A viscous composite phase change material, a viscous composite phase change sheet, and a preparation method and application thereof

By adding crystalline polymer polyolefin into the polystyrene-fatty acid methyl ester system, the volume change of the phase change composite material is adjusted, which solves the problem that the volume change of the existing composite phase change material cannot be adjusted, improves its temperature regulation effect, and is suitable for In the field of thermal protection and heat dissipation of electronic equipment.

CN117964983BActive Publication Date: 2024-10-01PHASE CHANGE ENERGY STORAGE (BEIJING) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410167091.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-06
Publication Date
2024-10-01
Estimated Expiration
2044-02-06

AI Technical Summary

Technical Problem

Existing composite phase change materials cannot effectively adjust volume changes, resulting in poor temperature regulation effects in their thermal conductivity and heat storage functions.

Method used

Add crystalline polymer polyolefin to the polystyrene-fatty acid methyl ester system, and use the difference in the diffusion rate and state of the phase change material in the amorphous region and the crystallized region to adjust the volume shrinkage/expansion performance of the phase change composite material, thereby improving Its temperature regulating effect.

Benefits of technology

By adjusting the volume shrinkage-expansion properties of phase change composite materials and controlling the voids and contact area between them and contact objects, their application effects in thermal protection and heat dissipation of electronic equipment are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004699981760000041
    Figure BDA0004699981760000041
  • Figure BDA0004699981760000081
    Figure BDA0004699981760000081
  • Figure BDA0004699981760000091
    Figure BDA0004699981760000091
Patent Text Reader

Abstract

The present invention provides a viscous composite phase change material, a viscous composite phase change sheet, and a preparation method and application thereof. The raw materials for preparing the viscous composite phase change material include the following components by weight: 5 to 45 parts of polystyrene, 5 to 50 parts of fatty acid methyl ester, 5 to 15 parts of styrene-based thermoplastic elastomer, and 5 to 35 parts of crystalline polymer polyolefin. The viscous composite phase change material of the present invention effectively adjusts the volume shrinkage / expansion performance of the phase change composite material by adding crystalline polymer polyolefin to the polystyrene-fatty acid methyl ester system and utilizing the difference in diffusion rate and state between the amorphous region and the crystalline region during the phase change process of the phase change material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of temperature regulating materials, and in particular to a viscous composite phase change material, a viscous composite phase change sheet material, and a preparation method and application thereof. Background Art

[0002] Phase change materials have the ability to absorb or release a large amount of heat energy when changing their physical state. Taking solid-liquid phase change as an example, from solid to liquid, phase change materials absorb and store a large amount of latent heat; from liquid to solid, phase change materials will dissipate the stored heat to the environment within a certain temperature range. In these two phase change processes, the energy stored or released is called phase change latent heat, and the temperature remains almost unchanged before the phase change is completed, forming a wide temperature platform. Although the temperature remains unchanged, the latent heat absorbed or released is quite large. Once this material is widely used in people's lives, it will become the best green environmental protection carrier for energy saving and environmental protection.

[0003] However, the heat that composite phase change materials can absorb / release is limited. The art adopts a variety of methods to combine with phase change materials to give full play to the temperature regulation ability of materials. Viscous composite phase change materials can provide good heat conduction and heat storage functions by using the change in volume before and after the phase change. However, if the change in volume cannot be effectively regulated, its temperature regulation effect will be affected.

[0004] CN108329893A discloses a flexible thermal interface phase-change composite sheet material and a preparation method thereof, wherein the flexible thermal interface phase-change composite sheet material comprises expanded graphite, a phase-change material and an elastomeric material, and the expanded graphite / phase-change composite sheet material is obtained by impregnating the phase-change material under vacuum heating and filling the phase-change material into the pores of the compressed expanded graphite sheet. Although the phase-change composite sheet material has a higher thermal conductivity due to the addition of expanded graphite, the change in the volume of the sheet material cannot be effectively regulated, and the temperature regulation effect is poor.

