Method, device, electronic device and medium for calculating composite crack shape factor
By performing axial high-period fatigue test and calculation of composite calculation formulas on nickel-based single-crystal high-temperature alloys, the problem that the existing technology cannot obtain its composite crack shape factor is solved, and the accuracy of the cracking characteristics of nickel-based single-crystal high-temperature alloys is achieved. Characterization and fatigue stress analysis.
Patent Information
- Application Number
- CN202410107535.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-01-25
AI Technical Summary
Existing calculation tools cannot effectively obtain the composite crack shape factor of nickel-based single-crystal high-temperature alloys, and cannot characterize their cracking characteristics.
Provide a calculation method and device for composite crack shape factor, collect the crack characteristics of nickel-based single crystal high-temperature alloy through axial high-period fatigue test, and calculate the composite crack shape factor Y composite by using the composite calculation formula, including Type I and II Calculation formulas for type and type III crack shape factors.
It realizes effective characterization of cracking characteristics of nickel-based single-crystal high-temperature alloys, provides accurate quantitative analysis of fatigue stress fractures, and meets engineering requirements.
Smart Images

Figure CN117894414B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of quantitative analysis of fatigue fracture of metal materials in metallurgical technology, and more specifically, to a method, device, electronic equipment and medium for calculating a composite crack shape factor. Background Art
[0002] Nickel-based single crystal high-temperature alloys use a directional solidification process to eliminate grain boundaries, reduce grain boundary strengthening elements that lower the melting point, and increase the initial melting temperature of the alloy. Given its excellent high-temperature properties, it is widely used in the manufacture of turbine hot end components of advanced aircraft engines.
[0003] The inventors of this application have found in practice that nickel-based single crystal high-temperature alloys are different from conventional steel and aluminum materials and have their own unique cracking characteristics. At 980°C and below, fatigue cracks in nickel-based single crystal high-temperature alloys mainly start from the octahedral slip system, with the main slip plane being the 111 plane, which forms a certain angle with the 001 plane in the load application direction, causing its slip plane to present a type I / II / III composite crack. However, existing calculation tools can only calculate the shape factor of type I cracks, and there is no corresponding technical means to obtain the composite crack shape factor that characterizes the cracking characteristics of nickel-based single crystal high-temperature alloys. Summary of the invention
[0004] In view of this, the present application provides a method, device, electronic device and medium for calculating a composite crack shape factor, which are used to obtain a composite crack shape factor that characterizes the cracking characteristics of a nickel-based single crystal high-temperature alloy.
[0005] In order to achieve the above objectives, the proposed solution is as follows:
[0006] A method for calculating a composite crack shape factor is applied to electronic equipment to obtain a composite crack shape factor capable of characterizing high cycle fatigue cracking characteristics of a nickel-based single crystal high temperature alloy. The method comprises the following steps:
[0007] Collecting crack characteristics of a high-cycle fatigue fracture surface of a sample when performing an axial high-cycle fatigue test on the sample, wherein the sample is a nickel-based single crystal high-temperature alloy bar of a specified size;
[0008] The crack characteristics are calculated based on the specified composite calculation formula to obtain the composite crack shape factor Y 复合 , the composite calculation formula is:
[0009]
[0010] Among them, Y Ι β is the mode I crack shape factor, is the crack shape factor of mode II, is the shape factor of mode III crack.
[0011] Optionally, the collecting of the high cycle fatigue life of the sample and the crack characteristics of the high cycle fatigue fracture surface when the sample is subjected to an axial high cycle fatigue test comprises the steps of:
[0012] Designing and processing a test specimen;
[0013] Performing an axial high cycle fatigue test on the sample under equal stress amplitude based on different load levels;
[0014] The front and side faces of the high cycle fatigue fracture surface of the sample are observed and recorded based on a stereo microscope to obtain the crack characteristics.
[0015] Optionally, the calculation formula of the type I crack shape factor is:
[0016] Y Ι β =Y Ι ×sin 2 β
[0017] Among them, Y I The crack front shape factor of the sample, β, is the angle between the normal direction of the main slip surface of the sample and the stress application direction.
