Methods for producing welded steel billets and related welded steel billets

By removing the pre-coating layer from the weld edge of the pre-coated steel plate and using a specific composition of filler wire and laser welding technology, the aluminum, nickel, and chromium content of the weld joint is controlled, solving the problems of insufficient mechanical strength and brittle fracture of the weld joint, and achieving high mechanical properties and corrosion resistance of the weld joint with high aluminum content.

CN117921177BActive Publication Date: 2026-11-10ARCELORMITTAL SA
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410274670.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-24
Filing Date
2019-12-24
Publication Date
2026-11-10
Estimated Expiration
2039-12-24

AI Technical Summary

Technical Problem

In existing technologies, when welding steel plates, the aluminum-based pre-coating is diluted during the welding process, leading to the formation of intermetallic compounds in the weld joint. This affects the austenitizing temperature and hardenability, resulting in insufficient mechanical strength of the weld joint, especially with the risk of brittle fracture in cases of high aluminum content.

Method used

By partially removing the pre-coating layer at the weld edge of the pre-coated steel plate, welding is performed using filler wire with a specific composition, and the aluminum, nickel, and chromium content of the weld joint is controlled. By combining laser ablation and laser welding technologies, the quenching factor and chemical composition of the weld joint are ensured to meet specific conditions to obtain satisfactory mechanical properties.

Benefits of technology

In the case of high aluminum content, by controlling welding parameters and chemical composition, complete austenitization of the welded joint can be achieved, resulting in high mechanical strength and corrosion resistance, avoiding brittle fracture, and improving the performance of the welded joint.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117921177B_ABST
    Figure CN117921177B_ABST
Patent Text Reader

Abstract

A method for producing welded steel billets (1) includes: - providing two pre-coated plates (2), each plate comprising a steel substrate (3) having a pre-coating layer (5) on each of its two main surfaces (4), each plate (2) including a removal area (18) at a weld edge (14) on each main surface (4), wherein the pre-coating layer (5) is removed in a removal fraction in the removal area; - butt welding the plates (2) using filler wire (20) to produce an Al content including an aluminum content between 0.1 wt% and 1.2 wt%. WJ The welded joint (22). The composition of the welding wire (20) and the proportion of the added welding wire (20) make the welded joint (22) have: (a) a quenching factor FT WJ This makes FT WJ -0.96FT BM ≥0, (b) Nickel content Ni WJ ≤14-3.4xAl WJ Furthermore, the chromium content CrWJ ≤ 5-2xAl WJ , where Al WJ It is the aluminum content of the welded joint (22).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention patent application is a divisional application of the invention patent application filed on December 24, 2019, with application number 201980088342.4 and invention title "Method for producing welded steel billets and related welded steel billets". Technical Field

[0002] The present invention relates to a method for producing welded steel billets, the welded steel billets obtained therefrom, a method for producing welded, hot-pressed and cooled steel parts from the welded steel billets, and the welded, hot-pressed and cooled steel parts obtained therefrom. Background Technology

[0003] Methods for butt-welding parts made of steel plates of different compositions and / or thicknesses are known from existing technology. More specifically, the weld blank is typically heated to a temperature that allows the steel to austenitize, and then hot-formed and cooled in a hot-pressing tool. The composition of the steel can be selected to both enable the subsequent heating and forming operations and to give the welded steel parts high mechanical strength, high impact strength, and good corrosion resistance.

[0004] This type of steel part is used particularly in the automotive industry, and even more so in the manufacture of intrusion-proof parts, structural parts, or parts that contribute to the safety of motor vehicles.

[0005] To prevent corrosion, steel sheets are pre-coated with an aluminum-based pre-coating by hot-dip coating in an aluminum-containing bath. If the steel sheets are welded without any prior preparation, the aluminum-based pre-coating will be diluted by the steel substrate within the molten metal during the welding operation. Within the range of aluminum content in the pre-coating, two phenomena may occur.

[0006] If the aluminum content in the molten metal is locally high, intermetallic compounds will form in the weld joint due to dilution of a portion of the pre-coating in the molten metal and alloying that occurs during subsequent heating of the weld joint before the thermoforming step. These intermetallic compounds are the most likely sites for initial cracking.

[0007] Furthermore, aluminum tends to increase the austenitizing temperature (Ac3) of the weld joint, and this change in the austenitic domain becomes more significant when the aluminum level in the weld joint is high. In some cases, this may prevent the weld joint from achieving full austenitization, which should occur during heating before forming and is the first step required after hot pressing and cooling, hot stamping, and obtaining a martensitic structure in the weld joint.

[0008] Furthermore, aluminum also has a detrimental effect on the hardenability of welded joints because it increases the critical cooling rate necessary to obtain a martensitic or bainitic structure in the welded joint during cooling.

[0009] Therefore, during the cooling process after hot forming, martensite or bainite can no longer be obtained, and the resulting weld joint will contain ferrite. The weld joint then exhibits less hardness and mechanical strength than the two adjacent plates, thus constituting the weakest region of the part.

[0010] Publication EP2007545 describes a solution involving the removal of the surface layer of a metallic alloy at the weld edge of a pre-coated steel sheet, the weld edge being designed to be at least partially incorporated into the weld metal area. Removal can be performed by brushing or using a laser beam. The intermetallic alloy layer is retained to ensure corrosion resistance and prevent decarburization and oxidation during heat treatment prior to forming operations. In this case, the influence of aluminum is reduced by locally removing the surface layer of the coating.

[0011] However, the inventors of this patent application have observed that even after removing the surface layer of the metal alloy at the weld edge of the pre-coated steel sheet, the weld joint may still have insufficient mechanical properties. In fact, due to the protrusions from the coating to the side of the steel sheet at the weld edge caused by the removal operation and / or for thin steel sheets with a thickness of, for example, less than or equal to 1.0 mm, the aluminum concentration in the weld joint may still be too high.

[0012] EP 2 737 971, US 2016 / 0144456 and WO 2014075824 attempt to provide a method in which a pre-coated steel sheet is welded using a filler wire containing austenitic stabilizing elements such as carbon, manganese or nickel, without prior removal of the pre-coating, with the aim of achieving a fully martensitic structure in the weld joint after hot pressing and cooling, despite the presence of aluminum in the weld due to the melting of the pre-coating.

[0013] However, these methods are not entirely satisfactory because they only address one of the problems related to the presence of aluminum in the weld pool: compensation for the austenitizing temperature (Ac3) and, in some cases, the use of high-carbon filler wire can cause segregation in the weld joint. In fact, the inventors of this invention have found that the methods disclosed in the aforementioned documents do not allow for satisfactory mechanical properties in parts obtained after hot pressing and cooling, particularly for weld joints with an aluminum content greater than or equal to 0.7% by weight. Specifically, for such parts, there is a high risk of failure in the weld joint under tensile testing along the weld seam transversely.

[0014] The methods disclosed in WO 2015 / 086781 and EP 2 942 143 also address this problem and describe methods for welding pre-coated steel plates with specific filler materials using specific welding methods.

[0015] More specifically, WO 2015 / 086781 proposes the use of twin-spot laser welding, with the simultaneous supply of filler material in the form of metal powder having the following composition, by weight percentage: C: 0-0.03 wt%, Mo: 2.0-3.0 wt%, Ni: 10-14 wt%, Mn: 1.0-2.0 wt%, Cr: 16-18 wt%, and Si: 0.0-1.0 wt%, with the remainder being iron.

[0016] EP 2 942 143 proposes the use of a hybrid laser / arc welding method, which uses an arc welding torch positioned in front of a laser beam, while simultaneously supplying filler material in the form of filler wire having the following composition: C: 0-0.3 wt%, Mo: 0-0.4 wt%, Ni: 6-20 wt%, Mn: 0.5-7 wt%, Cr: 5-22 wt%, and Si: 0-1.3 wt%, Nb: 0.0-0.7 wt%, with the remainder being iron.

[0017] These methods are also unsatisfactory. In fact, the inventors of this invention have observed that using the filler wire described herein results in a high risk of part failure in the region immediately adjacent to the weld after hot pressing and cooling.

[0018] Furthermore, the use of hybrid laser-arc welding is undesirable because hybrid laser / arc welding does not allow for the same welding speed as laser welding, thus resulting in a reduction in the overall productivity of the process.

[0019] Moreover, in large-scale industrial settings, powder addition is generally more difficult to implement than filler wire.

[0020] All the methods described above for adding filler materials only specify the range of chemical composition of the filler materials. Furthermore, because welding parameters and conditions affect the filler material ratio, a single filler wire can result in very different chemical compositions in the weld joint. Therefore, simply describing the composition of the filler wire seems insufficient to address the aforementioned issues. Summary of the Invention

[0021] Therefore, the object of the present invention is to provide a method for producing welded steel billets from two such pre-coated plates, which allows for obtaining parts with satisfactory impact performance characteristics even with relatively high aluminum content in the weld joint after hot pressing and cooling.

[0022] Therefore, it is particularly desirable to avoid complete brittle fracture in welded joints.

[0023] Therefore, the present invention relates to a method for producing welded steel billets, the method comprising the following sequential steps: - Two pre-coated plates are provided, each pre-coated plate comprising a steel substrate (3) having a pre-coating layer on each of its two main surfaces, the pre-coating layer comprising: an intermetallic alloy layer comprising at least iron and aluminum, and optionally a metal alloy layer extending on top of the intermetallic alloy layer, the metal alloy layer being an aluminum layer, an aluminum alloy layer, or an aluminum-based alloy layer. Each pre-coated plate includes a removal area on its respective main surface at the weld edge intended to be at least partially incorporated into the weld joint, in which the pre-coating has been removed with a removal fraction of between 30% and 100% of the thickness of the pre-coating. - Use filler wire to butt weld pre-coated plates to create a weld joint at the junction between the pre-coated plates, the weld joint having an average aluminum content (Al) between 0.1 wt% and 1.2 wt%. WJ , in, - To select the composition and proportion of filler wire added to the weld pool in such a way that the resulting weld joint is characterized by the following: (a) Quenching factor FT of welded joint WJ , making (Guideline C1) in, -FT BM It is the hardening factor of the steel matrix that is the most difficult to harden among the two pre-coated plates, and - Determine the quenching factor FT using the following formula. WJ and FT BM FT = 128 + 1553xC + 55xMn + 267xSi + 49xNi + 5xCr - 79xAl - 2xNi² - 1532xC² - 5xMn² - 127xSi² - 40xCxNi - 4xNixMn, where Al, Cr, Ni, C, Mn, and Si are the average contents of aluminum, chromium, nickel, carbon, manganese, and silicon, expressed as weight percentages, in the region where the quenching factor is to be determined, and this region is within the range of FT. WJ In the case of welded joints, in FT BM In this case, it is the most difficult matrix to harden. (b) Average nickel content (Ni) in the welded joint WJ Satisfy the following relationship: Ni WJ ≤14-3.4xAl WJ , where Al WJ It is the average aluminum content in the welded joint (criterion C2); and (c) Average chromium content (Cr) in the welded joint WJ Satisfy the following relationship: Cr WJ ≤5-2xAl WJ, where Al WJ It is the average aluminum content in the welded joint (Criterion C3).

[0024] According to a particular implementation, the method may include one or more of the following features, which may be taken individually or in any technically permissible combination: - At least one pre-coated sheet, for example, the steel substrate of each pre-coated sheet comprises, by weight: 0.10%≤C≤0.5% 0.5%≤Mn≤4.5% 0.1%≤Si≤1% 0.01%≤Cr≤1% Ti≤0.2% Al≤0.1% S≤0.05% P≤0.1% B≤0.010% The remainder consists of iron and impurities produced during manufacturing.

