In current research, there are many studies on the use of phase change materials to control heat, but there are very few studies on normal temperature phase change materials. For example, CN109135684A thermal battery uses molten salt for phase change heat storage. Molten salt has the disadvantage of high melting point as a phase change material; CN109802196A studies the phase change temperature control of crystalline hydrated salts such as calcium chloride hexahydrate. Although it is a normal temperature phase change material, calcium chloride hexahydrate is conductive and absorbs moisture after melting, which will cause the phase change material to be unstable and reduce reliability. It cannot be used alone as a normal temperature phase change material to control the heat of the power system. Animal fats, represented by lard and butter, are high in saturated fat and calories. They are generally used as human nutrition and a reasonable dietary intake, and are often the subject of nutrition or cosmetic research. However, due to the presence of water and oxygen in the earth's environment, microorganisms breed, and animal fats are prone to mold and deterioration. They have a short shelf life and a low melting point, making it difficult to use them as phase change materials for power thermal regulation research in practical scenarios.

[0004] In our concurrent research, we found that the use of lard, animal-derived oil and calcium chloride hexahydrate, and the use of pore-forming agents to form a porous structure to construct phase change materials can provide a better technical solution for room temperature phase change temperature control, especially lard has a long shelf life in a dry and cold environment. However, lard is prone to deterioration and corruption when left alone in humid and warm weather, and even mildew will occur during the rainy season, seriously reducing the safety of the battery pack and the reliability of room temperature control. The main reason is the hydrolysis and rancidity of the main component triglycerides and the growth and reproduction of microorganisms. The core reason for both is the water content in the material. Reducing the free water content, especially reducing the generation of free water in the intermediate chemical process, is of great significance for preventing animal fat corruption and increasing the service life of phase change materials. In addition, with the deepening of research, there are differences in the melting points of animal fats, and there will also be differences in the selection of phase change materials. For example, lard is 28-48°C, chicken fat and duck fat is 22-28°C, and butter is 40-46°C. When the difference in properties is small, there is a lack of direct means to intuitively and quickly distinguish animal fats in a solidified state. Summary of the invention

[0005] Based on the above technical application background, the present invention proposes a high specific energy battery pack thermal regulation composite phase change material, especially using antiseptics to prevent animal fats from hydrolyzing and rancidifying, using coloring sterilizers to improve the identification of animal fat types, and inhibiting microbial growth. More importantly, physical methods are used to form pores without reaction by-products, which can prevent the formation of free water in the intermediate chemical process. The core technical points of the present invention are:

[0006] 1. Dual phase change materials at room temperature that combine inorganic and organic rigidity and flexibility

[0007] The present invention uses materials with completely different properties to construct room temperature phase change materials. The first phase change material is organic animal fats and oils, the main component of which is triglyceride, which belongs to the hydrophobic material, and mainly utilizes the solid-liquid phase change to absorb and store heat. The second type of phase change material is crystalline hydrated salts, which belongs to the hydrophilic material, and mainly utilizes solid-liquid conversion. The dissociated water formed after the solid-liquid conversion has a higher specific heat capacity. The present invention just takes advantage of the difference in hydrophilicity and hydrophobicity of the two materials. First, it realizes the dissociation and combination of crystal water in a specific bound area, ensuring that the formed high specific heat capacity free water has a greater heat storage capacity to better regulate heat. Second, animal fats and oils can avoid the influence of the outside world (water and oxygen) on the second type of phase change material that is easy to deliquesce, ensuring the reliability of the performance of the phase change material. In addition, oil substances have good lubrication and shock absorption effects, and can adapt to the complex load environment faced by aerospace.