[0018] Optionally, the crack front shape factor Y I The calculation formula is:
[0019]
[0020] Among them, F I is the crack correction factor, and E(k) is the complete elliptic integral of the second kind.
[0021] Optionally, the calculation formula of the crack correction factor is:
[0022]
[0023] Wherein, x1=a / D, x2=a / b, m0-m5 are constants, D is the actual diameter of the high cycle fatigue fracture surface, a is the crack half length of the high cycle fatigue fracture surface, and b is the crack half width of the high cycle fatigue fracture surface;
[0024] The formula for the second kind of complete elliptic integral is:
[0025]
[0026] Optionally, the mode II crack shape factor is an empirical value.
[0027] Optionally, the calculation formula of the mode III crack shape factor is:
[0028]
[0029] Wherein, ν is the material parameter Poisson's ratio of the sample.
[0030] A composite crack shape factor computing device is applied to electronic equipment and is used to obtain a composite crack shape factor capable of characterizing cracking characteristics of a nickel-based single crystal high-temperature alloy. The computing device comprises:
[0031] A parameter acquisition module is configured to acquire crack characteristics of a high-cycle fatigue fracture surface of a sample when an axial high-cycle fatigue test is performed on the sample, wherein the sample is a nickel-based single crystal high-temperature alloy bar of a specified size;
[0032] The calculation execution module is configured to calculate the crack characteristics based on a specified composite calculation formula to obtain the composite crack shape factor Y 复合 , the composite calculation formula is:
[0033]
[0034] Among them, Y Ι β is the mode I crack shape factor, is the crack shape factor of mode II, is the shape factor of mode III crack.
[0035] An electronic device comprises at least one processor and a memory connected to the processor, wherein:
[0036] The memory is used to store computer programs or instructions;
[0037] The processor is used to execute the computer program or instruction so that the electronic device can implement the above-mentioned operation method.
[0038] A medium is applied to an electronic device, wherein the storage medium carries one or more computer programs, and the one or more computer programs can be executed by the electronic device, so that the electronic device can implement the above-mentioned operation method.
[0039] It can be seen from the above technical scheme that the present application discloses a method, device, electronic device and medium for calculating a composite crack shape factor. The method and device are applied to electronic devices to obtain a composite crack shape factor that can characterize the cracking characteristics of a nickel-based single crystal high-temperature alloy. Specifically, the method collects the crack characteristics of the high-cycle fatigue fracture surface of the sample when the sample is subjected to an axial high-cycle fatigue test. The sample is a nickel-based single crystal high-temperature alloy bar of a specified size. The crack characteristics are calculated based on a specified composite calculation formula to obtain a composite crack shape factor. This solves the problem that there is currently no corresponding technical means to obtain a composite crack shape factor that characterizes the cracking characteristics of a nickel-based single crystal high-temperature alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0041] Figure 1 A flow chart of a method for calculating a composite crack shape factor according to an embodiment of the present application;
[0042] Figure 2 Images of the front and side surfaces of the fracture surface obtained after the axial high cycle fatigue test;
[0043] Figure 3 The crack diagram of the calculation model of the crack shape factor on the cylindrical semi-elliptical surface;
[0044] Figure 4 This is a schematic diagram of the oblique crack on the side of the high cycle fatigue fracture crack;
[0045] Figure 5 is the ratio error between the modeled cylindrical semi-elliptical surface crack shape factor and the actual value;
[0046] Figure 6 A block diagram of a computing device for a composite crack shape factor according to an embodiment of the present application;
[0047] Figure 7 A block diagram of an electronic device according to an embodiment of the present application. DETAILED DESCRIPTION
[0048] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0049] Figure 1 The present invention is a flowchart of a method for calculating a composite crack shape factor according to an embodiment of the present application.
[0050] like Figure 1 As shown, the calculation method provided in this embodiment is applied to an electronic device for calculating the composite crack shape factor of a nickel-based single crystal high-temperature alloy. The electronic device can be understood as a computer, server or cloud platform with information processing and data computing capabilities. The calculation method includes the following process.