[0025] - The substrate of each pre-coated plate is made of pressure-hardening steel; - The average aluminum content of the welded joint is greater than or equal to 0.15% by weight; - The average aluminum content of the welded joint is less than or equal to 0.8% by weight; - The average nickel content of the welded joints ranges from 0.1 wt% to 13.6 wt%, and more particularly from 0.2 wt% to 12.0 wt%. - The welded steel billet, after hot pressing and cooling, has a Charpy energy of greater than or equal to 25 J / cm² at 20°C, and the ultimate tensile strength of the hot-pressed and cooled welded steel billet is greater than or equal to the ultimate tensile strength of the weakest matrix in the matrix of the pre-coated plate, the weakest matrix being the matrix with the lowest product of thickness and ultimate tensile strength after hot pressing and cooling. - The filler wire has a carbon content ranging from 0.01% to 0.45% by weight; - For at least one pre-coated board, for example, for two pre-coated boards, the removal fraction is strictly less than 100% of the thickness of the pre-coating layer; - For at least one pre-coated board, the pre-coating layer includes a metal alloy layer extending on top of the intermetallic alloy layer, the metal alloy layer being an aluminum layer, an aluminum alloy layer, or an aluminum-based alloy layer, and for at least one pre-coated board, such as for two pre-coated boards, the metal alloy layer has been removed over its entire thickness, while the intermetallic alloy layer remains intact in the removal areas on each of the main surfaces of the pre-coated board. - For at least one pre-coated board provided in the providing step, and for example for two pre-coated boards, in the removal area on each main surface of the pre-coated board, the removal fraction is equal to 100%, such that the pre-coating layer has been removed over its entire thickness. - Prior to providing the step, the method also includes the step of producing two pre-coated boards from the respective initial pre-coated boards, the step comprising the following sub-step: obtaining a removal area on each main surface of the respective pre-coated board by laser ablation at the weld edge of the pre-coated board to remove the pre-coating by a removal fraction of the thickness of the pre-coating, including 30% to 100%. - The steps for producing two pre-coated boards include: - Provide two initially pre-coated plates; - Arrange the two initially pre-coated plates adjacent to each other, with a predetermined gap between them; and - The pre-coating layer on two adjacent initial pre-coated plates is removed simultaneously by laser ablation so as to simultaneously create removal areas on the adjacent surfaces of the two initial pre-coated plates. The laser beam overlaps with the two adjacent initial pre-coated plates during the removal step, and optionally, during the welding step, the two adjacent pre-coated plates thus prepared are welded using the laser beam spot that overlaps with the two adjacent pre-coated plates. The time between the end of laser ablation and the start of welding is preferably less than or equal to 10 seconds. - The method also includes: preparing the welding edge of at least one pre-coated board using at least one of the following processing steps prior to butt welding: brushing, machining, chamfering and / or beveling; - The welding process is performed using a laser beam; - The two pre-coated plates have the same thickness; - The two pre-coated plates have different thicknesses; - For at least one pre-coated sheet, for example, for two pre-coated sheets, the steel base comprises, by weight: 0.15%≤C≤0.25% 0.8%≤Mn≤1.8% 0.1%≤Si≤0.35% 0.01%≤Cr≤0.5% Ti≤0.1% Al≤0.1% S≤0.05% P≤0.1% B≤0.005% The remainder consists of iron and impurities produced during manufacturing.

[0026] - For a pre-coated sheet, the steel matrix comprises, by weight: 0.040%≤C≤0.100% 0.80%≤Mn≤2.00% Si≤0.30% S≤0.005% P≤0.030% 0.010%≤Al≤0.070% 0.015%≤Nb≤0.100% Ti≤0.080% N≤0.009% Cu≤0.100% Ni≤0.100% Cr≤0.100% Mo≤0.100% Ca≤0.006%, The remainder consists of iron and impurities produced during manufacturing.

[0027] - For a pre-coated sheet, the steel matrix comprises, by weight: 0.24%≤C≤0.38% 0.40%≤Mn≤3% 0.10%≤Si≤0.70% 0.015%≤AI≤0.070% 0%≤Cr≤2% 0.25%≤Ni≤2% 0.015%≤Ti≤0.10% 0%≤Nb≤0.060% 0.0005%≤B≤0.0040% 0.003%≤N≤0.010% 0.0001%≤S≤0.005% 0.0001%≤P≤0.025% The titanium and nitrogen contents satisfy the following relationship: Ti / N > 3.42 Furthermore, the carbon, manganese, chromium, and silicon contents satisfy the following relationship: , Steel may optionally include one or more of the following elements: 0.05%≤Mo≤0.65% 0.001%≤W≤0.30% 0.0005%≤Ca≤0.005% The remainder consists of iron and impurities that are unavoidable during manufacturing.

[0028] Welding is performed using shielding gases, particularly helium and / or argon.

[0029] The present invention also relates to a method for producing welded, hot-pressed, and cooled steel parts, the method comprising the following sequential steps: - Perform the method described above in order to obtain the welded steel billet; - Heating and welding the steel billet to obtain a fully austenitic structure in the matrix of the pre-coated plate; - Hot pressing of welded steel billets in a pressing tool to obtain steel parts; and - Cool the steel parts in the pressing tool.

[0030] According to a specific embodiment of the method for producing welded, hot-pressed and cooled steel parts, during the cooling step, the cooling rate is greater than or equal to the cooling rate of the most hardenable bainite or martensite in the matrix of the pre-coated plate.

[0031] The present invention also relates to a welded steel billet comprising two pre-coated plates, each pre-coated plate comprising a steel substrate having a pre-coating layer on each of its main surfaces, the pre-coating layer comprising: an intermetallic alloy layer comprising at least iron and aluminum, and optionally a metal alloy layer extending on top of the intermetallic alloy layer, the metal alloy layer being an aluminum layer, an aluminum alloy layer, or an aluminum-based alloy layer. The pre-coated plates are joined by welded joints having an average aluminum content between 0.1% and 1.2% by weight, and the welded joints are also characterized by the following: (a) Quenching factor FT of welded joint WJ , making (Criterion C1), where, -FT BM It is the quenching factor of the steel matrix that is the most difficult to harden among the two pre-coated plates, and - Determine the quenching factor FT using the following formula. WJ and FT BM FT = 128 + 1553xC + 55xMn + 267xSi + 49xNi + 5xCr - 79xAl - 2xNi² - 1532xC² - 5xMn² - 127xSi² - 40xCxNi - 4xNixMn, where Al, Cr, Ni, C, Mn, and Si are the average contents of aluminum, chromium, nickel, carbon, manganese, and silicon, expressed as weight percentages, in the region where the quenching factor is to be determined, and this region is within the range of FT. WJ In the case of welded joints, in FT BM In this case, it is the most difficult matrix to harden, and (b) Average nickel content (Ni) in the welded joint WJ Satisfy the following relationship: NiWJ ≤14-3.4xAl WJ , where Al WJ It is the average aluminum content in the welded joint (criterion C2); and (c) Average chromium content (Cr) in the welded joint WJ Satisfy the following relationship: Cr WJ ≤5-2xAl WJ , where Al WJ It is the average aluminum content in the welded joint (criterion C3), and Each pre-coated board includes an intermediate region adjacent to the weld joint on its respective main surface, in which the pre-coating layer has been removed with a removal fraction between 30% and 100% of the pre-coating layer thickness.

[0032] According to a specific embodiment of the welded steel billet, the welded steel billet includes one or more of the following features, which may be taken individually or in any technically permissible combination: - The steel substrate of at least one pre-coated plate, such as two pre-coated plates, comprises by weight: 0.10%≤C≤0.5% 0.5%≤Mn≤4.5% 0.1%≤Si≤1% 0.01%≤Cr≤1% Ti≤0.2% Al≤0.1% S≤0.05% P≤0.1% B≤0.010% The remainder consists of iron and impurities produced during manufacturing. - The substrate of each pre-coated plate is made of pressure-hardening steel; - For each pre-coated board, the width of the central region includes a range of 5 μm to 2000 μm from the edge of the weld joint; - For at least one pre-coated board, for example, for two pre-coated boards, the removal fraction is equal to 100% of the thickness of the pre-coating layer; - For at least one pre-coated board, for example, for two pre-coated boards, the removal fraction is strictly less than 100% of the thickness of the pre-coating layer; - For at least one pre-coated board, such as for two pre-coated boards, the pre-coating layer includes a metal alloy layer extending over an intermetallic alloy layer, the metal alloy layer being an aluminum layer, an aluminum alloy layer, or an aluminum-based alloy layer, and wherein, for at least one pre-coated board, such as for two pre-coated boards, the metal alloy layer has been removed over its entire thickness, while the intermetallic alloy layer remains intact in the removal areas on the respective main surfaces of the pre-coated board. - The nickel content of the welded joints includes between 0.1 wt% and 13.6 wt%, more particularly between 0.2 wt% and 12.0 wt%; - The welded steel billet, after hot pressing and cooling, has a Charpy energy greater than or equal to 25 J / cm² at 20°C, and the ultimate tensile strength of the hot-pressed and cooled welded steel billet is greater than or equal to the ultimate tensile strength of the weakest matrix in the matrix of the pre-coated plate, the weakest matrix being the matrix with the lowest product of thickness and ultimate tensile strength after hot pressing and cooling. The welded joint ensures that, after hot pressing and cooling, the maximum hardness change ΔHV (WJ) across the welded joint is less than or equal to the average hardness HV of the welded joint. mean 20% of (WJ); - Each intermediate region includes curing stripes, and the curing stripes on the adjacent main surfaces of the two pre-coated plates are symmetrical with respect to the vertical intermediate plane between the two pre-coated plates. - Each intermediate region includes an inner edge located at the weld joint and an outer edge away from the weld joint, wherein the distance between the outer edges of adjacent intermediate regions of two pre-coated plates is constant along the longitudinal direction of the weld joint; - For at least one pre-coated sheet, for example, for two pre-coated sheets, the steel base comprises, by weight: 0.15%≤C≤0.25% 0.8%≤Mn≤1.8% 0.1%≤Si≤0.35% 0.01%≤Cr≤0.5% Ti≤0.1% Al≤0.1% S≤0.05% P≤0.1% B≤0.005% The remainder consists of iron and impurities produced during manufacturing; - For a pre-coated sheet, the steel matrix comprises, by weight: 0.040%≤C≤0.100% 0.80%≤Mn≤2.00% Si≤0.30% S≤0.005% P≤0.030% 0.010%≤Al≤0.070% 0.015%≤Nb≤0.100% Ti≤0.080% N≤0.009% Cu≤0.100% Ni≤0.100% Cr≤0.100% Mo≤0.100% Ca≤0.006%, The remainder consists of iron and impurities produced during manufacturing; - For a pre-coated sheet, the steel matrix comprises, by weight: 0.24%≤C≤0.38% 0.40%≤Mn≤3% 0.10%≤Si≤0.70% 0.015%≤AI≤0.070% 0%≤Cr≤2% 0.25%≤Ni≤2% 0.015%≤Ti≤0.10% 0%≤Nb≤0.060% 0.0005%≤B≤0.0040% 0.003%≤N≤0.010% 0.0001%≤S≤0.005% 0.0001%≤P≤0.025% The titanium and nitrogen contents satisfy the following relationship: Ti / N > 3.42 Furthermore, the carbon, manganese, chromium, and silicon contents satisfy the following relationship: , Steel may optionally include one or more of the following elements: 0.05%≤Mo≤0.65% 0.001%≤W≤0.30% 0.0005%≤Ca≤0.005% The remainder consists of iron and impurities that are unavoidable during manufacturing.

[0033] The present invention also relates to a welded, hot-pressed, and cooled steel part comprising a first coated steel part portion and a second coated steel part portion, each coated steel part portion comprising a steel substrate having a coating comprising at least iron and aluminum on at least one of its main surfaces. The first and second coated steel parts are joined by a weld joint having an average aluminum content between 0.1% and 1.2% by weight, and the weld joint is also characterized by the following: (a) Quenching factor FT of welded joint WJ , making (Criterion C1), where, -FT BM It is the quenching factor of the steel matrix that is the most difficult to harden among the two pre-coated plates, and - Determine the quenching factor FT using the following formula. WJ and FT BM FT = 128 + 1553xC + 55xMn + 267xSi + 49xNi + 5xCr - 79xAl - 2xNi² - 1532xC² - 5xMn² - 127xSi² - 40xCxNi - 4xNixMn, where Al, Cr, Ni, C, Mn, and Si are the average contents of aluminum, chromium, nickel, carbon, manganese, and silicon, expressed as weight percentages, in the region where the quenching factor is to be determined, and this region is within the range of FT. WJ In the case of welded joints, in FT BM In this case, it is the most difficult matrix to harden. (b) Average nickel content (Ni) in the welded joint WJ The following relationship must be satisfied: Ni ≤ 14 - 3.4xAl WJ , where Al WJ It is the average aluminum content in the welded joint (criterion C2); and (c) Average chromium content (Cr) in the welded joint WJ The following relationship must be satisfied: Cr ≤ 5-2xAl WJ , where Al WJ It is the average aluminum content in the welded joint (criterion C3), and Each coated steel part includes an intermediate region adjacent to the weld joint on its respective main surface, in which the coating thickness is strictly smaller than that of the adjacent regions of the coated steel part, which are located further away from the weld joint than the intermediate region, or in which the coating is absent.

