Self-healing enhanced quick-dissolving high-viscosity asphalt granules and preparation method thereof

By introducing polyurethane prepolymer and dynamic reversible covalent bonds into high-viscosity asphalt, combined with hollow fibers and graphene oxide, the problem of insufficient self-healing performance of high-viscosity asphalt is solved, achieving efficient autonomous repair and long-lasting service, which is suitable for porous Drainage pavement construction.

CN117965037BActive Publication Date: 2024-10-01BEIJING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410192815.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-21
Publication Date
2024-10-01
Estimated Expiration
2044-02-21

AI Technical Summary

Technical Problem

The existing high-viscosity asphalt loses its bonding performance during service, resulting in cracks and looseness of the pavement, and insufficient self-healing performance. Moreover, traditional self-healing enhancement technology cannot effectively repair the polymer structure.

Method used

It uses hollow fibers containing polyurethane prepolymer and dynamic reversible covalent bonds to enhance the self-healing properties of high-viscosity asphalt through intermolecular hydrogen bonds and multiple reversible covalent bonds, and uses hollow fibers to seal and protect the polyurethane prepolymer, combined with oxidation Graphene improves viscosity and high and low temperature performance.

Benefits of technology

It achieves the long-term active self-healing ability of high-viscosity asphalt, extends the service life of the pavement, simplifies the preparation process, is suitable for the construction of porous drainage pavement, and improves the viscosity and performance stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117965037B_ABST
    Figure CN117965037B_ABST
Patent Text Reader

Abstract

The present invention proposes a self-healing enhanced instant high-viscosity asphalt granule and a preparation method thereof, which belongs to the technical field of road engineering materials. The self-healing enhanced instant high-viscosity asphalt granule comprises the following raw material components by weight: 70-80 parts of matrix asphalt, 5-10 parts of hollow fibers containing polyurethane prepolymers and 25-50 parts of instant high-viscosity granules; wherein the mass ratio of the polyurethane prepolymer and the hollow fiber in the hollow fibers containing polyurethane prepolymers is 2: (1.8-2.1). Compared with the prior art, the self-healing enhanced instant high-viscosity asphalt granules prepared by the present invention can realize efficient self-repair and high-performance long-term service of high-viscosity asphalt, and have a simple and flexible use method, and also have the obvious advantage of avoiding secondary heating, and are suitable for porous drainage pavements with high viscosity and toughness requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of road engineering materials, and in particular relates to self-healing enhanced instant high-viscosity asphalt particles and a preparation method thereof. Background Art

[0002] High-viscosity asphalt is usually used as an important material for the construction and maintenance of high-performance pavements such as high-grade highways, large-void drainage and noise reduction asphalt pavements, and ultra-thin wear layers. During service, high-viscosity asphalt will gradually lose its bonding properties and cause cracks and looseness in the pavement, thereby affecting the safety of driving and the performance of the pavement. Traditional asphalt self-healing enhancement technology is mainly based on material supplementation and energy compensation. These methods only improve the flow and diffusion capacity of asphalt by supplementing asphalt components, and do not consider the repair of the degraded and broken polymer phase structure. On the other hand, waste rubber powder and recycled plastic are usually used to compositely modify the matrix asphalt to prepare a high-viscosity modified asphalt with controllable viscosity. For example, patent CN116554703A discloses a modified high-viscosity asphalt and a preparation method thereof, wherein the preparation method includes primary modification and secondary modification, wherein the primary modification includes the preparation of modified white carbon black, the preparation of modified epoxy resin and the mixing step, but the steps are relatively complicated, and the addition of too much adhesive will cause the asphalt to be gel-like, causing construction difficulties. Patent CN110643188A discloses a high-viscosity granular asphalt modifier and its preparation method and application, using ethylene-vinyl acetate (EVA) and acrylic adhesives as binders, which only improves the road performance and bonding strength of the modified asphalt, and has the problem of insufficient self-healing performance.

[0003] As for the self-healing properties of asphalt, the repair ability of asphalt itself is limited and takes a long time, which is not conducive to the long-term service of asphalt pavement. In recent years, many studies have shown that dynamic cross-linked network structures can improve the performance of polymer materials, so it is possible to consider introducing other chemical bonds to enhance its self-healing properties, but no patents have been found that use the reversible characteristics of dynamic chemical bonds to enhance the self-healing of modified asphalt. Therefore, it is urgent to study new methods for repairing asphalt concrete pavements. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a self-healing enhanced instant high-viscosity asphalt granule and a preparation method thereof.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] One of the technical solutions of the present invention:

[0007] A self-healing enhanced instant high-viscosity asphalt granule, comprising the following raw material components by weight: 70-80 parts of base asphalt, 5-10 parts of hollow fibers containing polyurethane prepolymer and 17-36 parts of instant high-viscosity granules;

[0008] Wherein, the mass ratio of the polyurethane prepolymer to the hollow fiber in the hollow fiber containing the polyurethane prepolymer is 2:(1.8-2.1).