[0051] S1. Crack characteristics of high cycle fatigue fracture surface of collected specimens.
[0052] The high cycle fatigue fracture surface is produced when the sample is subjected to an axial high cycle fatigue test. The sample is a nickel-based single crystal high temperature alloy bar of specified size. The crack characteristics are collected by the following means:
[0053] First, a sample as mentioned above is designed and processed, that is, a rod of a nickel-based single crystal high-temperature alloy of a certain size.
[0054] Then, an axial high-cycle fatigue test was carried out on the rod under test parameters of different stresses and different load levels at equal stress amplitude. After the test, the test life was recorded, and the high-cycle fatigue fracture surface generated by the rod during the test was obtained.
[0055] Finally, the front and side faces of the high cycle fatigue fracture surface were observed and recorded using a stereo microscope to obtain the crack characteristics.
[0056] in, Figure 2The images of the front and side faces of the fracture obtained after the axial high-cycle fatigue test. From the front face of the fracture, the crack source area, extension ridges, crystallographic slip planes, brittle fatigue bands and other features can be seen, all of which are traces left during the crack extension process. According to the convergence direction of the extension ridges, the location of the crack source area can be determined. According to the statistics of multiple fracture features, the crack origin of the nickel-based single crystal alloy is near the surface of the sample, and irregular casting looseness (voids) can be seen at the source area. According to the characteristics of the brittle fatigue band, the shape of the crack during the crack extension process can be observed. The shape of the fatigue arc is depicted, and it can be seen that the front edge of the crack is elliptical and has a certain boundary with the surface of the sample. The above fracture features are similar to elliptical semi-elliptical surface cracks. From the side face of the fracture, it can be seen that the fracture as a whole is a large inclined surface with a certain angle to the load application direction. It is an oblique crack, which is significantly different from traditional polycrystalline materials such as aluminum alloys and steel.
[0057] Figure 3 The schematic diagram of the crack shape factor calculation model of the cylindrical semi-elliptical surface crack, in which the cross section is perpendicular to the load application direction. From the cross-sectional shape, it can be seen that the crack front is elliptical as a whole; a is the half-length of the crack, and b is the half-width of the crack.
[0058] Figure 4 The figure is a schematic diagram of the side oblique crack of the high cycle fatigue fracture crack, which is the characteristic of type I / II / III composite oblique crack. The oblique crack is at a certain angle to the load application direction, which is defined as β in this application.
[0059] Figure 5 This is the error calculation of the correction factor for the semi-elliptical surface crack of a cylinder. The specific error values are shown in the following table:
[0060]
[0061]
[0062] In order to digitally model its value, a binary quadratic function mathematical model containing interactive terms is used to establish the relationship between the correction factor and the ratio of crack length to fracture surface diameter (a / D) and the ratio of crack length to width (a / b). Different (a / D) values are substituted into the established model to obtain the crack shape factor values under different (a / D) conditions. The values obtained by the model are compared with the values in the table to obtain the error. The relative error range is 0.41-4.13%, which meets the needs of daily inspection and engineering.
[0063] S2. Calculate the composite crack shape factor based on the specified composite calculation formula.
[0064] Specifically, the shape factor reflecting the crack characteristics is calculated by a pre-specified composite calculation formula to obtain the composite crack shape factor Y 复合 , the composite calculation formula is:
[0065]
[0066] Among them, Y Ι β is the mode I crack shape factor, is the crack shape factor of mode II, is the shape factor of mode III crack.
[0067] The calculation formula for the mode I crack shape factor is:
[0068] Y Ι β =Y Ι ×sin 2 β
[0069] Among them, Y I The crack front shape factor of the specimen, β, is the angle between the normal direction of the main slip plane of the specimen and the stress application direction.
[0070] Nickel-based single crystal high-temperature alloy is a face-centered cubic crystal. According to the crystal plastic slip theory, the octahedral slip system is mainly activated below 980°C, that is, the main slip plane is the (111) plane. The crack will crack along the main slip plane and then form microcracks and expand. The crack surface and the main slip plane are in the same plane. Therefore, the angle β between the crack surface and the stress application direction is calculated using the following formula.