[0034] According to a specific embodiment of a welded, hot-pressed, and cooled steel part, the welded, hot-pressed, and cooled steel part may include one or more of the following features, which may be taken individually or in any possible combination: At least one of the first and second steel part portions, for example, the steel of the base material of the first and second steel part portions comprises, by weight: 0.10%≤C≤0.5% 0.5%≤Mn≤4.5% 0.1%≤Si≤1% 0.01%≤Cr≤1% Ti≤0.2% Al≤0.1% S≤0.05% P≤0.1% B≤0.010% The remainder consists of iron and impurities produced during manufacturing. - The base of each of the first and second steel parts is made of pressure-hardening steel; - Each intermediate region includes curing stripes, and the curing stripes on the adjacent master surfaces of the two coated steel parts are symmetrical with respect to the vertical intermediate plane between the two coated steel parts. -Each intermediate region includes an inner edge located at the weld joint and an outer edge away from the weld joint, and wherein the distance between the outer edges of adjacent intermediate regions of two coated steel part portions is constant along the longitudinal direction of the weld joint; - Average hardness HV in welded joints mean (WJ) less than or equal to 700 HV; - The average nickel content in the welded joints ranges from 0.1 wt% to 13.6 wt%, and more particularly from 0.2 wt% to 12.0 wt%. - The Charpy energy of the welded joint at 20°C is greater than or equal to 25 J / cm², and the ultimate tensile strength of the welded, hot-pressed and cooled steel part is greater than or equal to the ultimate tensile strength of the weakest matrix in the matrix of the coated steel part, the weakest matrix being the matrix with the lowest product of thickness and ultimate tensile strength. The maximum hardness variation ΔHV (WJ) across the weld joint is less than or equal to the average hardness HV of the weld joint. mean 20% of (WJ); At least one of the first and second coated steel part portions, for example, the steel of the base material of the first and second coated steel part portions comprises, by weight: 0.15%≤C≤0.25% 0.8%≤Mn≤1.8% 0.1%≤Si≤0.35% 0.01%≤Cr≤0.5% Ti≤0.1% Al≤0.1% S≤0.05% P≤0.1% B≤0.005% The remainder consists of iron and impurities produced during manufacturing; The steel substrate of one of the first and second coated steel part portions comprises, by weight: 0.040%≤C≤0.100% 0.80%≤Mn≤2.00% Si≤0.30% S≤0.005% P≤0.030% 0.010%≤Al≤0.070% 0.015%≤Nb≤0.100% Ti≤0.080% N≤0.009% Cu≤0.100% Ni≤0.100% Cr≤0.100% Mo≤0.100% Ca≤0.006%, The remainder consists of iron and impurities produced during manufacturing; The steel substrate of one of the first and second coated steel part portions comprises, by weight: 0.24%≤C≤0.38% 0.40%≤Mn≤3% 0.10%≤Si≤0.70% 0.015%≤AI≤0.070% 0%≤Cr≤2% 0.25%≤Ni≤2% 0.015%≤Ti≤0.10% 0%≤Nb≤0.060% 0.0005%≤B≤0.0040% 0.003%≤N≤0.010% 0.0001%≤S≤0.005% 0.0001%≤P≤0.025% The titanium and nitrogen contents satisfy the following relationship: Ti / N > 3.42 Furthermore, the carbon, manganese, chromium, and silicon contents satisfy the following relationship: , Steel may optionally include one or more of the following elements: 0.05%≤Mo≤0.65% 0.001%≤W≤0.30% 0.0005%≤Ca≤0.005% The remainder consists of iron and impurities that are unavoidable during manufacturing.

[0035] The present invention also relates to the use of the welded, hot-pressed and cooled steel parts as described above for the production of anti-intrusion parts or energy-absorbing parts for motor vehicles. Attached Figure Description

[0036] The invention will be better understood upon reading the following specification, which is given by way of example only and with reference to the accompanying drawings, in which: Figure 1 It is a perspective view of a pre-coated board, which includes a removal area in the pre-coating layer at the periphery of the board; Figure 2 It is a 3D view of the initial pre-coated plate; Figure 3 This is a schematic cross-sectional view showing the start of the welding step according to the method of the present invention; Figure 4 This is a schematic cross-sectional view showing the end of the welding step according to the method of the present invention; and Figure 5 This is a schematic cross-sectional view of the welded steel billet according to the present invention. Detailed Implementation

[0037] Throughout the patent application, the content of elements is expressed as a weight percentage (wt%).

[0038] The present invention relates to a method for producing welded steel billets 1.

[0039] The method includes a first step of providing two pre-coated plates 2.

[0040] like Figure 1 As shown, each pre-coated plate 2 includes two main surfaces 4 and at least one side surface 13 extending from one main surface to the other between the two main surfaces 4. Figure 1 In the example shown, the pre-coated plate 2 includes four sides. For example, one of the sides forms an angle between 60° and 90° with the main surface.

[0041] Each pre-coated plate 2 includes a metal substrate having a pre-coated layer 5 on its respective main surface. The pre-coated layer 5 is overlapped on and in contact with the metal substrate.

[0042] The metal matrix is ​​more specifically a steel matrix 3.

[0043] More specifically, the base steel is steel with a ferrite-pearlite microstructure.

[0044] Preferably, the matrix is ​​made of steel intended for heat treatment, more particularly of pressure-hardenable steel, and for example of manganese-boron steel, such as 22MnB5 type steel.

[0045] According to one embodiment, the steel of the base material comprises, and in particular, the following components by weight: 0.10%≤C≤0.5% 0.5%≤Mn≤3% 0.1%≤Si≤1% 0.01%≤Cr≤1% Ti≤0.2% Al≤0.1% S≤0.05% P≤0.1% B≤0.010% The remainder consists of iron and impurities produced during manufacturing.

[0046] More specifically, the steel base comprises, and is specifically composed of, the following components by weight: 0.15%≤C≤0.25% 0.8%≤Mn≤1.8% 0.1%≤Si≤0.35% 0.01%≤Cr≤0.5% Ti≤0.1% Al≤0.1% S≤0.05% P≤0.1% B≤0.005% The remainder consists of iron and impurities produced during manufacturing.

[0047] According to the alternative embodiment, the steel of the base material comprises, and specifically consists of, the following components by weight: 0.040%≤C≤0.100% 0.80%≤Mn≤2.00% Si≤0.30% S≤0.005% P≤0.030% 0.010%≤Al≤0.070% 0.015%≤Nb≤0.100% Ti≤0.080% N≤0.009% Cu≤0.100% Ni≤0.100% Cr≤0.100% Mo≤0.100% Ca≤0.006% The remainder consists of iron and impurities produced during manufacturing.

[0048] According to the alternative embodiment, the steel of the base material comprises, and specifically consists of, the following components by weight: 0.24%≤C≤0.38% 0.40%≤Mn≤3% 0.10%≤Si≤0.70% 0.015%≤Al≤0.070% 0%≤Cr≤2% 0.25%≤Ni≤2% 0.015%≤Ti≤0.10% 0%≤Nb≤0.060% 0.0005%≤B≤0.0040% 0.003%≤N≤0.010% 0.0001%≤S≤0.005% 0.0001%≤P≤0.025% The titanium and nitrogen contents satisfy the following relationship: Ti / N > 3.42 Furthermore, the carbon, manganese, chromium, and silicon contents satisfy the following relationship: , Steel may optionally include one or more of the following elements: 0.05%≤Mo≤0.65% 0.001%≤W≤0.30% 0.0005%≤Ca≤0.005% The remainder consists of iron and impurities that are unavoidable during manufacturing.

[0049] According to one example, the substrates of the two pre-coated plates 2 have the same composition.

[0050] According to another example, the substrates of the two pre-coated plates 2 have different compositions. In particular, the two substrates have different compositions, each composition being selected from the four compositions described above. For example, the steel of the substrate of one pre-coated plate 2 has the first composition described above, while the steel of the substrate of the other pre-coated plate 2 has a composition selected from the second, third, or fourth composition described above.

[0051] Depending on the desired thickness of the matrix, the matrix can be obtained by hot rolling and / or cold rolling followed by annealing, or by any other suitable method.

[0052] The substrate advantageously has a thickness between 0.8 mm and 5 mm, more particularly between 1.0 mm and 3.0 mm. The two pre-coated plates 2 may have the same thickness or different thicknesses.

[0053] The pre-coating 5 is obtained by hot-dip coating (i.e., by immersing the substrate in a molten metal bath).

[0054] The pre-coating 5 includes at least an intermetallic alloy layer 9 in contact with the substrate. The intermetallic alloy layer 9 includes at least iron and aluminum. The intermetallic alloy layer 9 is formed specifically through a reaction between the substrate and the molten metal in the molten pool. More specifically, the intermetallic alloy layer 9 includes Fe. x-Al y Type of intermetallic compound, more particularly Fe2Al5.

[0055] exist Figure 1 In the example shown, the pre-coating 5 also includes a metal alloy layer 11 extending on top of the intermetallic alloy layer 9. The metal alloy layer 11 has a composition similar to that of the molten metal in the bath. The metal alloy layer is formed from the molten metal carried away by the plate as it travels through the molten metal bath during hot-dip coating. The metal alloy layer 11 is an aluminum layer, or an aluminum alloy layer, or an aluminum-based alloy layer.

[0056] In this context, aluminum alloys refer to alloys that contain more than 50% by weight of aluminum. Aluminum-based alloys are alloys in which aluminum is the main element by weight.

[0057] For example, the metal alloy layer 11 is an aluminum alloy layer that also includes silicon. More specifically, the metal alloy layer 11 comprises, by weight: 8%≤Si≤11% 2%≤Fe≤4% The remainder consists of aluminum and possible impurities.

[0058] The metal alloy layer 11 has a thickness, for example, between 19 μm and 33 μm or between 10 μm and 20 μm.

[0059] The pre-coating 5 includes a metal alloy layer 11. Figure 1 In the example shown, the thickness of the intermetallic alloy layer 9 is typically on the order of a few micrometers. In particular, its average thickness typically ranges from 2 micrometers to 8 micrometers.

[0060] Patent EP 2 007 545 discloses a specific structure of a pre-coating layer 5, including an intermetallic alloy layer 9 and a metal alloy layer 11, obtained by hot-dip coating.

[0061] According to another embodiment, the pre-coating 5 comprises only the intermetallic alloy layer 9 as described above. In this case, the thickness of the intermetallic alloy layer 9 is, for example, between 10 μm and 40 μm. This pre-coating 5, consisting of the intermetallic alloy layer 9, can be obtained, for example, by pre-alloying the pre-coating 5 comprising the intermetallic alloy layer 9 and the metal alloy layer 11 as described above. This pre-alloying process is performed at a selected temperature and holding time to alloy the pre-coating 5 with the substrate over at least a portion of its thickness. More specifically, the pre-alloying process may include the following steps: heating the plate to a pre-alloying temperature between 700°C and 900°C, and holding the pre-alloyed plate at this temperature for a time between 2 minutes and 200 hours. In this case, the intermetallic alloy layer 9 may be composed of different intermetallic sublayers, such as Fe2Al5, FeAl3, FeAl, and Fe6Al.12 Si5 and FeAl3 sublayers.

[0062] Advantageously, such as Figure 1 For example, the substrate has a pre-coating 5 as described above on its two main surfaces.

[0063] In addition, such as Figure 1 As shown, for each pre-coated board 2, the pre-coating layer 5 is removed on each main surface of the pre-coated board 2 at the weld edge 14 of the pre-coated board 2 to create a removal area 18 at the weld edge 14. More specifically, the pre-coating layer 5 is removed with a removal fraction F of the thickness of the pre-coating layer 5, which is between 30% and 100% (including the boundary).