[0005] CN114892307A discloses an aerogel-based phase-change composite material for thermal management of electronic components, wherein the aerogel is prepared by freezing and freeze-drying a nanosheet dispersion and a crosslinking agent solution after a mixed reaction. The organic phase-change material is at least one of paraffin, lauric acid, octadecane, adipic acid, capric acid, palmitic acid, stearic acid, erythritol, D-mannitol, phthalic anhydride, urea, acetamide, phthalic anhydride, polyethylene glycol or high-density polyethylene; the nanosheet material in the nanosheet dispersion is at least one of graphene, boron nitride, molybdenum disulfide, tungsten disulfide, black phosphorus, manganese dioxide, montmorillonite, expanded graphite or expanded vermiculite; although the phase-change composite sheet material uses aerogel as a carrier to encapsulate the organic phase-change material load in the aerogel, thereby improving the encapsulation rate of the phase-change material, the volume change of the sheet material cannot be effectively regulated, and the temperature adjustment effect is poor.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] One of the purposes of the present invention is to provide a viscous composite phase change material, wherein the raw materials for preparing the viscous composite phase change material include the following components by weight: 20 to 40 parts of polystyrene, 30 to 60 parts of fatty acid methyl ester, 5 to 15 parts of styrene-based thermoplastic elastomer, and 5 to 35 parts of crystalline high molecular weight polyolefin. The present invention adds crystalline high molecular weight polyolefin to the polystyrene-fatty acid methyl ester system, and utilizes the difference in diffusion rate and state between the amorphous region and the crystalline region during the phase change process of the phase change material, so as to effectively adjust the volume shrinkage / expansion performance of the phase change composite material.

[0008] The second object of the present invention is to provide a method for preparing the viscous composite phase change material, which comprises the following steps: mixing polystyrene, fatty acid methyl ester, styrene-based thermoplastic elastomer and crystalline polymer polyolefin, and performing banburying to obtain the viscous composite phase change material.

[0009] The third object of the present invention is to provide a viscous composite phase change sheet, which is obtained by pressing the viscous composite phase change material as mentioned above.

[0010] A fourth object of the present invention is to provide a method for preparing the viscous composite phase change sheet, which comprises the following steps: pressing the above-mentioned viscous composite phase change material into sheets to obtain the viscous composite phase change sheet.

[0011] A fifth object of the present invention is to provide an application of the viscous composite phase change material or the viscous composite phase change sheet in the preparation of a temperature regulating material.

[0012] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0013] In a first aspect, the present invention provides a viscous composite phase change material, wherein the raw materials for preparing the viscous composite phase change material include the following components in parts by weight:

[0014] 5 to 45 parts of polystyrene, 5 to 50 parts of fatty acid methyl ester, 5 to 15 parts of styrene-based thermoplastic elastomer, and 5 to 35 parts of crystalline high molecular weight polyolefin.

[0015] In order to make the viscous composite phase change material have a good temperature control effect, there will be specific requirements for its volume shrinkage / expansion rate. By adjusting the volume shrinkage-expansion properties of the viscous phase change composite material, the size of the cavity and contact area between it and the contact object can be controlled, thereby obtaining a better temperature control effect.

[0016] Based on this, the present invention adds crystalline high molecular weight polyolefin to the polystyrene-fatty acid methyl ester system, and utilizes the difference in diffusion rate and state between the amorphous region and the crystalline region during the phase change process of the phase change material to obtain a viscous composite phase change material that effectively regulates the volume shrinkage / expansion of the phase change composite material. The viscous composite phase change material has great application prospects in the fields of thermal protection and heat dissipation of electronic equipment, functional fabrics, etc.

[0017] In the preparation raw materials of the viscous composite phase change material, the added amount of polystyrene is 5 to 45 parts, for example, it can be 5 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 45 parts, etc.

[0018] In the preparation raw materials of the viscous composite phase change material, the added amount of fatty acid methyl ester is 5 to 50 parts, for example, it can be 5 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 46 parts, 48 ​​parts, 50 parts, etc.

[0019] In the raw materials for preparing the viscous composite phase change material, the added amount of styrene-based thermoplastic elastomer is 5 to 15 parts, for example, it can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, etc.

[0020] In the preparation raw materials of the viscous composite phase change material, the added amount of crystalline polymer polyolefin is 5 to 35 parts, for example, it can be 5 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, 35 parts, etc.

[0021] Preferably, the weight average molecular weight of the polystyrene is 6×10 4 ~10×10 4 g / mol, for example, 6×10 4 g / mol, 6.5×10 4 g / mol, 7×10 4 g / mol, 7.5×10 4 g / mol, 8×10 4 g / mol, 8.5×10 4 g / mol, 9×10 4 g / mol, 9.5×10 4 g / mol, 10×10 4 g / mol, etc.