[0071]
[0072] Wherein, the
[111] direction is the normal direction of the main slip plane (111) of the Ni-based single crystal alloy, and the
[001] direction is the stress application direction, which is also the growth direction of the crystal of the Ni-based single crystal high temperature alloy.
[0073] The calculation formula of mode II crack shape factor is: It is usually an empirical value, and the specific value can be 1.25.
[0074] Calculation formula for mode III crack shape factor The specific calculation is obtained through the following formula:
[0075] Where ν is the material parameter Poisson’s ratio of the specimen.
[0076] The crack front shape factor Y in the calculation formula of the above type I crack shape factor is I The calculation formula is:
[0077]
[0078] Among them, F Iis the crack correction factor, and E(k) is the complete elliptic integral of the second kind.
[0079] The crack correction factor is related to two parameters, namely the ratio of crack length to fracture surface diameter (a / D) and the ratio of crack half length to half width (a / b). In order to more accurately characterize the relationship between the correction factor and the two parameters, this application expresses the relationship between the correction factor and the two parameters using a binary quadratic function mathematical model containing an interaction term. The calculation formula of the factor is:
[0080]
[0081] In addition, the correction factor F Ι Refer to the correction factor for cylindrical semi-elliptical surface cracks in the Stress Intensity Factor Handbook. The handbook lists a variety of basic types of crack shape factor calculation methods, which can be selected according to the high-cycle fatigue cracking form of nickel-based single crystal high-temperature alloys.
[0082] In addition, the formula for the second kind of complete elliptic integral is:
[0083]
[0084] Among them, x1=a / D, x2=a / b, m0~m5 are constants, D is the actual diameter of the high cycle fatigue fracture surface, a is the crack half length of the high cycle fatigue fracture surface, and b is the crack half width of the high cycle fatigue fracture surface.
[0085] It can be seen from the above technical solution that this embodiment provides a method for calculating a composite crack shape factor, which is applied to electronic equipment and is used to obtain a composite crack shape factor that can characterize the cracking characteristics of a nickel-based single crystal high-temperature alloy. Specifically, the method collects the crack characteristics of the high-cycle fatigue fracture surface of the sample when the sample is subjected to an axial high-cycle fatigue test, and the sample is a nickel-based single crystal high-temperature alloy bar of a specified size; the crack characteristics are calculated based on a specified composite calculation formula to obtain a composite crack shape factor. This solves the problem that there is currently no corresponding technical means to obtain a composite crack shape factor that characterizes the cracking characteristics of a nickel-based single crystal high-temperature alloy.
[0086] Taking the high cycle fatigue specimen of nickel-based high temperature alloy DD6 as an example, the specific implementation steps of this application are as follows:
[0087] (1) Design and process rod-shaped high-cycle fatigue specimens, use stress control, and carry out axial high-cycle fatigue tests under equal stress amplitudes. The specimens are numbered D6H227 and D6H246, the temperature is 850℃, the stress ratio R=-1, the applied stress range Δσ=900MPa, and the specimen life is recorded after the test as shown in the table below, and high-cycle fatigue fractures are obtained.
[0088]
[0089] (2) Use a stereo microscope to observe the front and side of the fracture, and take photos to record. Obtain the crack characteristics of high-cycle fatigue cracks in nickel-based single crystal alloys. From the side of the fracture, it can be seen that the high-cycle fatigue cracks of nickel-based single crystal high-temperature alloys are oblique cracks, that is, they are at a certain angle to the stress application direction, showing the characteristics of I / II / III type composite cracking, as shown in Figure 1. Figure 2 From the front of the fracture, it can be seen that in the second stage of crack extension, traces left during the crack extension process can be seen, and its outline is elliptical, which is a typical elliptical crack.