[0064] The weld edge 14 includes a peripheral portion of the pre-coated plate 2, which is intended to be at least partially incorporated into the weld joint 22 during butt welding. More specifically, the weld edge 14 includes a side of the pre-coated plate 2 and a portion of the pre-coated plate 2 extending from that side and including a portion of the pre-coated coating 5 and a portion of the substrate.

[0065] The removal fraction F of the pre-coating 5 at the weld edge 14 is preferably performed using a laser beam (i.e., by laser ablation).

[0066] The removal area 18 can extend from the side of the plate 2 and includes a width between 0.5 mm and 3 mm.

[0067] Advantageously, the removal fraction F is strictly less than 100%, which means that only a portion of the pre-coating 5 is removed in the removal area 18, while a portion of it is retained.

[0068] For example, in Figure 1 In the illustrated embodiment, in removal region 18, the metal alloy layer 11 is removed, while the intermetallic alloy layer 9 is retained for at least a portion of its thickness. In this case, the remaining intermetallic alloy layer 9 protects the area of ​​the weld billet 1 adjacent to the weld joint 22 from oxidation and decarburization during subsequent hot pressing steps and from corrosion during its service life.

[0069] According to the implementation, during the removal step, the intermetallic alloy layer 9 retains its integrity or is retained at a fraction of strictly less than 100% of its initial thickness, for example, at only 60%, 80%, or 90% of its initial thickness.

[0070] According to an alternative embodiment (not shown), during the removal step, the pre-coating 5 is removed over its entire thickness in the removal region 18. In this embodiment, the removal fraction corresponds to 100% of the thickness of the pre-coating 5. In this embodiment, the pre-coating 5 is not present in the removal region 18.

[0071] More specifically, the method includes, before providing the steps, components such as... Figure 2 The corresponding initial pre-coated plate 2' shown is produced as follows: Figure 1 The steps for the two pre-coated plates 2 shown.

[0072] The initially pre-coated plate 2' has approximately the same geometry and composition as the pre-coated plate 2, the only difference being the absence of the removal region 18. In other words, the pre-coating layer 5 of the initially pre-coated plate 2' remains intact on both main surfaces of the initially pre-coated plate 2'. It completely covers both main surfaces of the initially pre-coated plate 2'.

[0073] This step includes a sub-step of obtaining a removal area 18 on each main surface of each pre-coated plate 2 by removing the pre-coating 5 at the weld edge 14 on the removal fraction F using laser ablation.

[0074] Optionally, the method further includes the step of preparing the welding edge 14 of at least one pre-coated plate 2 (e.g., two pre-coated plates 2).

[0075] The preparation of the weld edge 14 may include at least one of the following processing steps: - Brush and clean the welding edges 14; - Machining of the welded edge 14; - Chamfer the weld edge 14; and / or - Beveled weld edge 14.

[0076] The brushing step allows for at least partial removal of the pre-coating 5 on the weld edge 14, and more particularly on the sides, which is produced by mechanical cutting operations and / or removal of the pre-coating 5 at the weld edge 14.

[0077] Chamfering or beveling the weld edge 14 allows for an increase in the amount of filler material added without resulting in excessive thickness at the weld joint 22.

[0078] If the shape of the weld edge 14 prior to machining is not straight enough for laser welding, the weld edge 14 is machined.

[0079] The method also includes the step of using filler wire 20 to weld the pre-coated plate 2 after optionally preparing the weld edge 14 in order to obtain the weld billet 1.

[0080] Figure 3 and Figure 4 The two stages of the welding process for producing the welded steel billet 1 are illustrated.

[0081] exist Figure 3 and Figure 4 In the example shown, the two pre-coated plates 2 are as follows: Figure 1 The pre-coated board shown includes a removal area 18 at the corresponding weld edge 14, wherein the metal alloy layer 11 has been removed over its entire thickness, while the intermetallic alloy layer 9 remains intact.

[0082] The welding operation results in the formation of a molten metal area at the joint between the two plates 2, which subsequently solidifies, forming a welded joint 22.

[0083] The welding process, particularly the laser welding process, involves guiding a laser beam 24 toward the joint between the two plates 2. This laser beam 24 is configured to melt the filler wire 20 at its impact point 26.

[0084] Laser welding steps can be performed using, for example, a CO2 laser or a solid-state laser.

[0085] The laser source is preferably a high-power laser source. For example, the laser source can be selected from a CO2 laser with a wavelength of approximately 10 micrometers, a solid-state laser source with a wavelength of approximately 1 micrometer, or a semiconductor laser source, such as a diode laser with a wavelength approximately between 0.8 and 1 micrometer.

[0086] The power of the laser source is selected based on the thickness of plate 2. Specifically, the power is selected to allow for the fusion of the filler wire 20 and the weld edge 14 of plate 2, as well as sufficient mixing within the weld joint 22. For CO2 lasers, the laser power is, for example, between 3 kW and 12 kW. For solid-state lasers or semiconductor lasers, the laser power is, for example, between 2 kW and 8 kW.

[0087] For both types of laser sources, the diameter of the laser beam 24 at its impact point 26 on the plate 2 can be approximately 600 μm.

[0088] During the welding process, welding is performed, for example, under a protective atmosphere. This protective atmosphere specifically prevents oxidation and decarburization of the area where welding is performed, the formation of boron nitride in the weld joint 22, and cold cracking that may occur due to hydrogen absorption.

[0089] The protective atmosphere is, for example, an inert gas or a mixture of inert gases. The inert gas can be helium or argon or a mixture of these gases.

[0090] During this welding step, the distance between the facing sides of the two plates is, for example, less than or equal to 0.3 mm, and more specifically less than or equal to 0.1 mm. Providing such a gap between the facing sides of the two plates facilitates the deposition of filler metal during the welding operation and prevents excessive thickness at the weld joint 22. In the case of a chamfer or beveling edge being formed at the weld edge 14 of plate 2 during the preparation step, the deposition of filler metal and the prevention of excessive thickness are also improved.

[0091] Specifically, the average aluminum content Al in welded joint 22 WJ Included in the range of 0.1% to 1.2% by weight. More specifically, the average aluminum content Al in welded joint 22 WJ Greater than or equal to 0.15% by weight. Average aluminum content (Al) in welded joint 22. WJ For example, less than or equal to 0.8% of the weight.

[0092] The average aluminum content Al WJ The aluminum is produced by a portion of the pre-coating 5 that may remain in the removal area 18 after the removal of fraction F, and by trace amounts of aluminum present on the side at the weld edge 14, which is produced by the removal operation and / or cutting operation. In the weld joint 22, it is mixed with the steel of the base material and the steel of the filler wire 20.

[0093] During the welding step, the proportion of filler wire 20 added to the weld pool includes, for example, between 10% and 50%, and more specifically between 10% and 40%.

[0094] According to the invention, the composition and proportion of the filler wire 20 added to the weld pool are selected such that the resulting weld joint 22 is characterized by the following: (a) Quenching factor FT of welded joint 22 WJ , making (Guideline C1) in, -FT BM It is the hardening factor of the steel matrix 3 in the two pre-coated plates 2 that is the most difficult to harden, and - Determine the quenching factor FT using the following formula. WJ and FT BM :FT=128+1553xC+55xMn+267xSi+49xNi+5xCr-79xAl-2xNi²-1532xC² -5xMn²-127xSi²-40xCxNi-4xNixMn, where Al, Cr, Ni, C, Mn, and Si are the average contents (in weight percentage) of aluminum, chromium, nickel, carbon, manganese, and silicon in the region where the quenching factor is to be determined, and this region is in the FT... WJ In the case of welded joint 22, in FT BM In this case, it is the most difficult matrix to harden. (b) Average nickel content (Ni) of welded joint 22 WJ Satisfy the following relationship: Ni WJ ≤14-3.4xAl WJ , where Al WJIt is the average aluminum content of the welded joint (criterion C2); and (c) Average chromium content (Cr) of welded joint 22 WJ Satisfy the following relationship: Cr WJ ≤5-2xAl WJ , where Al WJ It is the average aluminum content of welded joint 22 (standard C3).

[0095] The substrate that is the most difficult to harden in the pre-coated board 2 is the substrate with the lowest carbon content.

[0096] In fact, the inventors of this invention discovered in a surprising way that, when the above criteria C1, C2, and C3 are cumulatively satisfied, the parts obtained from this welded steel billet 1 after heat treatment including an austenitizing step (hot pressing and cooling in a pressing tool) exhibit a temperature of greater than or equal to 25 J / cm² in the welded joint 22 at 20°C. 2 The Charpy energy, and exhibits an ultimate tensile strength greater than or equal to the ultimate tensile strength of the weakest matrix in the pre-coated plate 2 matrix.

[0097] The weakest matrix is ​​the one with the lowest product of thickness and ultimate tensile strength after hot pressing and cooling.

[0098] Specifically, greater than or equal to 25 J / cm 2 The Charpy energy of welded joint 22 at 20°C allows for the avoidance of complete brittle fracture in the welded joint.

[0099] Therefore, when the above criteria C1, C2 and C3 are cumulatively met, even if the weld joint 22 includes a relatively high aluminum content, the presence of the weld joint 22 will not reduce the properties of the welded steel parts obtained from the weld blank by hot pressing and cooling compared to the properties of the weakest matrix in the matrix of the pre-coated plate 2 after hot pressing and cooling.

[0100] Therefore, by means of the method according to the invention, parts with satisfactory impact performance can still be obtained despite the possible presence of a relatively high aluminum content in the weld joint 22.

[0101] Preferably, the composition and proportion of the filler wire 20 added to the weld pool are further selected such that the average nickel content (Ni) of the weld joint 22 is such that... WJ Included in the range of 0.1 wt% to 13.7 wt%, and more particularly in the range of 0.2 wt% to 12.0 wt%.

[0102] For example, the composition and proportion of the filler wire 20 added to the weld pool are further selected such that the average chromium content Cr of the weld joint 22 is [missing information]. WJGreater than or equal to 0.05% by weight. This chromium content in the weld joint is advantageous because it improves the corrosion resistance and hardenability of the weld joint 22.

[0103] Preferably, the composition of the welded joint 22 is such that it has a predominantly martensitic microstructure after hot pressing and cooling. "Predominantly" means that it comprises at least 95% martensite, and more particularly 100% martensite.

[0104] The filler wire 20 specifically has a carbon content ranging from 0.01% to 0.45% by weight. According to an example, the carbon content of the filler wire 20 is greater than or equal to the carbon content of the most difficult-to-harden matrix in the substrates of the two pre-coated plates 2.

[0105] In fact, the inventors of this invention discovered in a surprising way that, in order to reduce the risk of carbon segregation and thus hardness peaks in the weld joint 22 after hot pressing and cooling in a pressing tool, especially in the presence of a large amount of aluminum in the weld joint 22, the carbon content in the filler wire should be between 0.01% by weight and 0.45% by weight. Therefore, using such filler wire 20 reduces the risk of brittleness in the weld joint 22 and helps prevent failure in the weld joint 22 of parts obtained after hot pressing and cooling in a pressing tool under tension perpendicular to the weld joint 22.

[0106] In particular, the inventors of this invention have observed that the carbon content in the filler wire should be between 0.01% by weight and 0.45% by weight in order to obtain a weld joint 22 in which the maximum hardness variation ΔHV (WJ) across the weld joint 22 is less than or equal to the average hardness HV of the weld joint 22. mean 20% of (WJ), in other words, Wherein, ΔHV(WJ) is the difference between the maximum and minimum hardness measured in welded joint 22, and HV mean (WJ) is the average hardness measured in welded joint 22.

[0107] Preferably, the manganese content of the filler wire 20 is strictly less than the manganese content of the substrate of the pre-coated plate 2.