[0022] Preferably, the melt index of the polystyrene is 3 to 8 g / 10 min, for example, 3 g / mol, 3.5 g / mol, 4 g / mol, 4.5 g / mol, 5 g / mol, 5.5 g / mol, 6 g / mol, 6.5 g / mol, 7 g / mol, 7.5 g / mol, 8 g / mol, etc.

[0023] Preferably, the structural formula of the fatty acid methyl ester is as shown in Formula I below:

[0024]

[0025] Among them, R1 is selected from a straight chain or branched alkyl group with a carbon number of 10 or more (for example, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28, 30, etc.), preferably a C12-C24 straight chain or branched alkyl group, and more preferably a C14-C18 straight chain or branched alkyl group.

[0026] As some embodiments of the present invention, the fatty acid methyl esters include but are not limited to methyl dodecanoate (methyl caprate), methyl dodecanoate (methyl laurate), methyl tetradecanoate (methyl myristic acid), methyl hexadecanoate (methyl palmitate), methyl octadecanoate (methyl stearate), methyl eicosanoate (methyl arachidate), methyl docosanoate (methyl behenate), etc.

[0027] Preferably, the fatty acid methyl ester is selected from any one of methyl stearate, methyl palmitate, methyl myristic acid, methyl laurate or methyl arachidate, or a combination of at least two thereof.

[0028] Preferably, the styrene-based thermoplastic elastomer is selected from any one or a combination of at least two of a styrene-butadiene-styrene triblock polymer, a hydrogenated styrene-butadiene-styrene triblock polymer, a styrene-isoprene-styrene triblock copolymer, a hydrogenated styrene-isoprene diblock polymer, a star-shaped styrene-ethylene-butylene-styrene block copolymer or a hydrogenated styrene-butadiene / pentadiene-styrene triblock polymer.

[0029] Preferably, the crystalline high molecular weight polyolefin is selected from any one of high density polyethylene, linear low density polyethylene or crystalline polypropylene, or a combination of at least two thereof.

[0030] Preferably, the density of the high-density polyethylene is 0.945-0.970 g / cm 3 , for example, it can be 0.945 g / cm 3 、0.950g / cm 3 , 0.955g / cm 3 、0.960g / cm 3 , 0.965g / cm 3 、0.970g / cm 3 The weight average molecular weight of the high-density polyethylene is 60000 to 300000 g / mol, for example, 60000 g / mol, 80000 g / mol, 100000 g / mol, 120000 g / mol, 140000 g / mol, 160000 g / mol, 180000 g / mol, 200000 g / mol, 220000 g / mol, 240000 g / mol, 260000 g / mol, 280000 g / mol, 300000 g / mol, etc.; The molecular weight distribution width index of the high-density polyethylene is 3 to 20, for example, it can be 3, 4, 6, 8, 10, 12, 14, 16, 18, 20, etc.; the melt index of the high-density polyethylene is 1 to 19.6 g / 10min, for example, it can be 1 g / 10min, 2 g / 10min, 4 g / 10min, 6 g / 10min, 8 g / 10min, 10 g / 10min, 12 g / 10min, 14 g / 10min, 16 g / 10min, 18 g / 10min, 19.6 g / 10min, etc.

[0031] Preferably, the density of the linear low-density polyethylene is 0.920-0.930 g / cm 3 , for example, it can be 0.920 g / cm3 , 0.921g / cm 3 , 0.922g / cm 3 , 0.923g / cm 3 , 0.924g / cm 3 、0.925g / cm 3 , 0.926g / cm 3 , 0.927g / cm 3 , 0.928g / cm 3 , 0.929g / cm 3 、0.930g / cm 3 etc.; the weight average molecular weight of linear low density polyethylene is 1.0×10 5 ~1.5×10 5 g / mol, for example, it can be 1.0×10 5 g / mol, 1.1×10 5 g / mol, 1.2×10 5 g / mol, 1.3×10 5 g / mol, 1.4×10 5 g / mol, 1.5×10 5 g / mol, etc.; the molecular weight distribution width index of the linear low density polyethylene is 4 to 5, for example, it can be 4, 4.2, 4.4, 4.6, 4.8, 5, etc.; the melt index of the linear low density polyethylene is 0.7 to 20 g / 10 min, for example, it can be 0.7 g / 10 min, 1 g / 10 min, 2 g / 10 min, 4 g / 10 min, 6 g / 10 min, 8 g / 10 min, 10 g / 10 min, 12 g / 10 min, 14 g / 10 min, 16 g / 10 min, 18 g / 10 min, 20 g / 10 min, etc.