[0090] (3) According to the observed crack characteristics, the crack shape factor of the basic type of cylindrical specimen listed in the Stress Intensity Factor Handbook is selected, that is, the cylindrical semi-elliptical surface crack. This model is suitable for type I cracking, that is, the crack direction is perpendicular to the stress application direction, and it needs to be selected and adjusted according to the composite crack. The crack front shape factor calculation formula is:
[0091]
[0092] Where Y Ι is the type I crack shape factor, E(k) is calculated using the following formula, where the crack shape correction factor F Ι .
[0093]
[0094] Where a is the crack half-length and b is the crack half-width.
[0095] (4) Crack correction factor F Ι It is related to two parameters, the ratio of crack length to fracture surface diameter (a / D) and the ratio of crack half length to half width (a / b). In order to more accurately characterize the relationship between the correction factor and the two parameters and facilitate further application, the relationship between the correction factor and the two parameters is expressed by a binary quadratic function mathematical model containing an interaction term, as shown in the following formula.
[0096]
[0097] In the formula, D is the actual diameter of the cross section, x1=a / D, x2=a / b, and m0~m5 are constants.
[0098] Solve the constants in the formula according to the data in the sample life table to obtain the following formula:
[0099]
[0100] Where x1 = a / D, x2 = a / b. Then, the crack front shape factor expression is:
[0101]
[0102] (5) In the present application, the high cycle fatigue crack form of the nickel-based single crystal high temperature alloy is a composite oblique crack of type I / II / III, and the calculation formula of the composite crack shape factor is:
[0103]
[0104] Among them, Y Ι β =Y Ι ×sin 2 β, Y Ι β is the crack shape factor of mode I, is the II crack shape factor, is the shape factor of the mode III crack, Y 复合 is the shape factor of type I / II / III composite crack. β angle is the angle between the normal direction of the main slip plane of the nickel-based single crystal superalloy specimen and the stress application direction.
[0105] Nickel-based single crystal high-temperature alloy is a face-centered cubic crystal. According to the crystal plastic slip theory, below 980°C, the octahedral slip system is mainly activated, that is, the main slip plane is the (111) plane. The crack will crack along the main slip plane and then form microcracks and expand. The crack surface and the main slip plane are in the same plane. Therefore, the angle β between the crack surface and the stress application direction is calculated using the following formula, and the theoretical β is 35.3°.
[0106]
[0107] Wherein, the
[111] direction is the normal direction of the main slip plane of the Ni-based single crystal superalloy (111), and the
[001] direction is the stress application direction, which is also the growth direction of the Ni-based single crystal alloy.
[0108] According to the above formula, Y can be calculated 复合 The expression is as follows.
[0109]
[0110] The crack shape factor has a significant impact on the quantitative analysis results of the fatigue stress fracture of the specimen. In order to verify the effectiveness of the calculation results of the high-cycle fatigue composite crack shape factor of the Ni-based single crystal alloy by this method. The calculated crack shape factor is used to perform quantitative analysis and calculation of the high-cycle fatigue stress fracture of the Ni-based single crystal alloy. It can be seen from the calculation results that compared with the actual stress results of the specimen, the error range is between 1.04 and 1.27. The error range is between 1.04 and 1.27, which is enough to realize the accurate calculation of fatigue stress and meet the needs of engineering calculations. The specific calculation results are shown in the following table.
[0111] Table 1 D6H246 R=-1 stress calculation results
[0112]
[0113]
[0114] Table 2 D6H227 R=-1 stress calculation results
[0115]
[0116] The flow chart and block diagram in the accompanying drawings illustrate the possible architecture, function and operation of the system, method and computer program product according to various embodiments of the present disclosure. In this regard, each square box in the flow chart or block diagram can represent a module, a program segment or a part of a code, and the module, the program segment or a part of the code contains one or more executable instructions for realizing the specified logical function. It should also be noted that in some implementations as replacements, the functions marked in the square box can also occur in a sequence different from that marked in the accompanying drawings. For example, two square boxes represented in succession can actually be executed substantially in parallel, and they can sometimes be executed in the opposite order, depending on the functions involved. It should also be noted that each square box in the block diagram and / or flow chart, and the combination of the square boxes in the block diagram and / or flow chart can be implemented with a dedicated hardware-based system that performs a specified function or operation, or can be implemented with a combination of dedicated hardware and computer instructions.