[0008] 2. Water limitation control and animal fat anti-corrosion and anti-deterioration

[0009] The deterioration of animal fats is mainly caused by oxidation and microorganisms. Since animal fats are used to coat crystalline hydrates, hydrates are confined to micro-regions. Therefore, the hydrophobic and hydrophilic differences of the two materials can achieve the limited control of crystal water. In addition, only water dissociates and combines in the micro-region, shielding the unfavorable factors that cause oxidation due to the simultaneous presence of water and oxygen. The joint action of the two can slow down the innate conditions of animal fat oxidation from the reaction area and reaction depth, and can effectively prevent the deterioration of fats. Secondly, crystalline hydrates have strong deliquescent hygroscopic properties, which can frantically dispatch free water around fats, allowing hydrophobic fats to continue to dry and prevent fats from hydrolyzing. Even if part of the crystal water is lost in the long-term phase change equilibrium, the newly formed anhydrous salt has a stronger hygroscopic capacity, which further prevents fats from hydrolyzing. Then traditional antiseptic additives are added to the fats, which can prevent the growth of microorganisms, reduce the generation of fat free radicals, slow down the deterioration of animal fats, and maintain the phase change material in a long-term working state. Finally, the present invention strictly controls the water-oxygen conditions and microbial growth. The fats are not only conducive to sterilization and elimination of microorganisms during high-temperature melting and refining, but also conducive to the release of free water.

[0010] 3. Highly stable color-adjusting sterilizing agent

[0011] The present invention uses inorganic substances with stable chemical properties and high color saturation as colorants to distinguish the types of phase change materials characterized by raw materials, melting points, phase change enthalpy, etc., which is conducive to rapid identification. The inorganic substances (such as cinnabar and orpiment) used neither react with oil nor change with water during long-term storage, and have high color recognition. It is particularly important that the material used has a stable morphological structure and excellent antibacterial and bactericidal ability. Some substances can destroy the protein structure of microorganisms and can prevent the influence of microorganisms and molds when the phase change material is stored in non-adjacent space.

[0012] 4. Non-conductive functional additives

[0013] Although phase change materials have good phase change heat storage capacity, they generally have poor thermal conductivity, such as the animal fats and water in dissociated or combined forms in the present invention. Therefore, carbon-based, metal-based or ionic molten salts are introduced into traditional phase change materials, which have strong thermal conductivity and strong electrical conductivity, and the two are generally positively correlated. There is a risk of high-voltage leakage in high-energy-density battery packs, so the functional additives introduced in the present invention, such as beryllium oxide, silicon nitride, etc., have both high thermal conductivity and good insulation properties, which can meet the insulation requirements of electronic components and currents inside high-energy-density battery packs in near space.

[0014] 5. Dry ice bubbling promotes the control of water-free environment

[0015] The present invention uses dry ice to form inert bubbles. Compared with the traditional method of adding surfactants or gas generators, new impurities (such as calcium carbonate), water, and oxygen may be introduced, and even the components of animal fats may be changed, increasing uncertainty. Therefore, the formation of chemically inert bubbles has a high technical difficulty. The present invention adds powdered dry ice to viscous animal fats. The low temperature of dry ice allows the fats to cool and condense rapidly. Under the action of rapid tumbling and stirring, the ungasified dry ice particles are wrapped therein. After the dry ice is completely gasified, the generated carbon dioxide gas is confined therein due to the viscous animal fat coating, and the long-term continuous stirring and dispersion effect forms a paste in which bubbles are dispersed. After the paste is condensed, a gas-dispersed solid phase material is obtained, and then the bubble transfer is promoted according to the low pressure state of the adjacent space, leaving a solid-phase porous composite phase change material with bubble holes. Therefore, the present invention does not introduce other products in the whole process, especially the dry ice bubbling method is a physical process, which does not cause chemical damage to the original material, does not generate byproduct water or other substances, and the preparation method is simple, rough, efficient, and reliable. In addition, in the concurrent research of the present invention, the porous structure of the phase change material can adapt well to the low pressure environment, and the bubbling of dry ice and low pressure treatment can better prevent the material components (such as carbon dioxide bubbles) from being deformed and damaged by the changes in internal and external air pressure, thereby affecting reliability.

[0016] Specifically, the purpose of the present invention is achieved through the following technical solutions:

[0017] The present invention relates to a thermally controlled composite phase change material, which consists of a first phase change material, a second phase change material, and a functional additive, and the phase change temperature range is 20°C to 60°C; the first phase change material includes animal fat, a preservative deteriorating agent, and a coloring sterilizing agent, and the second phase change material is a crystalline hydrate salt.