[0009] Beneficial effects: The present invention innovatively proposes to introduce intermolecular hydrogen bonds and multiple reversible covalent bonds into high-viscosity asphalt, and proposes to use hollow fibers as carriers to protect the terminal isocyanate groups of the polyurethane prepolymer, and further fuse the above raw materials to prepare self-healing enhanced instant high-viscosity particles that can be directly used.

[0010] Preferably, the polyurethane prepolymer is a polyurethane prepolymer containing a dynamic disulfide bond and a polyurethane prepolymer containing a DA bond.

[0011] Furthermore, the polyurethane prepolymer containing dynamic disulfide bonds is prepared from diphenylmethane diisocyanate (MDI), polypropylene glycol (PPG) and 2,2-dithiodiethanol (HEDS) in a molar ratio of 1: (0.5-1): (1.2-2).

[0012] Furthermore, the specific preparation process of the polyurethane prepolymer containing dynamic disulfide bonds is as follows:

[0013] Diphenylmethane diisocyanate was dissolved in DMF in a four-necked round-bottom flask filled with nitrogen, and the temperature was raised to 50°C. After the solution was fully dissolved, polypropylene glycol was added, and then the temperature was adjusted to 75°C and stirred for 20 minutes to generate a polyurethane prepolymer containing -NCO end-capping; then 2,2-dithiodiethanol (HEDS) was added thereto to obtain a polyurethane prepolymer solution containing dynamic disulfide bonds.

[0014] Furthermore, the polyurethane prepolymer containing DA bonds is prepared from diphenylmethane diisocyanate (MDI), polypropylene glycol (PPG), furfurylamine (Fam) and bismaleimide (BMI) in a molar ratio of 1:(0.5-1):1.25:1.25.

[0015] Furthermore, the specific preparation process of the polyurethane prepolymer containing DA bonds is as follows:

[0016] The preparation process of the polyurethane prepolymer containing -NCO end-capping is the same as above. Furfurylamine (Fam) is added dropwise to the polyurethane prepolymer solution containing -NCO end-capping. After half an hour of ice water bath, the reaction temperature is restored to room temperature. The FT-IR is used to detect the concentration of 2270 cm -1 The disappearance of the characteristic peak of the -NCO group was used to determine the end point of the reaction, and a furan-terminated polyurethane prepolymer (MPF) was obtained. Bismaleimide (BMI) was then added, and the reaction was stirred at 60°C under nitrogen for 24 hours to obtain a polyurethane prepolymer solution containing DA bonds.

[0017] Preferably, the hollow fiber is a polyimide hollow fiber.

[0018] Furthermore, the preparation method of the polyimide hollow fiber refers to patent CN110404423A.

[0019] Furthermore, the polyurethane prepolymer encapsulation hollow fiber process refers to patent CN113731181A.

[0020] Preferably, the preparation step of the hollow fiber containing polyurethane prepolymer is: injecting the polyurethane prepolymer solution containing DA bonds and the polyurethane prepolymer solution containing dynamic disulfide bonds into the inner cavity of the hollow fiber respectively with a syringe to ensure sufficient coverage so that it can be effectively sealed.

[0021] Preferably, the fast-dissolving high-viscosity particles include graphene oxide and a high-viscosity particle binder.

[0022] Furthermore, the preparation process of the instant high-viscosity particles is as follows: the graphene oxide, desulfurized rubber powder, SBS, cosolvent, antioxidant, and C9 petroleum resin are added into a high-pressure tubular reactor via a compressor to carry out a polymerization reaction, and the obtained reaction product is separated by a high-pressure separator and a low-pressure separator to obtain the instant high-viscosity particles.

[0023] Furthermore, the temperature in the high-pressure tubular reactor is 210-230° C., and the absolute pressure is 160-170 MPa.

[0024] Furthermore, the cosolvent is composed of low molecular weight polyethylene wax and aromatic oil in a mass ratio of 2:1;

[0025] The antioxidant is composed of Irganox 168 and Irganox 1010 in a mass ratio of 2:1.

[0026] Preferably, the self-healing enhanced instant high-viscosity asphalt particles include the following components in parts by weight:

[0027] 70-80 parts of base asphalt, 5-10 parts of hollow fibers containing polyurethane prepolymer, 1-3 parts of graphene oxide, 5-10 parts of desulfurized rubber powder, 5-10 parts of SBS, 1-3 parts of C9 petroleum resin, 15-20 parts of cosolvent and 1-3 parts of antioxidant.

[0028] The second technical solution of the present invention:

[0029] A method for preparing self-healing enhanced instant high-viscosity asphalt particles comprises the following steps:

[0030] (1) Weigh the above raw material components according to their usage amounts for later use;

[0031] (2) Add the hollow fiber containing polyurethane prepolymer and the instant high-viscosity particles into the matrix asphalt, heat and stir evenly, then pour into a polytetrafluoroethylene (PTFE) mold, cool and wait for 2 hours to solidify, and obtain the self-healing enhanced instant high-viscosity asphalt particles.

[0032] Preferably, the heating and stirring temperature in step (2) is 180-190° C., the heating and stirring speed is 700 r / min, and the stirring time is 30 min.