[0117] Although operations are depicted in a particular order, this should not be understood as requiring that the operations be performed in the particular order shown or in a sequential order.Multitasking and parallel processing may be advantageous under certain circumstances.
[0118] It should be understood that the various steps described in the method embodiments of the present disclosure may be performed in different orders and / or in parallel. In addition, the method embodiments may include additional steps and / or omit the steps shown. The scope of the present disclosure is not limited in this respect.
[0119] Computer program code for performing the operations of the present disclosure may be written in one or more programming languages or a combination thereof, including, but not limited to, object-oriented programming languages, such as Java, Smalltalk, C++, and conventional procedural programming languages, such as C or similar programming languages. The program code may be executed entirely on the user's computer, partially on the user's computer, as a separate software package, partially on the user's computer and partially on a remote computer, or entirely on a remote computer or server. In cases involving a remote computer, the remote computer may be connected to the user's computer through any type of network, including a local area network (LAN) or a wide area network (WAN), or may be connected to an external computer.
[0120] Figure 6 This is a block diagram of a device for calculating a composite crack shape factor according to an embodiment of the present application.
[0121] like Figure 6 As shown, the computing device provided in this embodiment is applied to an electronic device for calculating the composite crack shape factor of a nickel-based single crystal high-temperature alloy. The electronic device can be understood as a computer, server or cloud platform with information processing and data computing capabilities. The computing device includes a parameter acquisition module 10 and a computing execution module 20.
[0122] The parameter acquisition module is used to collect the crack characteristics of the high cycle fatigue fracture surface of the specimen.
[0123] The high cycle fatigue fracture surface is generated when the sample is subjected to an axial high cycle fatigue test. The sample is a nickel-based single crystal high temperature alloy bar of specified size. Specifically, this module collects crack characteristics by the following means:
[0124] First, a sample as mentioned above is designed and processed, that is, a rod of a nickel-based single crystal high-temperature alloy of a certain size.
[0125] Then, an axial high-cycle fatigue test was carried out on the rod under test parameters of different stresses and different load levels at equal stress amplitude. After the test, the test life was recorded, and the high-cycle fatigue fracture surface generated by the rod during the test was obtained.
[0126] Finally, the front and side faces of the high cycle fatigue fracture surface were observed and recorded using a stereo microscope to obtain the crack characteristics.
[0127] The calculation execution module is used to calculate the composite crack shape factor based on a specified composite calculation formula.
[0128] Specifically, the crack characteristics are calculated by a pre-specified composite calculation formula to obtain the composite crack shape factor Y复合 The specific execution process is as described above and will not be repeated here.
[0129] It can be seen from the above technical solution that this embodiment provides a device for calculating a composite crack shape factor, which is applied to electronic equipment and is used to obtain a composite crack shape factor that can characterize the cracking characteristics of a nickel-based single crystal high-temperature alloy. Specifically, the device collects the crack characteristics of the high-cycle fatigue fracture surface of the sample when the sample is subjected to an axial high-cycle fatigue test. The sample is a nickel-based single crystal high-temperature alloy bar of a specified size; the crack characteristics are calculated based on a specified composite calculation formula to obtain a composite crack shape factor. This solves the problem that there is currently no corresponding technical means to obtain a composite crack shape factor that characterizes the cracking characteristics of a nickel-based single crystal high-temperature alloy.
[0130] The units involved in the embodiments described in the present disclosure may be implemented by software or hardware. The name of a unit does not limit the unit itself in some cases. For example, the first acquisition unit may also be described as a "unit for acquiring at least two Internet Protocol addresses".
[0131] The functions described above herein may be performed at least in part by one or more hardware logic components. For example, without limitation, exemplary types of hardware logic components that may be used include: field programmable gate arrays (FPGAs), application specific integrated circuits (ASICs), application specific standard products (ASSPs), systems on chips (SOCs), complex programmable logic devices (CPLDs), and the like.