[0018] As an embodiment of the present invention, the mass proportion of each component in the composite phase change material is: 10% to 90% of the first phase change material, 5% to 85% of the second phase change material, and 5% to 40% of the functional additive. The two phase change materials can be freely matched according to design needs. It is generally not recommended that the first phase change material, that is, the animal fat phase change material, is too low, preferably 30% to 90% (at this time the second phase change material is 5% to 65%). If it is too low, the animal fat cannot fully cover the second type of phase change material. The proportion of the second type of phase change material can be determined according to the design state. If the proportion of functional additives is too low, the effect is not obvious. If it is too high, the amount of phase change material is reduced and the heat regulation ability is poor.

[0019] As an embodiment of the present invention, the animal fat includes at least one of lard, beef tallow, sheep tallow, horse fat, dog fat, chicken fat, duck fat, goose fat, camel fat, yak fat, donkey fat, fish oil, whale oil, bear fat, cat fat, butter, cream and other animal fats. Preferably, at least one of lard, beef tallow, sheep tallow, donkey fat, yak fat, dog fat, butter and cream is used. There are many types of animal fats and oils, which cannot be listed one by one. Preferably, the animal fats and oils are easy to obtain, abundant in output and low in cost.

[0020] As an embodiment of the present invention, the preservatives include at least one of vitamins, citric acid, benzoic acid, potassium sorbate, nitrite, butylated hydroxyanisole BHA, butylated hydroxytoluene ether BHT, sodium sulfate, sodium isoascorbate, sodium nitrate, sodium sulfite, and soybean oil.

[0021] As an embodiment of the present invention, the coloring sterilizing agent includes at least one of cinnabar (HgS), iron oxide (Fe2O3), realgar (As4S4), orpiment (As2S3), arsenic (As2O3), nickel oxide (NiO), titanium dioxide (TiO2), and malachite (Cu2(OH)2CO3). The coloring sterilizing agent has a highly recognizable color, stable chemical properties, antibacterial and sterilization capabilities, and some are toxic. Although the present invention studies animal fat additives, it is based on the field of materials science, not food nutrition research, and reference personnel should not eat or eat by mistake.

[0022] As an embodiment of the present invention, the functional additive includes at least one of beryllium oxide, aluminum oxide, magnesium oxide, silicon dioxide, aluminum nitride, boron nitride, silicon nitride, and silicon carbide.

[0023] As an embodiment of the present invention, the melting point or dehydration temperature of the crystalline hydrate salt does not exceed 100°C. Preferably, the melting point or dehydration temperature of the crystalline hydrate salt is between 20 and 100°C. Preferably, at least one of calcium chloride hexahydrate, sodium thiosulfate pentahydrate, sodium sulfate decahydrate, ferric chloride hexahydrate, manganese chloride tetrahydrate, manganese chloride hexahydrate, ferrous sulfate heptahydrate, potassium aluminum sulfate dodecahydrate, sodium hydrogen sulfate monohydrate, and sodium acetate trihydrate. The crystalline hydrate salt should be dried with ventilation at 20°C before use to reduce the influence of moisture-absorbing free water.

[0024] The present invention also relates to a method for preparing a thermally regulated composite phase change material, comprising: adding dry ice powder to a paste-like composite phase change material obtained by mixing a first phase change material, a second phase change material, and a functional additive, and rapidly tumbling and stirring the material to ensure that the paste quickly wraps the dry ice powder, and after the dry ice sublimates, a paste-like composite phase change material with bound carbon dioxide bubbles is obtained; after solidifying in an environment of -10 to 20°C, the material is placed in a low pressure environment of 100 to 5000 Pa for more than 1 hour to obtain a porous composite phase change material.