[0032] Preferably, the density of the crystalline polypropylene is 0.90 to 0.91 g / cm 3 , for example, it can be 0.90 g / cm 3 , 0.902g / cm 3 , 0.904g / cm 3 , 0.906g / cm 3 , 0.908g / cm 3 、0.91g / cm 3 etc.; the weight average molecular weight of crystalline polypropylene is 1.4×10 5 ~1.8×10 5 g / mol, for example, 1.4×10 5The molecular weight distribution width index of the crystalline polypropylene is 1.6 to 1.8, for example, it can be 1.6, 1.65, 1.7, 1.75, 1.8, etc. The melt index of the crystalline polypropylene is 2.69 to 24.55 g / 10min, for example, it can be 2.69 g / 10min, 4 g / 10min, 6 g / 10min, 8 g / 10min, 10 g / 10min, 12 g / 10min, 14 g / 10min, 16 g / 10min, 18 g / 10min, 20 g / 10min, 22 g / 10min, 24.55 g / 10min, etc.

[0033] Preferably, the raw materials for preparing the viscous composite phase change material also include 0.5 to 5 parts of thermally conductive inorganic filler, for example, 0.5 parts, 0.6 parts, 0.8 parts, 1 parts, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, etc.

[0034] Preferably, the thermally conductive inorganic filler is selected from any one of aluminum oxide, boron nitride, carbon powder or expanded graphite, or a combination of at least two thereof.

[0035] In the present invention, the thermally conductive inorganic filler has excellent thermal stability and chemical stability, high mechanical strength and high thermal conductivity. Adding the thermally conductive inorganic filler to the viscous composite phase change material can further improve the thermal conductivity of the composite material by constructing a continuous inorganic skeleton in the polymer.

[0036] In a second aspect, the present invention provides a method for preparing the viscous composite phase change material as described in the first aspect, the preparation method comprising the following steps:

[0037] The viscous composite phase change material is obtained by mixing polystyrene, fatty acid methyl ester, styrene-based thermoplastic elastomer and crystalline high molecular weight polyolefin and performing banburying.

[0038] Preferably, the temperature of the banburying is 170-190°C, for example, it may be 170°C, 172°C, 175°C, 178°C, 180°C, 182°C, 185°C, 188°C, 190°C, etc.

[0039] Preferably, a thermally conductive inorganic filler is added during the mixing process.

[0040] Preferably, the kneading time is 0.5 to 2 h, for example, 0.5 h, 0.6 h, 0.8 h, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, 2 h, etc.

[0041] In a third aspect, the present invention provides a viscous composite phase change sheet, wherein the viscous composite phase change sheet is obtained by pressing the viscous composite phase change material as described in the first aspect.

[0042] Preferably, the thickness of the adhesive composite phase change sheet is 1 to 3 mm, for example, it may be 1 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm, 2 mm, 2.2 mm, 2.4 mm, 2.6 mm, 2.8 mm, 3 mm, etc.

[0043] Preferably, the thermal expansion coefficient of the viscous composite phase change sheet is 0.9-1.6%, for example, it can be 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.6%, 1.6%, etc.

[0044] Preferably, the thermal shrinkage rate of the adhesive composite phase change sheet is 0.9-1.6%, for example, it can be 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, etc.

[0045] In a fourth aspect, the present invention provides a method for preparing the viscous composite phase change sheet, the method for preparing the viscous composite phase change sheet comprising the following steps:

[0046] The viscous composite phase change material is pressed into sheets to obtain the viscous composite phase change sheet.

[0047] Preferably, the tableting is carried out in a vulcanizing press.

[0048] Preferably, the tabletting pressure is 1 to 3 MPa, for example, 1 MPa, 1.2 MPa, 1.4 MPa, 1.6 MPa, 1.8 MPa, 2 MPa, 2.2 MPa, 2.4 MPa, 2.6 MPa, 2.8 MPa, 3 MPa, etc.