[0132] Figure 7 The block diagram is a block diagram of an electronic device according to an embodiment of the present application.
[0133] refer to Figure 7 As shown, it shows a schematic diagram of the structure of an electronic device suitable for implementing the embodiments of the present disclosure. The terminal device in the embodiments of the present disclosure may include but is not limited to mobile terminals such as mobile phones, laptops, digital broadcast receivers, PDAs (personal digital assistants), PADs (tablet computers), PMPs (portable multimedia players), vehicle-mounted terminals (such as vehicle-mounted navigation terminals), etc., and fixed terminals such as digital TVs, desktop computers, etc. The electronic device is only an example and should not bring any limitations to the functions and scope of use of the embodiments of the present disclosure.
[0134] The electronic device may include a processing device (e.g., a central processing unit, a graphics processing unit, etc.) 701, which can perform various appropriate actions and processes according to a program stored in a read-only memory ROM 702 or a program loaded from an input device 706 into a random access memory RAM 703. In the RAM, various programs and data required for the operation of the electronic device are also stored. The processing device, ROM, and RAM are connected to each other via a bus 704. An input / output (I / O) interface 705 is also connected to the bus 704.
[0135] Typically, the following devices may be connected to the I / O interface: input devices including, for example, a touch screen, a touchpad, a keyboard, a mouse, a camera, a microphone, an accelerometer, a gyroscope, etc.; output devices 707 including, for example, a liquid crystal display (LCD), a speaker, a vibrator, etc.; storage devices 708 including, for example, a magnetic tape, a hard disk, etc.; and communication devices 709. The communication device 709 may allow the electronic device to communicate with other devices wirelessly or by wire to exchange data. Although the figure shows an electronic device with various devices, it should be understood that it is not required to implement or have all the devices shown. More or fewer devices may be implemented or have alternatively.
[0136] This embodiment also provides a computer-readable medium.
[0137] The computer-readable medium is applied to an electronic device and carries one or more computer programs. When the one or more computer programs are executed by the electronic device, the electronic device is used to obtain a composite crack shape factor that can characterize the cracking characteristics of a nickel-based single crystal high-temperature alloy. Specifically, the crack characteristics of the high-cycle fatigue fracture surface of the sample are collected when the sample is subjected to an axial high-cycle fatigue test. The sample is a nickel-based single crystal high-temperature alloy bar of a specified size. The crack characteristics are calculated based on a specified composite calculation formula to obtain a composite crack shape factor. This solves the problem that there is currently no corresponding technical means to obtain a composite crack shape factor that characterizes the cracking characteristics of a nickel-based single crystal high-temperature alloy.
[0138] It should be noted that the computer-readable medium disclosed above may be a computer-readable signal medium or a computer-readable storage medium or any combination of the above two. The computer-readable storage medium may be, for example, but not limited to, an electrical, magnetic, optical, electromagnetic, infrared, or semiconductor system, device or device, or any combination of the above. More specific examples of computer-readable storage media may include, but are not limited to: an electrical connection with one or more wires, a portable computer disk, a hard disk, a random access memory (RAM), a read-only memory (ROM), an erasable programmable read-only memory (EPROM or flash memory), an optical fiber, a portable compact disk read-only memory (CD-ROM), an optical storage device, a magnetic storage device, or any suitable combination of the above.
[0139] In the present disclosure, a computer-readable storage medium may be any tangible medium containing or storing a program that may be used by or in combination with an instruction execution system, apparatus, or device. In the present disclosure, a computer-readable signal medium may include a data signal propagated in a baseband or as part of a carrier wave, which carries a computer-readable program code. Such propagated data signals may take a variety of forms, including but not limited to electromagnetic signals, optical signals, or any suitable combination of the above. A computer-readable signal medium may also be any computer-readable medium other than a computer-readable storage medium, which may send, propagate, or transmit a program for use by or in combination with an instruction execution system, apparatus, or device. The program code contained on the computer-readable medium may be transmitted using any suitable medium, including but not limited to: wires, optical cables, RF (radio frequency), etc., or any suitable combination of the above.