[0025] As an embodiment of the present invention, a method for preparing a thermally regulated composite phase change material comprises the following steps:

[0026] S1. Preparation of the first phase change material: After heating and refining the animal fat, cool it down to 30-70°C, add the preservative and deterioration agent and the coloring sterilizer in sequence, continue stirring, and cool it down to 20-50°C to form the first phase change material;

[0027] S2. Preparation of composite phase change material: weigh the second phase change material and the functional adsorbent in proportion, add them to the first phase change material respectively, stir continuously, mix evenly, and obtain a paste-like composite phase change material;

[0028] S3, dry ice bubbling: adding dry ice powder to the paste-like composite phase change material, rapidly tumbling and stirring at a speed of 100 to 1000 r / min to ensure that the paste quickly wraps the dry ice powder, and after the dry ice sublimates, a paste-like composite phase change material with bound carbon dioxide bubbles is obtained;

[0029] S4. Porosification: After solidifying the paste-like composite phase change material with bound carbon dioxide bubbles in an environment of -10 to 20°C, the paste-like composite phase change material is placed in a low pressure environment of 100 to 5000 Pa for more than 1 hour to obtain a porous composite phase change material.

[0030] The preparation method of the present invention needs to be carried out in an environment with a humidity of less than 3% or a water and oxygen value of less than 1 ppm, such as a drying room with a humidity of less than 3%, or an argon protection glove box with a water and oxygen value of less than 1 ppm.

[0031] As an embodiment of the present invention, step S2 further includes a microbial sterilization step, specifically: sterilizing the obtained paste-like composite phase change material with anhydrous ethanol and ultraviolet light successively. Alternatively, after step S4, sterilizing the obtained porous composite phase change material with anhydrous ethanol and ultraviolet light successively.

[0032] As an embodiment of the present invention, in step S1, animal fat is placed in a container and heated to be refined; the temperature may be 80°C to 200°C.

[0033] As an embodiment of the present invention, in step S3, the particle size of the dry ice powder is 50μm to 5mm. The amount of dry ice relative to the paste-like composite phase change material is in the range of 1wt% to 10wt%, which is determined specifically according to the design state. In addition, dry ice needs to be of appropriate particle size. If the particle size is too small or too little, it will sublime quickly, and carbon dioxide bubbles cannot be obtained or the amount of bubbles obtained is small. If the particle size is too large, the carbon dioxide dispersion effect is poor. If the particle size is too large, the bubbles may be too large, resulting in bubble explosion, causing hot oil splashing, causing scalding or causing equipment safety hazards.

[0034] As an embodiment of the present invention, in step S4, the sample is placed in a low pressure environment of 100 to 5000 Pa for 10 min to 6 h.

[0035] The present invention also relates to a use of a thermally regulated composite phase change material in a thermally regulated high-energy-density battery pack, wherein the thermally regulated composite phase change material is filled in the internal space gap of the battery pack; the high-energy-density battery pack is temperature-controlled and regulated. Specifically, it is used to reduce the temperature gradient difference of the high-energy-density battery pack in the low-temperature and low-pressure environment of near space.

[0036] As an embodiment of the present invention, the paste-like composite phase change material obtained by mixing the first phase change material, the second phase change material, and the functional additive is subjected to dry ice bubbling treatment to obtain a paste-like composite phase change material with bound carbon dioxide bubbles; the bubbled paste-like composite phase change material is injected into the internal space gaps of the battery pack (such as the space gaps of the battery cells), placed in an environment of -10 to 20°C for solidification, and then the battery pack is placed in a low pressure environment of 100 to 5000 Pa for more than 1 hour to obtain a porous composite phase change material.

[0037] As an embodiment of the present invention, the high specific energy battery includes a lithium ion battery, a metal lithium battery, and a sodium ion battery.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] 1) The composite phase change material prepared by the present invention has hydrophilic crystalline hydrate and hydrophobic animal fat, which can utilize solid-liquid phase change to store heat. In addition, the dissociated water of the crystalline hydrate has a high specific heat capacity, so it has good heat regulation ability and can maintain high specific energy battery pack with excellent cycle performance;

[0040] 2) The present invention uses the method of oil-in-crystallized hydrate to achieve limited control of water, prevent the coexistence of water and oxygen, weaken the innate conditions for the oxidation of animal fats, and use preservatives to prevent animal fats from corrosion and deterioration, thereby extending the storage life of the phase change material;

[0041] 3) The highly stable color-adjusting sterilizing agent has a color with high color saturation, which is convenient for classification and quick identification; and the color-adjusting sterilizing agent has excellent antibacterial and sterilization ability, which prevents the phase change material from mildewing during long-term storage;

[0042] 4) Non-conductive functional additives have good thermal conductivity, but phase change materials are insulating materials, which are beneficial to the insulation protection and use of high-energy-density battery packs.