[0108] For example, filler wire 20 has the following composition by weight: 0.01% ≤ C ≤ 0.45%, for example, 0.02% ≤ C ≤ 0.45%. 0.001%≤Mn≤0.45%, for example 0.05%≤Mn≤0.45%, and more specifically 0.05%≤Mn≤0.20%. 0.001%≤Si≤1% 0.02%≤Ni≤56%, for example, 0.2%≤Ni≤10.0% 0.001%≤Cr≤30% 0.001%≤Mo≤5% 0.001%≤Al≤0.30% 0.001%≤Cu≤1.80% 0.001%≤Nb≤1.50% 0.001%≤Ti≤0.30% 0.001%≤N≤10% 0.001%≤V≤0.1% 0.001%≤Co≤0.20% The remainder consists of iron and unavoidable impurities.

[0109] In the above exemplary filler wire composition, the content of Mn, Si, Cr, Mo, Al, Cu, Nb, Ti, N, V ​​and Co equal to about 0.001% corresponds to trace amounts of these elements at the impurity level produced by the melting and refining of the raw materials, or is produced by the measuring device with very low accuracy for the content. This may result in elements that are not present in the steel being analyzed at all being measured as present in very low amounts, or elements that are present in very low amounts being measured as not present in the steel.

[0110] For example, the filler wire 20 is composed of the elements described above.

[0111] The filler wire 20 is, for example, a solid wire or a flux-cored wire.

[0112] The present invention also relates to a weldable steel billet 1 that can be obtained using the above method.

[0113] Figure 5 An example of such a welded steel billet is shown in the figure.

[0114] The welded steel billet 1 includes two pre-coated plates 2, each pre-coated plate 2 including a steel substrate 3 having a pre-coating layer 5 on each of its main surfaces. The pre-coating layer 5 includes an intermetallic alloy layer 9 comprising at least iron and aluminum, and optionally a metal alloy layer 11 extending on top of the intermetallic alloy layer 9. The metal alloy layer 11 is an aluminum layer, an aluminum alloy layer, or an aluminum-based alloy layer. The pre-coated plates 2 are joined by a welded joint 22.

[0115] The welded steel billet 1 includes an intermediate region 28 on each side of the welded joint 22, in which the pre-coating 5 has been removed at the removal fraction F as defined above.

[0116] In addition, such as Figure 5As can be seen, each intermediate region 28 includes an inner edge 30 located at the weld joint 22 and an outer edge 32 located away from the weld joint 22.

[0117] The width W of each intermediate region 28, measured from the edge of the welded joint 22, i.e. the distance between the inner edge 30 and the outer edge 32, is between 5 μm and 2000 μm, and more particularly between 5 μm and 1500 μm.

[0118] Preferably, in the intermediate region 28, the pre-coating 5 has been removed with a removal fraction F strictly less than 100%. In particular, the metal alloy layer 11 has been removed, but the intermetallic alloy layer 9 remains intact.

[0119] According to the alternative scheme, in the intermediate region 28, the pre-coating 5 has been removed at a removal fraction F equal to 100% (i.e., over its entire thickness).

[0120] Therefore, in the intermediate region 28, the thickness of the pre-coated layer 5 is strictly less than, or even non-existent in, the region of the pre-coated plate 2 further away from the weld joint 22.

[0121] The intermediate region 28 is generated by the removal region 18 on the corresponding pre-coated plate 2.

[0122] The pre-coated plate 2 and the welded joint 22 have the features disclosed above regarding the method for producing welded steel billets 1.

[0123] Therefore, welded joint 22 complies with the above-mentioned criteria C1, C2 and C3.

[0124] In addition, the average aluminum content Al of welded joint 22 WJ Included in the range of 0.1 wt% to 1.2 wt%. More specifically, the average aluminum content Al of welded joint 22 is... WJ Greater than or equal to 0.15% by weight. Average aluminum content (Al) of welded joint 22. WJ For example, less than or equal to 0.8% of the weight.

[0125] For example, after hot pressing and cooling in a pressing tool, the welded joint 22 has a Charpy energy greater than or equal to 25 J / cm² at 20°C. 2 .

[0126] Furthermore, after hot pressing and cooling, the ultimate tensile strength of the hot-pressed and cooled welded steel billet is greater than or equal to the ultimate tensile strength of the weakest matrix in the matrix of the pre-coated plate 2. In this context, the weakest matrix is ​​defined as described above.

[0127] For example, the average nickel content Ni of welded joint 22 WJIncluded in the range of 0.1 wt% to 13.6 wt%, and more particularly in the range of 0.2 wt% to 12.0 wt%.

[0128] For example, the average chromium content (Cr) of welded joint 22 WJ Greater than or equal to 0.05% by weight.

[0129] For example, after hot pressing and cooling in a pressing tool, the maximum hardness change ΔHV (WJ) across the weld joint 22 is less than or equal to the average hardness HV of the weld joint 22. mean (WJ) 20%. In other words, .

[0130] For example, the welded joint 22 after hot pressing and cooling in a pressing tool results in an average hardness HV. mean (WJ) less than or equal to 700 HV.

[0131] Preferably, the composition of the welded joint 22 is such that it has a predominantly martensitic microstructure after hot pressing and cooling. "Predominantly" means that it comprises at least 95% martensite, and more particularly 100% martensite.

[0132] The present invention also relates to a method for producing welded, hot-pressed, and cooled steel parts, the method comprising: - Produce welded steel billet 1 using the method described above; - Heat the welded steel billet 1 to obtain a fully austenitic structure in the matrix of the pre-coated plate 2 that constitutes the welded billet 1; - Hot pressing of welded steel billet 1 in a pressing tool to obtain steel parts; and - Cool the steel parts in the pressing tool.

[0133] More specifically, during the heating step, the weld billet 1 is heated to the austenitizing temperature. It is then held at the austenitizing temperature for a duration depending on the thickness of the plate 2 forming the weld billet 1. This holding time is selected based on the austenitizing temperature to austenitize the weld billet 1 and to allow the formation of an alloyed intermetallic layer of predetermined thickness through alloying between the substrate and the pre-coating 5. For example, the holding time is approximately 5 minutes.

[0134] Before hot pressing, the thus heated welded steel billet 1 is transferred to a hot forming pressing tool. The transfer time is advantageously between 5 and 10 seconds. The transfer time is chosen to be as short as possible in order to avoid metallurgical transformation in the welded steel billet 1 before hot pressing.

[0135] During the cooling step, the cooling rate is greater than or equal to the critical martensite or bainite cooling rate of at least one matrix of the two steel plates (e.g., the most hardenable steel plate, i.e., the steel plate with the lowest critical cooling rate).

[0136] After cooling, the welded joint 22 has a microstructure that is predominantly martensite. "Predominantly" means that it comprises at least 95% martensite, and more specifically 100% martensite.

[0137] The present invention also relates to welded, hot-pressed and cooled steel parts obtained using the above method.

[0138] More specifically, the steel part comprises a first coated steel part portion and a second coated steel part portion, which are respectively produced by hot pressing and cooling of two pre-coated steel sheets in a pressing tool.

[0139] More specifically, each coated steel part comprises a steel substrate having a coating comprising iron and aluminum on its respective main surfaces, and the first and second steel parts are joined by a weld joint 22 as described above.

[0140] Specifically, the coatings on the first and second steel parts are produced by at least partial alloying of the pre-coating 5 during hot pressing.

[0141] The substrates of the first and second steel parts have the composition of the pre-coated plate 2 described above. They are produced by hot pressing and cooling the substrate of the pre-coated plate 2.

[0142] Each steel part is adjacent to the weld joint 22 and includes an intermediate region on each surface of the steel part. This intermediate region is created by the intermediate region 28 described with respect to the welded steel billet 1. In the intermediate region, the coating thickness is strictly less than the thickness in the rest of the steel part, or even nonexistent.

[0143] Welded joint 22 shall comply with the above guidelines C1, C2 and C3.

[0144] Furthermore, the welded joint 22 has an average aluminum content Al ranging from 0.1 wt% to 1.2 wt%. WJ The average aluminum content of welded joint 22 is, for example, greater than or equal to 0.15% by weight. For example, the average aluminum content of welded joint 22 is less than or equal to 0.8% by weight.

[0145] The Charpy energy of welded joint 22 at 20℃ is greater than or equal to 25 J / cm². 2 Furthermore, the ultimate tensile strength of the part is greater than or equal to the ultimate tensile strength of the weakest matrix in the coating steel part.

[0146] For example, welded joint 22 has an average nickel content (Ni) ranging from 0.1 wt% to 13.6 wt%, and more particularly from 0.2 wt% to 12.0 wt%. WJ .

[0147] For example, welded joint 22 has an average chromium content of Cr greater than or equal to 0.05% by weight. WJ .

[0148] For example, the maximum hardness variation ΔHV (WJ) across the weld joint 22 is less than or equal to the average hardness HV of the weld joint 22. mean (WJ) 20%. In other words, .

[0149] Average hardness HV in welded joint 22 mean (WJ) For example, less than or equal to 700 HV.

[0150] Preferably, the welded joint 22 has a microstructure that is predominantly martensitic. "Predominantly" means that it comprises at least 95% martensite, and more particularly 100% martensite.

[0151] The inventors of this invention conducted an experiment to produce welded steel billet 1 by laser welding two pre-coated plates A and B together using filler wire W.

[0152] Table 1 below lists the experimental conditions for each experiment, E1 to E20.

[0153] The initially supplied pre-coated plates A and B have a pre-coating layer 5 with a thickness of approximately 25 micrometers on their two main surfaces 4.

[0154] For all tested pre-coated plates A and B, the pre-coating layer 5 was obtained by hot-dip coating in a molten metal bath and includes a metal alloy layer 11 and an intermetallic alloy layer 9.

[0155] The metal alloy layer 11 of the pre-coating 5 comprises, by weight: Si: 9% Fe: 3% The remainder consists of aluminum and possible impurities produced by refining.

[0156] The average total thickness of the metal alloy layer 11 is 20 μm.

[0157] Intermetallic alloy layer 9 contains Fe x -Aly type intermetallic compounds, mostly Fe2Al3, Fe2Al5 and Fe... x Al y Si z It has an average thickness of 5 µm.

[0158] For all tested pre-coated boards A and B, removal areas 18 were created on both main surfaces by removing the metal alloy layer 11, while the intermetallic alloy layer remained intact. Removal was performed by laser ablation using the method disclosed in previous application WO 2007 / 118939.

[0159]

[0160] Table 1: List of experimental conditions

[0161] In the table above, experiments not included in this invention are indicated by underline.

[0162] In the table above, "0" in the "Percentage of filler wire added to the weld pool" column means that no filler wire was added.

[0163] The steel matrix used in the different experiments described in Table 1 has the composition listed in Table 2 below, with the content expressed as % by weight.

[0164]

[0165] Table 2: Composition of the matrix

[0166] For all the matrix components, the remaining composition consists of iron, possible impurities, and unavoidable elements produced during manufacturing.

[0167] In Table 2 above, "-" means that the matrix includes at most trace amounts of the elements under consideration.

[0168] The filler wire W used in the different experiments described in Table 1 has the composition listed in Table 3 below, with the content expressed as a percentage by weight.

[0169]

[0170] Table 3: Composition of filler wire W

[0171] For all filler wires, the remaining composition consists of iron, possible impurities, and unavoidable elements produced during manufacturing.

[0172] Unless otherwise indicated, these filler wires may include Al, Cu, Nb, Ti, N, V ​​and Co in amounts of about 0.001%, which corresponds to trace amounts of these elements.

[0173] Then, for each experiment E1 to E20, the inventors used conventional measurement methods to measure the composition of the obtained welded joints 22.

[0174] The average manganese, aluminum, nickel, chromium, and silicon contents of weld joint 22 were determined by averaging across the entire surface of the weld, analyzed using an energy-dispersive spectroscopy detector integrated into a scanning electron microscope. The average carbon content was determined using a Castaing electron microprobe on a cross-section of a sample taken perpendicular to weld joint 22. These measurements are listed in Table 4 below.

[0175]

[0176] Table 4: Content measured in welded joints

[0177] Furthermore, the inventors subjected the welded steel billet 1 produced therefrom to a heat treatment including austenitization, followed by rapid cooling, to obtain a heat-treated part. This heat-treated part exhibits the same characteristics as parts that are hot-pressed and cooled.

[0178] The inventors then conducted measurements to determine the mechanical properties of these parts (the ultimate tensile strength of hot-pressed and cooled parts and the Charpy energy of welded joints).