[0140] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0141] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.
[0142] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or terminal device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or terminal device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or terminal device including the elements.
[0143] The technical solution provided by the present invention is introduced in detail above. Specific examples are used in this article to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for calculating a composite crack shape factor, applied to electronic equipment, for obtaining a composite crack shape factor capable of characterizing high cycle fatigue cracking characteristics of a nickel-based single crystal high temperature alloy, characterized in that: The operation method comprises the steps of: Collecting crack characteristics of a high-cycle fatigue fracture surface of a sample when performing an axial high-cycle fatigue test on the sample, wherein the sample is a nickel-based single crystal high-temperature alloy bar of a specified size; The crack characteristics are calculated based on the specified composite calculation formula to obtain the composite crack shape factor Y 复合 , the composite calculation formula is: Among them, Y Ι β is the mode I crack shape factor, is the crack shape factor of mode II, is the shape factor of mode III crack; The calculation formula of the I-type crack shape factor is: AND Ι β =And Ι ×without 2 β Among them, Y I The crack front shape factor of the sample, β is the angle between the normal direction of the main slip surface of the sample and the stress application direction; The type II crack shape factor is an empirical value; The calculation formula of the mode III crack shape factor is: Wherein, ν is the material parameter Poisson's ratio of the sample.
2. The calculation method according to claim 1, characterized in that: The method of collecting crack characteristics of a high cycle fatigue fracture surface of a sample when the sample is subjected to an axial high cycle fatigue test comprises the following steps: Designing and processing a test specimen; Performing an axial high cycle fatigue test on the sample under equal stress amplitude based on different load levels; The front and side faces of the high cycle fatigue fracture surface of the sample are observed and recorded based on a stereo microscope to obtain the crack characteristics.
3. The calculation method according to claim 1, characterized in that: The crack front shape factor Y I The calculation formula is: Among them, F I is the crack correction factor, and E(k) is the complete elliptic integral of the second kind.
4. The calculation method according to claim 3, characterized in that: The calculation formula of the crack correction factor is: Wherein, x1=a / D, x2=a / b, m0-m5 are constants, D is the actual diameter of the high cycle fatigue fracture surface, a is the crack half length of the high cycle fatigue fracture surface, and b is the crack half width of the high cycle fatigue fracture surface; The formula for the second kind of complete elliptic integral is:
5. A composite crack shape factor computing device, applied to electronic equipment, for obtaining a composite crack shape factor capable of characterizing high cycle fatigue cracking characteristics of a nickel-based single crystal high temperature alloy, characterized in that: The computing device comprises: A parameter acquisition module is configured to acquire crack characteristics of a high-cycle fatigue fracture surface of a sample after an axial high-cycle fatigue test is performed on the sample, wherein the sample is a nickel-based single crystal high-temperature alloy bar of a specified size; The calculation execution module is configured to calculate the crack characteristics based on a specified composite calculation formula to obtain the composite crack shape factor Y 复合 , the composite calculation formula is: Among them, Y Ι β is the mode I crack shape factor, is the crack shape factor of mode II, is the shape factor of mode III crack; The calculation formula of the I-type crack shape factor is: AND Ι β =And Ι ×without 2 β Among them, Y I The crack front shape factor of the sample, β is the angle between the normal direction of the main slip surface of the sample and the stress application direction; The type II crack shape factor is an empirical value; The calculation formula of the mode III crack shape factor is: Wherein, ν is the material parameter Poisson's ratio of the sample.
6. An electronic device, characterized in that: The method comprises at least one processor and a memory connected to the processor, wherein: The memory is used to store computer programs or instructions; The processor is used to execute the computer program or instruction so that the electronic device implements the operation method according to any one of claims 1 to 4.
7. A storage medium, applied to an electronic device, characterized in that: The storage medium carries one or more computer programs, and the one or more computer programs can be executed by the electronic device, so that the electronic device can implement the computing method according to any one of claims 1 to 4.