[0049] In a fifth aspect, the present invention provides a use of the viscous composite phase change material or the viscous composite phase change sheet in the preparation of a temperature regulating material.

[0050] Compared with the prior art, the present invention has the following beneficial effects:

[0051] (1) The present invention can effectively adjust the volume shrinkage / expansion performance of the phase change composite material by adding a crystalline polymer to the polystyrene-methyl stearate system and utilizing the difference in diffusion rate and state between the amorphous region and the crystalline region during the phase change process of the phase change material;

[0052] (2) The present invention can control the size of the cavity and contact area between the viscous phase change composite material and the contact object by adjusting the volume shrinkage-expansion performance of the phase change composite material, so that the phase change material can obtain a better temperature regulation effect. DETAILED DESCRIPTION

[0053] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0054] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0055] Example 1

[0056] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0057] The viscous composite phase change material comprises the following components by weight:

[0058]

[0059]

[0060] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0061] S1. Preparation of viscous composite phase change material:

[0062] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0063] S2. Preparation of viscous composite phase change sheet:

[0064] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0065] Example 2

[0066] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0067] The viscous composite phase change material comprises the following components by weight:

[0068]

[0069] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0070] S1. Preparation of viscous composite phase change material:

[0071] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0072] S2. Preparation of viscous composite phase change sheet:

[0073] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0074] Example 3

[0075] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0076] The viscous composite phase change material comprises the following components by weight:

[0077]

[0078] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0079] S1. Preparation of viscous composite phase change material:

[0080] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0081] S2. Preparation of viscous composite phase change sheet:

[0082] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0083] Example 4

[0084] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0085] The viscous composite phase change material comprises the following components by weight:

[0086]

[0087] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0088] S1. Preparation of viscous composite phase change material:

[0089] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0090] S2. Preparation of viscous composite phase change sheet:

[0091] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0092] Example 5

[0093] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0094] The viscous composite phase change material comprises the following components by weight:

[0095]

[0096] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0097] S1. Preparation of viscous composite phase change material:

[0098] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0099] S2. Preparation of viscous composite phase change sheet:

[0100] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0101] Example 6

[0102] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0103] The viscous composite phase change material comprises the following components by weight:

[0104]

[0105] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0106] S1. Preparation of viscous composite phase change material:

[0107] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0108] S2. Preparation of viscous composite phase change sheet:

[0109] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0110] Example 7

[0111] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0112] The viscous composite phase change material comprises the following components by weight:

[0113]

[0114] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0115] S1. Preparation of viscous composite phase change material:

[0116] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0117] S2. Preparation of viscous composite phase change sheet:

[0118] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0119] Example 8

[0120] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0121] The viscous composite phase change material comprises the following components by weight:

[0122]

[0123]

[0124] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0125] S1. Preparation of viscous composite phase change material:

[0126] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0127] S2. Preparation of viscous composite phase change sheet:

[0128] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0129] Example 9

[0130] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0131] The viscous composite phase change material comprises the following components by weight:

[0132]

[0133]

[0134] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0135] S1. Preparation of viscous composite phase change material:

[0136] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0137] S2. Preparation of viscous composite phase change sheet:

[0138] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0139] Example 10

[0140] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0141] The viscous composite phase change material comprises the following components by weight:

[0142]

[0143]

[0144] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0145] S1. Preparation of viscous composite phase change material:

[0146] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0147] S2. Preparation of viscous composite phase change sheet:

[0148] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0149] Embodiment 11

[0150] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0151] The viscous composite phase change material comprises the following components by weight:

[0152]

[0153] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0154] S1. Preparation of viscous composite phase change material:

[0155] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0156] S2. Preparation of viscous composite phase change sheet:

[0157] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0158] Example 12

[0159] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0160] The viscous composite phase change material comprises the following components by weight:

[0161]

[0162] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0163] S1. Preparation of viscous composite phase change material:

[0164] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0165] S2. Preparation of viscous composite phase change sheet:

[0166] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0167] Example 13

[0168] This embodiment provides a viscous composite phase change material and a sheet prepared therefrom; the only difference from embodiment 1 is that no thermally conductive inorganic filler is added, the content of crystalline polymer polyolefin is increased to 7 parts, and the contents of other components and the preparation method are exactly the same as those in embodiment 1.