[0179] They further compared the measured ultimate tensile strength (UTS) of hot-pressed and cooled parts. part ) and the ultimate tensile strength (UTS) of the weakest matrix after heat treatment weakest substrate ).

[0180] The mechanical properties determined as a result are shown in Table 5 below.

[0181]

[0182] Table 5: Mechanical properties after heat treatment

[0183] In the table above, "nd" means "undetermined".

[0184] Tensile tests were performed on transverse weld tensile specimens of type EN 12.5×50 (240×30 mm) extracted perpendicular to the laser welding direction at ambient temperature (approximately 20°C) using the methods disclosed in the following standards: NF EN ISO 4136 and NF ISO 6892-1. Five tensile tests were performed for each test (E1 to E21).

[0185] Charpy energy was measured using a standard Charpy impact test, employing a specimen with a V-notch in weld joint 22, the V-notch having a depth of 2 mm and a total width of 8 mm. The notch was positioned in the weld joint with an accuracy of better than or equal to 0.2 mm, and the width was the dimension of the specimen parallel to the notch depth. The test was conducted at 20°C.

[0186] Based on the measured composition of the welded joint 22, the inventors determined whether each of the experiments E1 to E20 met the above criteria C1 to C3.

[0187] The results are summarized in Table 6 below.

[0188]

[0189] Table 6: Determination of Criteria in Welded Joints

[0190] Underlined value: does not correspond to this invention.

[0191] As can be seen from Table 6, the experiments with reference numbers E1, E2, E5 to E14, E16 and E17 are embodiments of the present invention: in these experiments, criteria C1 to C3 are satisfied.

[0192] Conversely, the experiments with reference numbers E3, E4, E15, E18 to E20 are not according to the invention: in these experiments, at least one of the criteria C1 to C3 is not satisfied.

[0193] As can be seen from Table 5 above, in experiments E1, E2, E5 to E14, E16 and E17 that satisfy criteria C1 to C3, the hot-pressed and cooled parts obtained from the welded steel billet 1 have satisfactory mechanical properties, especially the ultimate tensile strength after heat treatment, which is greater than or equal to the ultimate tensile strength of the weakest matrix among the two matrices of the welded steel billet 1, and greater than or equal to 25 J / cm. 2 Charpy energy of welded joint 22 at 20°C.

[0194] Therefore, for parts obtained from the welded steel billet 1 according to the invention, after hot pressing and cooling, the presence of the weld joint 22 does not reduce the properties of the welded steel parts compared to the properties of the weakest matrix. Thus, despite the presence of aluminum in the weld joint, these parts will have satisfactory impact resistance.

[0195] Conversely, in experiments E3, E4, E15, E18 to E20 not according to the invention, at least one of the ultimate tensile strength of the hot-pressed and cooled parts or the Charpy energy of the weld joint is too low due to failure to meet at least one of criteria C1 to C3, and is therefore unsatisfactory. Thus, for these parts, there is a risk, for example, that the parts will fail in the weld joint under impact conditions.

[0196] Therefore, the method according to the invention is particularly advantageous because it allows for the production of parts with excellent mechanical properties (including in the weld joint 22) after hot pressing and cooling in a pressing tool, despite the presence of aluminum in the weld joint.

[0197] Therefore, this method is particularly suitable for manufacturing intrusion-proof parts, structural parts, or energy-absorbing parts that contribute to the safety of motor vehicles.

[0198] According to a specific embodiment of the method for producing welded steel billet 1 of the present invention, the step of producing two pre-coated plates 2 includes: - Provide two initially pre-coated plates 2'; - Arrange the two initially pre-coated plates 2' adjacent to each other, with a predetermined gap between them; and - The pre-coating layer 5 on two adjacent initial pre-coated plates 2' is simultaneously removed by laser ablation on the removal fraction F, so that removal areas 18 are simultaneously generated on the adjacent surfaces of the two initial pre-coated plates 2', and the laser beam overlaps with the two adjacent initial pre-coated plates 2' during the removal step.

[0199] During the welding step, the two adjacent pre-coated plates 2 thus prepared are welded by a laser beam spot that overlaps with the two pre-coated plates 2. Preferably, the time between the end of laser ablation and the start of welding is less than or equal to 10 seconds.

[0200] The resulting welded steel billet 1 has various intermediate regions 28 including solidified stripes produced by laser ablation.

[0201] Because the pre-coating layer 5 is removed simultaneously on the removal fraction F using a laser beam that overlaps with the two initially pre-coated plates 2, the curing stripes on the adjacent main surfaces of the two pre-coated plates 2 are symmetrical with respect to the vertical mid-plane M between the two pre-coated plates 2.

[0202] In addition, as previously mentioned Figure 5 As mentioned, each intermediate region 28 includes an inner edge 30 located at the weld joint 22 and an outer edge 32 located away from the weld joint 22.

[0203] In this particular embodiment, due to the simultaneous ablation method, the distance between the outer edges of adjacent intermediate regions of the two pre-coated plates is approximately constant along the longitudinal direction of the weld joint 22. "Approximately constant" means that the distance between the outer edges 32 of adjacent intermediate regions of the two pre-coated plates 2 varies by at most 5% along the weld joint 22 (i.e., along the longitudinal direction of the weld joint 22).

[0204] The present invention also relates to a part obtained by hot pressing and cooling welding of a steel billet 1 using a method according to a particular embodiment.

[0205] The hot-pressed and cooled part has the same characteristics as described above.

[0206] Furthermore, in this part, each intermediate region includes curing stripes, and the curing stripes on the adjacent main surfaces of the two coated steel parts are symmetrical with respect to the vertical intermediate plane between the two coated steel parts.

[0207] Preferably, each intermediate region includes an inner edge located at the weld joint 22 and an outer edge away from the weld joint 22, and the distance between the outer edges of adjacent intermediate regions of two coated steel part portions is substantially constant along the longitudinal direction of the weld joint 22. "Substantially constant" means that the distance between the outer edges of adjacent intermediate regions of two coated steel part portions varies by at most 5% along the weld joint 22 (i.e., along the longitudinal direction of the weld joint 22).

[0208] According to embodiments of the present invention, the following notes are also disclosed: 1. A method for producing welded steel billets (1), the method comprising the following sequential steps: - Provide two pre-coated plates (2), each pre-coated plate (2) comprising a steel substrate (3) having a pre-coating layer (5) on each of its two main surfaces (4), the pre-coating layer (5) comprising: an intermetallic alloy layer (9) comprising at least iron and aluminum. Each pre-coated plate (2) includes a removal area (18) on its respective main surface (4) at the weld edge (14) intended to be at least partially incorporated into the weld joint (22), in which the pre-coating layer (5) has been removed with a removal fraction (F) of the thickness of the pre-coating layer (5) between 30% and 100%. - The pre-coated plates (2) are butt-welded using filler wire (20) to create a weld joint (22) at the joint between the pre-coated plates (2), the weld joint (22) having an average aluminum content between 0.1% and 1.2% by weight. Its features are: -So that the resulting weld joint (22) is characterized by selecting the composition and proportion of the filler wire (20) added to the weld pool in a manner as follows: (a) The quenching factor FT of the welded joint WJ , making , in, -FT BM It is the quenching factor of the steel matrix (3) that is the most difficult to harden among the two pre-coated plates (2) and - The quenching factor FT is determined using the following formula. WJ and FT BMFT = 128 + 1553xC + 55xMn + 267xSi + 49xNi + 5xCr - 79xAl - 2xNi² - 1532xC² - 5xMn² - 127xSi² - 40xCxNi - 4xNixMn, where Al, Cr, Ni, C, Mn, and Si are the average weight percentages of aluminum, chromium, nickel, carbon, manganese, and silicon in the region where the quenching factor is to be determined, and this region is defined by FT. WJ In the case of the welded joint (22), in FT BM In this case, it is the most difficult steel matrix to harden. (b) The average nickel content of the welded joint (22) satisfies the following relationship: Ni WJ ≤14-3.4xAl WJ , where Al WJ The average aluminum content, Ni of the welded joint (22) is... WJ The average nickel content of the welded joint (22); and (c) The average chromium content of the welded joint (22) satisfies the following relationship: Cr WJ ≤5-2xAl WJ , where Al WJ The average aluminum content, Cr of the welded joint (22) is... WJ It is the average chromium content of the welded joint (22).

[0209] 2. According to the method described in Appendix 1, wherein, for at least one of the pre-coated plates (2), the pre-coating layer (5) further includes: a metal alloy layer (11) extending on top of the intermetallic alloy layer (9), the metal alloy layer (11) being an aluminum layer, an aluminum alloy layer or an aluminum-based alloy layer.

[0210] 3. The method according to Appendix 1 or 2, wherein the steel of the substrate (3) of at least one of the pre-coated plates (2) comprises, by weight: 0.10%≤C≤0.5% 0.5%≤Mn≤4.5% 0.1%≤Si≤1% 0.01%≤Cr≤1% Ti≤0.2% Al≤0.1% S≤0.05% P≤0.1% B≤0.010% The remainder consists of iron and impurities produced during manufacturing.

[0211] 4. The method according to Appendix 1 or 2, wherein the steel of the substrate (3) of both pre-coated plates (2) comprises, by weight: 0.10%≤C≤0.5% 0.5%≤Mn≤4.5% 0.1%≤Si≤1% 0.01%≤Cr≤1% Ti≤0.2% Al≤0.1% S≤0.05% P≤0.1% B≤0.010% The remainder consists of iron and impurities produced during manufacturing.

[0212] 5. The method according to Appendix 1 or 2, wherein the average aluminum content of the welded joint (22) is greater than or equal to 0.15 by weight.

[0213] 6. The method according to Appendix 1 or 2, wherein the average aluminum content of the welded joint (22) is less than or equal to 0.8% by weight.

[0214] 7. The method according to Appendix 1 or 2, wherein the average nickel content of the welded joint (22) is between 0.1% by weight and 13.6% by weight.

[0215] 8. The method according to Appendix 1 or 2, wherein the average nickel content of the welded joint (22) is between 0.2% by weight and 12.0% by weight.

[0216] 9. The method according to Appendix 1 or 2, wherein the welded steel billet is such that, after hot pressing and cooling, - The Charpy energy of the welded joint (22) at 20°C is greater than or equal to 25 J / cm²; and The ultimate tensile strength of the hot-pressed and cooled welded steel billet is greater than or equal to the ultimate tensile strength of the weakest matrix in the matrix (3) of the pre-coated plate (2), the weakest matrix (3) being the matrix (3) with the lowest product of thickness and ultimate tensile strength after hot pressing and cooling.

[0217] 10. The method according to Appendix 1 or 2, wherein the filler wire (20) has a carbon content ranging from 0.01% by weight to 0.45% by weight.

[0218] 11. The method according to Appendix 1 or 2, wherein, for at least one pre-coated plate (2), the removal fraction (F) is strictly less than 100% of the thickness of the pre-coating layer (5).

[0219] 12. The method according to Appendix 1 or 2, wherein, for at least one pre-coated plate (2), the pre-coating layer (5) comprises a metal alloy layer (11) extending on top of the intermetallic alloy layer (9), the metal alloy layer (11) being and wherein the metal alloy layer (11) has been removed over its entire thickness, while the intermetallic alloy layer (9) remains intact in the removal area (18) on each of the main surfaces (4) of the pre-coated plate (2).

[0220] 13. The method according to Appendix 1 or 2, wherein, for at least one pre-coated board (2) provided in the step of providing two pre-coated boards (2), the removal fraction in the removal area (18) on each main surface (4) of the pre-coated board (2) is equal to 100%, such that the pre-coating layer (5) has been removed over its entire thickness.

[0221] 14. According to the method described in Appendix 1 or 2, prior to the step of providing two pre-coated plates (2), the method further includes a step of producing the two pre-coated plates (2) from the respective initial pre-coated plates (2'), which includes the following sub-step: obtaining the removal area (18) on each main surface (4) of each pre-coated plate (2) by laser ablation at the weld edge (14) of the pre-coated plate (2) to remove the pre-coating (5) with a removal fraction (F) of the thickness of the pre-coating (5) including between 30% and 100%.