[0043] 5) The method of the present invention adopts the dry ice bubbling method. The pore-forming method is a physical process, which does not cause chemical damage to the original material, does not produce process byproducts such as water or other substances, and has high quality reliability;

[0044] 6) The raw materials of the present invention are cheap, the equipment is simple, and the method is simple, efficient, and fast, which is conducive to quantitative production. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0046] Figure 1 This is a schematic diagram of the raw material lard;

[0047] Figure 2 It is the DSC test curve diagram of Example 1;

[0048] Figure 3 The temperature variation curve of the high specific energy battery pack of Application Example 1 and Comparative Example 1 in the environment of -70°C and 7000Pa is shown;

[0049] Figure 4 The charge and discharge performance curves of the high specific energy battery pack of Application Example 1 and Comparative Example 1 in an environment of -70°C and 7000Pa;

[0050] Figure 5 Schematic diagram of the space before and after a typical phase change material is injected into an ultra-high specific energy battery pack. DETAILED DESCRIPTION

[0051] The present invention is described in detail below in conjunction with embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0052] Example 1

[0053] A formula of a high specific energy battery pack thermal regulation composite phase change material is shown in Table 1:

[0054] Table 1 Composite phase change material formula 1

[0055] substance The first phase change material Second phase change material Preservatives Color Sterilizer Function Enhancer Material lard <![CDATA[Na2SO4·10H2O]]> Vitamin E Titanium dioxide Boron Nitride percentage 50% 24% 1% 5% 20%

[0056] A method for preparing a high-energy-density battery pack thermally controlled composite phase change material, in a dry environment with a humidity of less than 1% (dew point less than -40°C), with 100g / batch preparation as a reference, specifically comprising the following steps:

[0057] S1. Preparation of the first phase change material: animal fat lard ( Figure 1) is placed in a stainless steel container for heating and refining for 10 minutes until it boils without producing white steam, then cooled to 45°C, and vitamin E as a preservative and titanium dioxide (TiO2) as a colorant and sterilizer are added in sequence, stirred for 10 minutes, and cooled to 30°C to form a first phase change material.

[0058] S2. Preparation of composite phase change material: weigh the second phase change material sodium sulfate decahydrate and the functional additive boron nitride in proportion, add them to the first phase change material respectively, stir continuously, mix evenly, and obtain a paste-like composite phase change material.

[0059] S3. Dry ice bubbling: Add dry ice powder with a particle size of about 1 mm at an amount of 1 g / time into the paste-like composite phase change material, and stir rapidly (reference stirring speed 300 r / min) to ensure that the paste quickly wraps the dry ice powder. Add once every 10 minutes for a total of 6 times. After the dry ice sublimates, a paste-like composite phase change material with bound carbon dioxide bubbles is obtained.

[0060] S4, Porosification: Inject the bubble paste composite phase change material into the internal space gap of the battery pack (such as Figure 5 As shown), put it in a -10°C environment for 2 hours, and after it is completely solidified, place the battery pack in a low pressure environment of 1700 Pa for more than 1 hour to obtain a porous composite phase change material.

[0061] S5. Disinfection of microorganisms: The obtained porous composite phase change material is sprayed with anhydrous ethanol for disinfection, and after it evaporates, it is sterilized with ultraviolet light for 1 hour.

[0062] The high specific energy battery pack thermal control composite phase change material treated as above was subjected to DSC analysis. The test curve is as follows Figure 2 shown.