[0169] Comparative Example 1

[0170] This comparative example provides a viscous composite phase change material, and a sheet prepared therefrom;

[0171] The viscous composite phase change material comprises the following components by weight:

[0172]

[0173] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0174] S1. Preparation of viscous composite phase change material:

[0175] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler and styrene-based thermoplastic elastomer are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0176] S2. Preparation of viscous composite phase change sheet:

[0177] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0178] Comparative Example 2

[0179] This comparative example provides a viscous composite phase change material, and a sheet prepared therefrom;

[0180] The viscous composite phase change material comprises the following components by weight:

[0181]

[0182] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0183] S1. Preparation of viscous composite phase change material:

[0184] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0185] S2. Preparation of viscous composite phase change sheet:

[0186] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0187] Comparative Example 3

[0188] This comparative example provides a viscous composite phase change material, and a sheet prepared therefrom;

[0189] The viscous composite phase change material comprises the following components by weight:

[0190]

[0191] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0192] S1. Preparation of viscous composite phase change material:

[0193] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0194] S2. Preparation of viscous composite phase change sheet:

[0195] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0196] Comparative Example 4

[0197] This comparative example provides a viscous composite phase change material, and a sheet prepared therefrom;

[0198] The viscous composite phase change material comprises the following components by weight:

[0199]

[0200] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0201] S1. Preparation of viscous composite phase change material:

[0202] The polystyrene, fatty acid methyl ester, thermally conductive inorganic filler, styrene-based thermoplastic elastomer and crystalline polymer polyolefin are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 180° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0203] S2. Preparation of viscous composite phase change sheet:

[0204] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0205] Comparative Example 5

[0206] This comparative example provides a viscous composite phase change material and a sheet prepared therefrom; the only difference from Example 10 is that methyl stearate is replaced with an equal mass of octadecane, and the contents of other components and the preparation method are exactly the same as those in Example 10.

[0207] Comparative Example 6

[0208] This comparative example provides a viscous composite phase change material and a sheet prepared therefrom; the only difference from Implementation 10 is that methyl stearate is replaced with ethyl stearate of equal mass, and the contents of other components and the preparation method are exactly the same as those in Example 10.

[0209] Test Case

[0210] Test samples: the viscous composite phase change sheets provided in Examples 1 to 13, and the viscous composite phase change sheets provided in Comparative Examples 1 to 6;

[0211] Test method:

[0212] (1) Enthalpy: According to GB / T 19466.3-2004 / ISO 11357-3, DSC was used to measure the enthalpy at a heating and cooling rate of 10°C / min under nitrogen protection.

[0213] (2) Thermal expansion and thermal contraction: Cut a sheet with a side length of 20×20×1 mm; place it on an aluminum foil and mark the four sides with a marker; place it on a heated hot plate or oven at a temperature of phase change temperature + 20°C for 10 min; then cool it to a temperature of -20°C at the phase change temperature; measure the dimensions of the sheet in the warp and weft directions after the test; and calculate the thermal expansion and thermal contraction.

[0214] The specific test results are shown in Table 1:

[0215] Table 1

[0216]

[0217]

[0218] As can be seen from the test data in Table 1, the enthalpy value of the viscous composite phase change sheet of the present invention is 52-95 J / g; and the thermal expansion rate of the viscous composite phase change sheet can be controlled to be 0.9-1.6% by adjusting the content of the high melting point regulator and the nucleating agent; the thermal shrinkage rate of the viscous composite phase change sheet is 0.9-1.6%, and especially the thermal shrinkage rate is effectively improved.

[0219] It can be seen from Comparative Examples 1 to 3 that the thermal shrinkage of the adhesive composite phase change sheet is significantly reduced when no crystalline high molecular weight polyolefin is added, the content of crystalline high molecular weight polyolefin is too low, or non-crystalline high molecular weight polyolefin is used.

[0220] It can be seen from Comparative Example 4 that the thermal expansion rate and thermal shrinkage rate of the composite phase change sheet prepared by using the crystalline polymer polyolefin-fatty acid methyl ester system instead of the polystyrene-fatty acid methyl ester system are significantly reduced.