[0222] 15. The method according to Appendix 14, wherein the step of producing the two pre-coated plates (2) comprises: - Provide two initially pre-coated plates (2'); - Arrange the two initially pre-coated plates (2') adjacent to each other, with a predetermined gap between them; and - The pre-coating layer (5) on the two adjacent initially pre-coated plates (2') is removed simultaneously by laser ablation, so that the removal area (18) is generated simultaneously on the adjacent surfaces of the two initially pre-coated plates (2'), and the laser beam for laser ablation overlaps with the two adjacent initially pre-coated plates (2') during the removal step.

[0223] 16. The method according to Appendix 1 or 2 further comprises: preparing the welding edge (14) of at least one of the pre-coated plates (2) using at least one of the following processing steps prior to butt welding: brushing, machining, chamfering and / or beveling.

[0224] 17. The method according to Appendix 1 or 2, wherein the welding step is performed using a laser beam.

[0225] 18. The method according to Appendix 1 or 2, wherein, for at least one of the pre-coated plates (2), the steel of the substrate (3) comprises, by weight: 0.15%≤C≤0.25% 0.8%≤Mn≤1.8% 0.1%≤Si≤0.35% 0.01%≤Cr≤0.5% Ti≤0.1% Al≤0.1% S≤0.05% P≤0.1% B≤0.005% The remainder consists of iron and impurities produced during manufacturing.

[0226] 19. The method according to Appendix 1 or 2, wherein, for one of the pre-coated plates (2), the steel of the substrate (3) comprises, by weight: 0.040%≤C≤0.100% 0.80%≤Mn≤2.00% Si≤0.30% S≤0.005% P≤0.030% 0.010%≤Al≤0.070% 0.015%≤Nb≤0.100% Ti≤0.080% N≤0.009% Cu≤0.100% Ni≤0.100% Cr≤0.100% Mo≤0.100% Ca≤0.006%, The remainder consists of iron and impurities produced during manufacturing.

[0227] 20. The method according to Appendix 1 or 2, wherein, for one of the pre-coated plates (2), the steel of the substrate (3) comprises, by weight: 0.24%≤C≤0.38% 0.40%≤Mn≤3% 0.10%≤Si≤0.70% 0.015%≤AI≤0.070% 0%≤Cr≤2% 0.25%≤Ni≤2% 0.015%≤Ti≤0.10% 0%≤Nb≤0.060% 0.0005%≤B≤0.0040% 0.003%≤N≤0.010% 0.0001%≤S≤0.005% 0.0001%≤P≤0.025% The titanium and nitrogen contents satisfy the following relationship: Ti / N > 3.42 Furthermore, the contents of carbon, manganese, chromium, and silicon satisfy the following relationship: , The steel comprises one or more of the following elements: 0.05%≤Mo≤0.65% 0.001%≤W≤0.30% 0.0005%≤Ca≤0.005% The remainder consists of iron and impurities that are unavoidable during manufacturing.

[0228] 21. The method according to Appendix 1 or 2, wherein the welding is performed using a shielding gas.

[0229] 22. A method for producing welded, subsequently hot-pressed, and cooled steel parts, the method comprising the following sequential steps: - Perform the method described in any one of notes 1 to 18 to obtain the welded steel billet (1); - Heating the welded steel billet (1) to obtain a fully austenitic structure in the matrix (3) of the pre-coated plate (2); - The welded steel billet (1) is hot-pressed in a pressing tool to obtain a steel part; and - Cool the steel part in the pressing tool.

[0230] 23. The method according to Appendix 22, wherein during the cooling step, the cooling rate is greater than or equal to the cooling rate of the most hardenable bainite or martensite in the substrate (3) of the pre-coated plate (2).

[0231] 24. A welded steel billet (1) comprising two pre-coated plates (2), each pre-coated plate (2) comprising a steel substrate (3) having a pre-coating layer (5) on each of its main surfaces (4), the pre-coating layer (5) comprising: an intermetallic alloy layer (9) comprising at least iron and aluminum. The pre-coated plate (2) is joined by a weld joint (22) having an average aluminum content between 0.1% by weight and 1.2% by weight, and the weld joint (22) is also characterized by the following: (a) The quenching factor FT of the welded joint (22) WJ , making , in, -FT BM It is the quenching factor of the steel matrix (3) that is the most difficult to harden among the two pre-coated plates (2) and - The quenching factor FT is determined using the following formula. WJ and FT BM FT = 128 + 1553xC + 55xMn + 267xSi + 49xNi + 5xCr - 79xAl - 2xNi² - 1532xC² - 5xMn² - 127xSi² - 40xCxNi - 4xNixMn, where Al, Cr, Ni, C, Mn, and Si are the average contents of aluminum, chromium, nickel, carbon, manganese, and silicon, expressed as weight percentages, in the region where the quenching factor is to be determined, and this region is within the range of FT. WJ In the case of the welded joint (22), in FT BM In this case, it is the most difficult steel matrix to harden. (b) The average nickel content of the welded joint (22) satisfies the following relationship: Ni WJ ≤14-3.4xAl WJ , where Al WJ It is the average aluminum content of the welded joint (22), Ni WJ The average nickel content of the welded joint (22); and (c) The average chromium content of the welded joint (22) satisfies the following relationship: Cr WJ ≤5-2xAl WJ , where Al WJ It is the average aluminum content of the welded joint (22), Cr WJ The average chromium content of the welded joint (22) and Each pre-coated plate (2) includes an intermediate region (28) adjacent to the weld joint (22) on its respective main surface (4), in which the pre-coating layer (5) has been removed with a removal fraction (F) of the thickness of the pre-coating layer (5) between 30% and 100%.

[0232] 25. The welded steel billet (1) according to Appendix 24, wherein, for at least one of the pre-coated plates (2), the pre-coating layer (5) comprises: a metal alloy layer (11) extending on top of the intermetallic alloy layer (9), the metal alloy layer (11) being an aluminum layer, an aluminum alloy layer or an aluminum-based alloy layer.

[0233] 26. The welded steel billet (1) according to Appendix 24 or 25, wherein the steel of the substrate (3) of at least one of the pre-coated plates (2) comprises, by weight: 0.10%≤C≤0.5% 0.5%≤Mn≤4.5% 0.1%≤Si≤1% 0.01%≤Cr≤1% Ti≤0.2% Al≤0.1% S≤0.05% P≤0.1% B≤0.010% The remainder consists of iron and impurities produced during manufacturing.

[0234] 27. The welded steel billet (1) according to Appendix 24 or 25, wherein the steel of the substrate (3) of both pre-coated plates (2) comprises, by weight: 0.10%≤C≤0.5% 0.5%≤Mn≤4.5% 0.1%≤Si≤1% 0.01%≤Cr≤1% Ti≤0.2% Al≤0.1% S≤0.05% P≤0.1% B≤0.010% The remainder consists of iron and impurities produced during manufacturing.

[0235] 28. The welded steel billet (1) according to Appendix 24 or 25, wherein, for each pre-coated plate (2), the width of the intermediate region (28) includes a distance of 5 μm to 2000 μm from the edge of the weld joint (22).

[0236] 29. The welded steel billet (1) according to Appendix 24 or 25, wherein, for at least one pre-coated plate (2), the removal fraction (F) is equal to 100% of the thickness of the pre-coating layer (5).

[0237] 30. The welded steel billet (1) according to Appendix 24 or 25, wherein, for at least one pre-coated plate (2), the removal fraction (F) is strictly less than 100% of the thickness of the pre-coating layer (5).

[0238] 31. The welded steel billet (1) according to Appendix 30, wherein, for at least one pre-coated plate (2), the pre-coating layer (5) comprises a metal alloy layer (11) extending on top of the intermetallic alloy layer (9), the metal alloy layer (11) being an aluminum layer, an aluminum alloy layer or an aluminum-based alloy layer, and wherein, for at least one pre-coated plate (2), and wherein the metal alloy layer (11) has been removed over its entire thickness, while the intermetallic alloy layer (9) remains intact in the removed areas (18) on each of the main surfaces (4) of the pre-coated plate (2).

[0239] 32. The welded steel billet (1) according to Appendix 24 or 25, wherein the nickel content of the welded joint (22) is between 0.1% by weight and 13.6% by weight.

[0240] 33. The welded steel billet (1) according to Appendix 24 or 25, wherein the nickel content of the welded joint (22) is between 0.2% by weight and 12.0% by weight.

[0241] 34. The welded steel billet (1) according to Appendix 24 or 25, wherein the welded steel billet (1) is such that, after hot pressing and cooling, - The Charpy energy of the welded joint (22) at 20°C is greater than or equal to 25 J / cm²; and - The ultimate tensile strength of the hot-pressed and cooled welded steel billet is greater than or equal to the ultimate tensile strength of the weakest matrix in the matrix (3) of the pre-coated plate (2), the weakest matrix (3) being the matrix with the lowest product of thickness and ultimate tensile strength after hot pressing and cooling.

[0242] 35. The welded steel billet (1) according to Appendix 24 or 25, wherein the welded joint (22) is such that, after hot pressing and cooling, the maximum hardness variation across the welded joint (22) is less than or equal to 20% of the average hardness of the welded joint (22).

[0243] 36. The welded steel billet (1) according to Appendix 24 or 25, wherein each intermediate region (28) includes curing stripes, and the curing stripes on the adjacent main surfaces (4) of the two pre-coated plates (2) are symmetrical with respect to the vertical intermediate plane (M) between the two pre-coated plates (2).

[0244] 37. The welded steel billet (1) according to Appendix 24 or 25, wherein each intermediate region (28) includes an inner edge (30) located at the weld joint (22) and an outer edge (32) away from the weld joint (22), and wherein the distance between the outer edges (32) of the adjacent intermediate regions (28) of the two pre-coated plates (2) is constant along the longitudinal direction of the weld joint (22).

[0245] 38. A welded, hot-pressed, and cooled steel part, the steel part comprising a first coated steel part portion and a second coated steel part portion, each coated steel part portion comprising a steel substrate (3) having a coating comprising at least iron and aluminum on at least one of its main surfaces. The first coated steel part portion and the second coated steel part portion are joined by a weld joint (22), the weld joint (22) having an average aluminum content between 0.1% by weight and 1.2% by weight, and the weld joint (22) is also characterized by the following: (a) The quenching factor FT of the welded joint (22) WJ , making , in, -FT BM It is the quenching factor of the steel matrix (3) that is the most difficult to harden among the steel matrix (3) of the first coated steel part portion and the second coated steel part portion, and - The quenching factor FT is determined using the following formula. WJ and FT BM FT = 128 + 1553xC + 55xMn + 267xSi + 49xNi + 5xCr - 79xAl - 2xNi² - 1532xC² - 5xMn² - 127xSi² - 40xCxNi - 4xNixMn, where Al, Cr, Ni, C, Mn, and Si are the average contents of aluminum, chromium, nickel, carbon, manganese, and silicon, expressed as weight percentages, in the region for which the quenching factor is to be determined. WJ In the case of the welded joint (22), in FT BM In this case, it is the most difficult steel matrix to harden. (b) The average nickel content of the welded joint (22) satisfies the following relationship: Ni WJ ≤14-3.4xAl WJ , where Al WJ The average aluminum content, Ni of the welded joint (22) is... WJ The average nickel content of the welded joint (22); and (c) The average chromium content of the welded joint (22) satisfies the following relationship: Cr WJ ≤5-2xAl WJ , where Al WJ The average aluminum content, Cr of the welded joint (22) is... WJ The average chromium content of the welded joint (22) is... and Each coated steel part includes an intermediate region (28) adjacent to the weld joint (22) on its respective main surface, in which the thickness of the coating is strictly smaller than that of the adjacent regions of the coated steel part, which are located further away from the weld joint (22) than the intermediate region, or in which the coating is not present.

[0246] 39. The welded, hot-pressed, and cooled steel part according to Appendix 38, wherein the steel of the substrate (3) of at least one of the first coated steel part portion and the second coated steel part portion comprises, by weight: 0.10%≤C≤0.5% 0.5%≤Mn≤4.5% 0.1%≤Si≤1% 0.01%≤Cr≤1% Ti≤0.2% Al≤0.1% S≤0.05% P≤0.1% B≤0.010% The remainder consists of iron and impurities produced during manufacturing.