[0063] Example 2

[0064] A formula of a high specific energy battery pack thermal regulation composite phase change material is shown in Table 2:

[0065] Table 2 Composite phase change material formula 1

[0066] substance The first phase change material Second phase change material Preservatives Color Sterilizer Function Enhancer Material Lard + Butter <![CDATA[CaCl2·6H2O]]> benzoic acid realgar Alumina percentage 40%+15% 15% 0.5% 1.5% 28%

[0067] A method for preparing a high-energy-density battery pack thermally controlled composite phase change material, in a dry environment with a humidity of less than 1% (dew point less than -40°C), with 100g / batch preparation as a reference, specifically comprising the following steps:

[0068] S1. Preparation of the first phase change material: Put animal fats lard and beef tallow into a stainless steel container and heat and refine for 10 minutes until it boils without producing white steam, cool to 45°C, add preservative benzoic acid and colorant sterilizer realgar powder (As4S4) in sequence, continue stirring for 10 minutes, and cool to 32°C to form the first phase change material.

[0069] S2. Preparation of composite phase change material: weigh the second phase change material sodium sulfate decahydrate and the functional additive aluminum oxide in proportion, add them to the first phase change material respectively, stir continuously, mix evenly, and obtain a paste-like composite phase change material.

[0070] S3. Dry ice bubbling: Add dry ice powder with a particle size of about 1 mm at an amount of 1 g / time into the paste-like composite phase change material, and stir rapidly (reference stirring speed 300 r / min) to ensure that the paste quickly wraps the dry ice powder. Add once every 10 minutes for a total of 6 times. After the dry ice sublimates, a paste-like composite phase change material with bound carbon dioxide bubbles is obtained.

[0071] S4. Porosification: Inject the bubbled paste composite phase change material into the internal space gap of the battery pack, place it in a -20°C environment for 1 hour, wait for it to completely solidify, and then place the battery pack in a low pressure environment of 1700 Pa for more than 1 hour to obtain a porous composite phase change material.

[0072] S5. Disinfection of microorganisms: The obtained porous composite phase change material is sprayed with anhydrous ethanol for disinfection, and after it evaporates, it is sterilized with ultraviolet light for 1 hour.

[0073] Example 3

[0074] A formula of a high specific energy battery pack thermal regulation composite phase change material is shown in Table 3:

[0075] Table 3 Composite phase change material formula 1

[0076] substance The first phase change material Second phase change material Preservatives Color Sterilizer Function Enhancer Material Lard + Butter <![CDATA[Na2S2O3·5H2O]]> Butylated Hydroxyanisole Cinnabar Aluminum Nitride percentage 5%+45% 20% 0.8% 1.2% 28%

[0077] A method for preparing a high-energy-density battery pack thermally controlled composite phase change material, in a dry environment with a humidity of less than 1% (dew point less than -40°C), with 100g / batch preparation as a reference, specifically comprising the following steps:

[0078] S1. Preparation of the first phase change material: Put animal fats lard and beef tallow into a stainless steel container and heat and refine for 10 minutes until boiling without producing white steam, cool to 45°C, add preservative butyl hydroxyanisole (BHA) and colorant sterilizer cinnabar powder (HgS) in sequence, continue stirring for 10 minutes, and cool to 40°C to form a first phase change material.

[0079] S2. Preparation of composite phase change material: Weigh the second phase change material sodium thiosulfate pentahydrate (Na2S2O3·5H2O) and the functional additive aluminum nitride in proportion, add them to the first phase change material respectively, continue stirring, mix evenly, and obtain a paste-like composite phase change material.

[0080] S3. Dry ice bubbling: Add dry ice powder with a particle size of about 1 mm at an amount of 1 g / time into the paste-like composite phase change material, and stir rapidly (reference stirring speed 300 r / min) to ensure that the paste quickly wraps the dry ice powder. Add once every 10 minutes for a total of 6 times. After the dry ice sublimates, a paste-like composite phase change material with bound carbon dioxide bubbles is obtained.

[0081] S4. Porosification: Inject the bubbled paste composite phase change material into the internal space gap of the battery pack, place it in a -10°C environment for 1 hour, wait for it to completely solidify, and then place the battery pack in a low pressure environment of 1700 Pa for more than 1 hour to obtain a porous composite phase change material.

[0082] S5. Disinfection of microorganisms: The obtained porous composite phase change material is sprayed with anhydrous ethanol for disinfection, and after it evaporates, it is sterilized with ultraviolet light for 1 hour.