[0221] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A viscous composite phase change sheet, characterized in that: The viscous composite phase change sheet is obtained by pressing a viscous composite phase change material; Wherein, the thermal expansion coefficient of the viscous composite phase change sheet is 1.2-1.6%, and the thermal shrinkage coefficient of the viscous composite phase change sheet is 1.1-1.6%; The raw materials for preparing the viscous composite phase change material include the following components by weight: 20-45 parts of polystyrene, 5-50 parts of fatty acid methyl ester, 5-15 parts of styrene-based thermoplastic elastomer, 5-20 parts of crystalline polymer polyolefin, and 0.5-5 parts of thermally conductive inorganic filler; The structural formula of the fatty acid methyl ester is shown in the following formula I: Formula I Wherein, R1 is selected from C14~C18 straight chain or branched chain alkyl; The crystalline high molecular weight polyolefin is selected from any one or a combination of at least two of high density polyethylene, linear low density polyethylene or crystalline polypropylene; The thermally conductive inorganic filler is selected from any one of aluminum oxide, boron nitride, carbon powder or expanded graphite, or a combination of at least two thereof.

2. The adhesive composite phase change sheet according to claim 1, characterized in that: The weight average molecular weight of the polystyrene is 6×10 4 ~10×10 4 g / mol.

3. The adhesive composite phase change sheet according to claim 1, characterized in that: The melt index of the polystyrene is 3-8 g / 10min.

4. The adhesive composite phase change sheet according to claim 1, characterized in that: The fatty acid methyl ester is selected from any one of methyl stearate, methyl palmitate or methyl myristic acid, or a combination of at least two thereof.

5. The adhesive composite phase change sheet according to claim 1, characterized in that: The styrene-based thermoplastic elastomer is selected from any one or a combination of at least two of styrene-butadiene-styrene triblock polymers, hydrogenated styrene-butadiene-styrene triblock polymers, styrene-isoprene-styrene triblock copolymers, hydrogenated styrene-isoprene diblock polymers, star-shaped styrene-ethylene-butylene-styrene block copolymers, or hydrogenated styrene-butadiene / pentadiene-styrene triblock polymers.

6. The adhesive composite phase change sheet according to claim 1, characterized in that: The density of the high-density polyethylene is 0.945-0.970 g / cm 3 ; The weight average molecular weight of high-density polyethylene is 60,000~300,000 g / mol; the molecular weight distribution width index of high-density polyethylene is 3~20; the melt index of high-density polyethylene is 1~19.6 g / 10min.

7. The adhesive composite phase change sheet according to claim 1, characterized in that: The density of the linear low-density polyethylene is 0.920-0.930 g / cm 3 ; The weight average molecular weight of linear low density polyethylene is 1.0×10 5 ~1.5×10 5 g / mol; the molecular weight distribution width index of linear low density polyethylene is 4~5; the melt index of linear low density polyethylene is 0.7~20g / 10min.

8. The adhesive composite phase change sheet according to claim 1, characterized in that: The density of the crystalline polypropylene is 0.90-0.91 g / cm 3 ; The weight average molecular weight of crystalline polypropylene is 1.4×10 5 ~1.8×10 5 g / mol; the molecular weight distribution width index of crystalline polypropylene is 1.6~1.8; The melt index of crystalline polypropylene is 2.69~24.55 g / 10min.

9. The adhesive composite phase change sheet according to claim 1, characterized in that: The thickness of the viscous composite phase change sheet is 1-3 mm.

10. A method for preparing a viscous composite phase change sheet according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: The viscous composite phase change material is obtained by mixing polystyrene, fatty acid methyl ester, styrene-based thermoplastic elastomer, crystalline polymer polyolefin and thermally conductive inorganic filler, and performing banburying. The viscous composite phase change material is pressed into sheets to obtain the viscous composite phase change sheet.

11. The method for preparing the adhesive composite phase change sheet according to claim 10, characterized in that: The temperature of the banburying is 170-190° C.; the time of the banburying is 0.5-2 h.

12. The method for preparing the adhesive composite phase change sheet according to claim 10, characterized in that: The tableting is carried out in a vulcanizing press.

13. The method for preparing the adhesive composite phase change sheet according to claim 10, characterized in that: The tabletting pressure is 1-3 MPa.

14. Use of the viscous composite phase change sheet according to any one of claims 1 to 9 in preparing a temperature regulating material.