[0247] 40. The welded, hot-pressed, and cooled steel part according to Appendix 38, wherein the steel of the substrate (3) of the first coated steel part portion and the second coated steel part portion comprises, by weight: 0.10%≤C≤0.5% 0.5%≤Mn≤4.5% 0.1%≤Si≤1% 0.01%≤Cr≤1% Ti≤0.2% Al≤0.1% S≤0.05% P≤0.1% B≤0.010% The remainder consists of iron and impurities produced during manufacturing.

[0248] 41. The welded, hot-pressed and cooled steel parts according to Appendix 38 or 39, wherein each intermediate region includes curing stripes, and the curing stripes on adjacent main surfaces (4) of the two coated steel parts are symmetrical with respect to the vertical intermediate plane between the two coated steel parts.

[0249] 42. The welded, hot-pressed and cooled steel part according to Appendix 38 or 39, wherein each intermediate region includes an inner edge located at the weld joint (22) and an outer edge away from the weld joint (22), and wherein the distance between the outer edges of the adjacent intermediate regions of the two coated steel part portions is constant along the longitudinal direction of the weld joint (22).

[0250] 43. The welded, hot-pressed and cooled steel parts according to Appendix 38 or 39, wherein the average hardness of the welded joint (22) is less than or equal to 700 HV.

[0251] 44. The welded, hot-pressed and cooled steel parts according to Appendix 38 or 39, wherein the average nickel content of the welded joint (22) is between 0.1% by weight and 13.6% by weight.

[0252] 45. The welded, hot-pressed and cooled steel parts according to Appendix 38 or 39, wherein the average nickel content of the welded joint (22) is between 0.2% by weight and 12.0% by weight.

[0253] 46. ​​The welded, hot-pressed, and cooled steel parts as described in Appendix 38 or 39, wherein, - The Charpy energy of the welded joint (22) at 20°C is greater than or equal to 25 J / cm²; and - The ultimate tensile strength of the welded, hot-pressed and cooled steel part is greater than or equal to the ultimate tensile strength of the weakest matrix in the matrix (3) of the coated steel part portion, the weakest matrix (3) being the matrix with the lowest product of thickness and ultimate tensile strength.

[0254] 47. The welded, hot-pressed and cooled steel parts according to Appendix 38 or 39, wherein the maximum hardness variation across the weld joint (22) is less than or equal to 20% of the average hardness of the weld joint (22).

[0255] 48. The welded, hot-pressed, and cooled steel part according to Appendix 38 or 39, wherein the steel of the substrate (3) of at least one of the first coated steel part portion and the second coated steel part portion comprises, by weight: 0.15%≤C≤0.25% 0.8%≤Mn≤1.8% 0.1%≤Si≤0.35% 0.01%≤Cr≤0.5% Ti≤0.1% Al≤0.1% S≤0.05% P≤0.1% B≤0.005% The remainder consists of iron and impurities produced during manufacturing.

[0256] 49. The welded, hot-pressed, and cooled steel part according to Appendix 38 or 39, wherein the steel of the substrate (3) of one of the first coated steel part portion and the second coated steel part portion comprises, by weight: 0.040%≤C≤0.100% 0.80%≤Mn≤2.00% Si≤0.30% S≤0.005% P≤0.030% 0.010%≤Al≤0.070% 0.015%≤Nb≤0.100% Ti≤0.080% N≤0.009% Cu≤0.100% Ni≤0.100% Cr≤0.100% Mo≤0.100% Ca≤0.006%, The remainder consists of iron and impurities produced during manufacturing.

[0257] 50. The welded, hot-pressed, and cooled steel part according to Appendix 38 or 39, wherein the steel of the substrate (3) of one of the first coated steel part portion and the second coated steel part portion comprises, by weight: 0.24%≤C≤0.38% 0.40%≤Mn≤3% 0.10%≤Si≤0.70% 0.015%≤AI≤0.070% 0%≤Cr≤2% 0.25%≤Ni≤2% 0.015%≤Ti≤0.10% 0%≤Nb≤0.060% 0.0005%≤B≤0.0040% 0.003%≤N≤0.010% 0.0001%≤S≤0.005% 0.0001%≤P≤0.025% The titanium and nitrogen contents satisfy the following relationship: Ti / N > 3.42 Furthermore, the contents of carbon, manganese, chromium, and silicon satisfy the following relationship: , The steel comprises one or more of the following elements: 0.05%≤Mo≤0.65% 0.001%≤W≤0.30% 0.0005%≤Ca≤0.005% The remainder consists of iron and impurities that are unavoidable during manufacturing.

[0258] 51. The use of welded, hot-pressed and cooled steel parts as described in Appendix 38 or 39 for the production of intrusion prevention parts or energy-absorbing parts for motor vehicles.

Claims

1. A welded, hot-pressed, and cooled steel part, the steel part comprising a first coated steel part portion and a second coated steel part portion, each coated steel part portion comprising a steel substrate (3) having a coating comprising at least iron and aluminum on at least one main surface thereof. The first coated steel part portion and the second coated steel part portion are joined by a weld joint (22), said weld joint (22) having an average aluminum content (Al) between 0.1 wt% and 1.2 wt%. WJ Furthermore, the welded joint (22) is also characterized by the following: (a) The quenching factor FT of the welded joint (22) WJ , making , in, -FT BM It is the hardening factor of the steel matrix (3) that is the most difficult to harden among the first coated steel part portion and the second coated steel part portion, and - The quenching factor FT is determined using the following formula. WJ and FT BM FT = 128 + 1553xC + 55xMn + 267xSi + 49xNi + 5xCr - 79xAl - 2xNi² - 1532xC² - 5xMn² - 127xSi² - 40xCxNi - 4xNixMn, where Al, Cr, Ni, C, Mn, and Si are the average contents of aluminum, chromium, nickel, carbon, manganese, and silicon, expressed as weight percentages, in the region for which the quenching factor is to be determined. WJ In the case of the welded joint (22), in FT BM In this case, it is the most difficult steel matrix to harden. (b) The average nickel content of the welded joint (22) satisfies the following relationship: Ni WJ ≤14-3.4xAl WJ , where Al WJ The average aluminum content and Ni of the welded joint (22) are... WJ The average nickel content of the welded joint (22); and (c) The average chromium content of the welded joint (22) satisfies the following relationship: Cr WJ ≤5-2xAl WJ , where Al WJ The average aluminum content and Cr of the welded joint (22) are... WJ The average chromium content of the welded joint (22) is... Each coated steel part portion includes an intermediate region (28) adjacent to the weld joint (22) on its respective main surface, in which the thickness of the coating is strictly smaller than that of the adjacent regions of the coated steel part portion, which are located further away from the weld joint (22) than the intermediate region, or in which the coating is absent; and The microstructure of the welded joint (22) comprises at least 95% martensite.

2. The welded, hot-pressed, and cooled steel part according to claim 1, wherein, The steel substrate (3) of at least one of the first coated steel part portion and the second coated steel part portion comprises, by weight: 0.10%≤C≤0.5% 0.5%≤Mn≤4.5% 0.1%≤Si≤1% 0.01%≤Cr≤1% Ti≤0.2% Al≤0.1% S≤0.05% P≤0.1% B≤0.010% The remainder consists of iron and impurities produced during manufacturing.

3. The welded, hot-pressed, and cooled steel part according to claim 1, wherein, The steel substrate (3) in both the first coated steel part portion and the second coated steel part portion comprises, by weight: 0.10%≤C≤0.5% 0.5%≤Mn≤4.5% 0.1%≤Si≤1% 0.01%≤Cr≤1% Ti≤0.2% Al≤0.1% S≤0.05% P≤0.1% B≤0.010% The remainder consists of iron and impurities produced during manufacturing.

4. The welded, hot-pressed, and cooled steel part according to claim 1 or 2, wherein, Each intermediate region includes curing stripes, and the curing stripes on the adjacent main surfaces (4) of the first coated steel part and the second coated steel part are symmetrical with respect to the vertical intermediate plane between the first coated steel part and the second coated steel part.

5. The welded, hot-pressed, and cooled steel part according to claim 1 or 2, wherein, Each intermediate region includes an inner edge located at the weld joint (22) and an outer edge away from the weld joint (22), and wherein the distance between the outer edges of adjacent intermediate regions of the first coated steel part and the second coated steel part portions is constant along the longitudinal direction of the weld joint (22).

6. The welded, hot-pressed, and cooled steel part according to claim 1 or 2, wherein, The average hardness of the welded joint (22) is less than or equal to 700 HV.

7. The welded, hot-pressed, and cooled steel part according to claim 1 or 2, wherein, The average nickel content (Ni) of the welded joint (22) WJ (Included in the range of 0.1% by weight to 13.6% by weight) 8. The welded, hot-pressed, and cooled steel part according to claim 1 or 2, wherein, The average nickel content of the welded joint (22) is between 0.2% by weight and 12.0% by weight.

9. The welded, hot-pressed, and cooled steel part according to claim 1 or 2, wherein, - The Charpy energy of the welded joint (22) at 20°C is greater than or equal to 25 J / cm²; and - The ultimate tensile strength of the welded, hot-pressed and cooled steel part is greater than or equal to the ultimate tensile strength of the weakest matrix in the steel matrix (3) of the coated steel part portion, the weakest matrix being the matrix with the lowest product of thickness and ultimate tensile strength.

10. The welded, hot-pressed, and cooled steel part according to claim 1 or 2, wherein, The maximum hardness variation across the weld joint (22) is less than or equal to 20% of the average hardness of the weld joint (22).

11. The welded, hot-pressed, and cooled steel part according to claim 1 or 2, wherein, The steel substrate (3) of at least one of the first coated steel part portion and the second coated steel part portion comprises, by weight: 0.15%≤C≤0.25% 0.8%≤Mn≤1.8% 0.1%≤Si≤0.35% 0.01%≤Cr≤0.5% Ti≤0.1% Al≤0.1% S≤0.05% P≤0.1% B≤0.005% The remainder consists of iron and impurities produced during manufacturing.

12. The welded, hot-pressed, and cooled steel part according to claim 1 or 2, wherein, The steel substrate (3) of one of the first coated steel part portion and the second coated steel part portion comprises, by weight: 0.040%≤C≤0.100% 0.80%≤Mn≤2.00% Si≤0.30% S≤0.005% P≤0.030% 0.010%≤Al≤0.070% 0.015%≤Nb≤0.100% Ti≤0.080% N≤0.009% Cu≤0.100% Ni≤0.100% Cr≤0.100% Mo≤0.100% Ca≤0.006%, The remainder consists of iron and impurities produced during manufacturing.

13. The welded, hot-pressed, and cooled steel part according to claim 1 or 2, wherein, The steel substrate (3) of one of the first coated steel part portion and the second coated steel part portion comprises, by weight: 0.24%≤C≤0.38% 0.40%≤Mn≤3% 0.10%≤Si≤0.70% 0.015%≤AI≤0.070% 0%≤Cr≤2% 0.25%≤Ni≤2% 0.015%≤Ti≤0.10% 0%≤Nb≤0.060% 0.0005%≤B≤0.0040% 0.003%≤N≤0.010% 0.0001%≤S≤0.005% 0.0001%≤P≤0.025% in, Ti and N satisfy the following relationship: Ti / N > 3.42 Furthermore, the contents of carbon, manganese, chromium, and silicon satisfy the following relationship: , The steel may optionally include one or more of the following elements: 0.05%≤Mo≤0.65% 0.001%≤W≤0.30% 0.0005%≤Ca≤0.005% The remainder consists of iron and impurities that are unavoidable during manufacturing.

14. The use of the welded, hot-pressed and cooled steel parts according to claim 1 or 2 for the production of anti-intrusion parts or energy-absorbing parts for motor vehicles.

Citation Information

Patent Citations

  • Method for manufacturing a welded component with very high mechanical characteristics from a coated lamination sheet

    EP2007545A1

  • Tailor welded blank, manufacturing method thereof, and hot stamped component using tailor welded blank

    EP2737971A1

  • Methods for joining two blanks and blanks and products obtained

    EP2942143A1

  • Method of manufacturing tailor welded blanks

    US20160144456A1

  • Method of producing a welded part having very high mechanical properties from a rolled and coated sheet

    WO2007118939A1