[0083] Application Example 1

[0084] The application example adopts a design capacity of 22Ah for the battery cell, and a specific energy of about 570Wh / kg at a charge and discharge rate of 0.2C. The battery manufacturing refers to the previous results (authorized invention patent ZL202111063559.5). The overall battery design scheme can adopt a high-nickel ternary positive electrode (commercially available), a metal lithium negative electrode (Tianjin Zhongneng Lithium Industry Co., Ltd.), and the electrolyte of Example 1 in ZL202111063559.5. 48 battery cells (about 7kg) manufactured in the same batch are connected in series to design a battery pack. The battery shell adopts aluminum-magnesium alloy + aerogel + carbon fiber. The paste-like composite phase change materials S1-S3 in the preparation method of Example 1 are injected into the gaps of the battery cells in the battery pack, and then the battery pack is treated according to the methods S4-S5 in Example 1. The total mass of the battery pack increases to 7.9kg. The high specific energy thermal battery pack loaded with composite phase change materials was placed in a -70°C, 7000pa environment for charge and discharge cycles. The initial specific energy of the battery pack was 490.6Wh / kg, and the specific energy after 30 cycles was 426.5Wh / kg ( Figure 3 ) and compared the temperature changes at different locations of the battery pack, and found that the battery pack temperature was maintained at around 28°C ( Figure 4 ).

[0085] Comparative Example 1

[0086] The comparative example uses a battery cell with a design capacity of 22Ah, and a specific energy of about 570Wh / kg at a charge and discharge rate of 0.2C. The battery manufacturing refers to the previous results (authorized invention ZL202111063559.5). The overall battery design scheme can use a high-nickel ternary positive electrode (commercially available), a metal lithium negative electrode (Tianjin Zhongneng Lithium Co., Ltd.) and the electrolyte of Example 1 in ZL202111063559.5. 48 battery cells (about 7kg) manufactured in the same batch were connected in series to design a battery pack. The battery shell is made of aluminum-magnesium alloy + aerogel + carbon fiber. On the basis of not using phase change materials, the total mass of the battery pack is about 7.8kg. The battery is placed in a -70°C, 7000pa environment for charge and discharge cycles. The overall initial specific energy of the battery pack is 483.9.1Wh / kg, and the specific energy after 30 cycles is 340.4Wh / kg ( Figure 3 ), it was found that the temperature of the battery pack was very different at different locations ( Figure 4 ).

[0087] Application Example 2

[0088] The composite phase change material with a melting point of 25 to 35°C is treated with titanium dioxide as a coloring and antibacterial agent, and the phase change material becomes milky white;

[0089] The composite phase change material with a melting point of 35 to 45°C is treated with orpiment as a coloring and antibacterial agent, and the phase change material is yellow;

[0090] The composite phase change material with a melting point above 45° C. uses iron red or cinnabar as a coloring and antibacterial agent, and the phase change material is red.

[0091] The specific specifications and colors can be adjusted to prevent bacteria according to the design status and actual conditions.

[0092] Comparative Example 2

[0093] Put lard into a stainless steel container and heat it for 10 minutes until it boils without producing white steam. Then cool it to 45°C, add vitamin E as a preservative and titanium dioxide (TiO2) as a colorant and sterilizer, and continue stirring for 10 minutes. After condensation, a solid first phase change material is obtained.

[0094] When the first phase change material and lard were stored in an environment of 25±5°C and 80% humidity for 30 days, the lard turned yellow, rancid and spoiled, and had an unpleasant rancid smell, while the first phase change material did not change in appearance and had no unpleasant rancid smell, indicating that the addition of preservatives and colorants and sterilizers can extend the shelf life of lard and ensure the performance of lard.

[0095] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A thermally controlled composite phase change material, characterized in that: The composite phase change material is composed of 10% to 90% of a first phase change material, 5% to 85% of a second phase change material, and 5% to 40% of a functional additive, and the phase change temperature range is 20°C to 60°C; the first phase change material includes animal fat, a preservative deterioration agent, and a coloring sterilizing agent, and the second phase change material is a crystalline hydrate salt; The animal fat comprises at least one of lard, beef tallow, sheep tallow, horse tallow, dog tallow, chicken tallow, duck tallow, goose tallow, camel tallow, donkey tallow, fish tallow, whale tallow, bear tallow, cat tallow, and butter; The crystalline hydrate salt is at least one of calcium chloride hexahydrate, sodium thiosulfate pentahydrate, sodium sulfate decahydrate, ferric chloride hexahydrate, manganese chloride tetrahydrate, ferrous sulfate heptahydrate, potassium aluminum sulfate dodecahydrate, sodium hydrogen sulfate monohydrate, and sodium acetate trihydrate.

2. The thermally controlled composite phase change material according to claim 1, characterized in that: The animal fat is at least one of lard, beef tallow, sheep tallow, donkey fat, dog fat and butter.

3. The thermally controlled composite phase change material according to claim 1, characterized in that: The preservatives include at least one of vitamins, benzoic acid, potassium sorbate, nitrite, butylated hydroxyanisole BHA, butylated hydroxytoluene ether BHT, sodium sulfate, sodium isoascorbate, sodium nitrate and sodium sulfite.

4. The thermally controlled composite phase change material according to claim 1, characterized in that: The color-adjusting sterilizer includes at least one of cinnabar HgS, iron oxide red Fe2O3, realgar As4S4, orpiment As2S3, arsenic As2O3, nickel oxide NiO, titanium dioxide TiO2, and malachite Cu2(OH)2CO3; the functional additive includes at least one of beryllium oxide, aluminum oxide, magnesium oxide, silicon dioxide, aluminum nitride, boron nitride, silicon nitride, and silicon carbide.

5. The thermally controlled composite phase change material according to claim 1, characterized in that: The melting point or dehydration temperature of the crystalline hydrate salt does not exceed 100°C.

6. A method for preparing a thermally controlled composite phase change material according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: S1. Preparation of the first phase change material: After heating and refining the animal fat, cool it down to 30-70°C, add the preservative and deterioration agent and the coloring sterilizer in sequence, continue stirring, and cool it down to 20-50°C to form the first phase change material; S2. Preparation of composite phase change material: weigh the second phase change material and the functional adsorbent in proportion, add them to the first phase change material respectively, stir continuously, mix evenly, and obtain a paste-like composite phase change material; S3, dry ice bubbling: adding dry ice powder to the paste-like composite phase change material, rapidly tumbling and stirring at a speed of 100 to 1000 r / min to ensure that the paste quickly wraps the dry ice powder, and after the dry ice sublimates, a paste-like composite phase change material with bound carbon dioxide bubbles is obtained; S4. Porosification: After solidifying the paste-like composite phase change material with bound carbon dioxide bubbles in an environment of -10 to 20°C, the paste-like composite phase change material is placed in a low pressure environment of 100 to 5000 Pa for more than 1 hour to obtain a porous composite phase change material.

7. Use of the thermally regulated composite phase change material according to any one of claims 1 to 5 in a thermally regulated high specific energy battery pack, characterized in that: The thermal regulation composite phase change material is filled in the internal space gap of the battery pack.

8. The use according to claim 7, characterized in that The paste-like composite phase change material obtained by mixing the first phase change material, the second phase change material and the functional additive is subjected to dry ice bubbling treatment to obtain a paste-like composite phase change material with bound carbon dioxide bubbles; the bubbled paste-like composite phase change material is injected into the internal space gap of the battery pack, placed in an environment of -10 to 20°C for solidification, and then the battery pack is placed in a low pressure environment of 100 to 5000 Pa for more than 1 hour to obtain a porous composite phase change material.

9. The use according to claim 7, characterized in that: The high specific energy battery includes a lithium ion battery, a metal lithium battery, and a sodium ion battery.

Citation Information

Patent Citations

  • Composite phase change material for thermal batteries and method for preparing composite phase change material

    CN109135684A

  • Rapid battery heating device with hydrated salt phase change material

    CN109802196A

  • Lithium electrolyte of solvent self-sacrifice in-situ protection electrode, preparation and application thereof

    CN113782810A

  • Preparation method of high-crystallization enthalpy value low-temperature phase transition nanometer cold storage material

    CN105838330A

  • Composition of phase-change material and preparing method of composition

    CN109609102A