[0033] The third technical solution of the present invention:

[0034] The application of the above self-healing enhanced quick-dissolving high-viscosity asphalt particles in porous drainage pavement.

[0035] Compared with the prior art, the present invention has the following advantages and technical effects:

[0036] (1) The present invention uses PI (polyimide) hollow fibers as carriers to seal and protect dynamically cross-linked polyurethane prepolymers, so as to prevent the terminal isocyanate group (-NCO) of the prepolymer from prematurely reacting with active hydrogen during the preparation and construction process, thereby causing the prepolymer to lose its activity. Under the action of damage cracks generated during the service of the pavement, the hollow fibers rupture and release internal active groups, which can react with aged and degraded polymers to repair the ruptured polymer network structure, thereby giving high-viscosity asphalt excellent long-term active self-healing ability.

[0037] (2) The present invention provides a method for preparing self-healing enhanced instant high-viscosity asphalt particles. The method can adopt a dry direct casting process to add hollow fibers containing polyurethane prepolymers and instant high-viscosity particles into a matrix asphalt to prepare self-healing enhanced instant high-viscosity asphalt particles. The method of use is simple and avoids the loss of chemical activity caused by secondary heating. The method has strong flexibility and is suitable for the construction of porous drainage pavements with high requirements for viscosity and toughness.

[0038] (3) The present invention adopts the method of adding graphene oxide to the self-healing enhanced instant high-viscosity asphalt particles. Graphene oxide contains hydrogen bonds, which can increase the intermolecular forces, promote the close arrangement of molecules, and enhance the viscosity and high and low temperature performance of high-viscosity asphalt. On the other hand, dynamic reversible covalent bonds are introduced into high-viscosity asphalt, and its reversible fracture-exchange reaction characteristics are utilized to promote the mutual entanglement of the polymer network in the high-viscosity asphalt, while constructing a dynamic reversible polyurethane cross-linking structure in the asphalt, so as to achieve efficient self-repair and high-performance long-term service of high-viscosity asphalt. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0040] Figure 1 This is a process flow chart of a self-healing enhanced instant high-viscosity asphalt granule preparation method disclosed in an embodiment of the present invention;

[0041] Figure 2 This is a comparison chart of the fluorescence microscopy results of the asphalt prepared in Example 1 of the present invention and Comparative Example 1;

[0042] Among them, (a) is a fluorescence micrograph of the self-healing enhanced instant high-viscosity asphalt particles prepared in Example 1, and (b) is a fluorescence micrograph of the asphalt prepared in Comparative Example 1. DETAILED DESCRIPTION

[0043] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0044] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0045] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0046] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0047] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0048] The present invention sets examples and comparative examples based on the control variable method to demonstrate the proposed beneficial effects. Comparative Example 1 is designed as ordinary modified asphalt. By comparing with the examples, it can be verified that the product of the present invention can enhance the self-healing performance of asphalt materials; in Comparative Example 2, only high-viscosity particle binder (desulfurized rubber powder, SBS, cosolvent, antioxidant, C9 petroleum resin) is added to verify the protective effect of the protective measures of the present invention on the hollow fibers and matrix asphalt containing polyurethane prepolymers in high-viscosity asphalt particles; the performance test results of Comparative Examples 3-4 and Comparative Example 1 show that the introduced hydrogen bonds, disulfide bonds and DA bonds can effectively enhance the performance of high-viscosity asphalt particles. In addition, through the indoor aging experiment in the laboratory, the performance differences of each sample before and after aging are tested to clarify the self-healing effect of different high-viscosity modified asphalts.

[0049] All raw materials used in the examples of the present invention are purchased from the market. Specifically:

[0050] 70# matrix asphalt was purchased from Taifu Asphalt Plant; 4.4-diphenylmethane diisocyanate (MDI) was purchased from Tianjin Damao Chemical Reagent Factory; polypropylene glycol was purchased from Beijing Inokai Technology Co., Ltd., N,N-dimethylformamide was purchased from Shanghai Myril Biochemical Technology Co., Ltd.; 2,2-dithiodiethanol (HEDS) was purchased from Hebei Yancheng Biotechnology Co., Ltd., furfural (Fam) was purchased from Shanghai Myril Biochemical Technology Co., Ltd., bismaleimide (BMI) was purchased from Beijing Inokai Technology Co., Ltd., and graphene oxide was purchased from Anhui Zesheng Technology Co., Ltd.; the cosolvent was made of low molecular weight polyethylene wax and aromatic oil according to quality. The ratio of 2:1 is 2:1, low molecular weight polyethylene wax was purchased from Shanghai Myrel Biochemical Technology Co., Ltd., aromatic oil was purchased from Shanghai McLean Biochemical Technology Co., Ltd.; desulfurized rubber powder was purchased from Beijing Hanlongda Technology Development Co., Ltd.; styrene block copolymer SBS / 5516 was purchased from Li Changrong Chemical (Fu Ju); C9 petroleum resin was purchased from Shenzhen Yoshida Chemical Co., Ltd.; antioxidant composed of Irganox168 and Irganox1010 in a mass ratio of 2:1, both purchased from Beijing Boning Biotechnology Co., Ltd.; catalyst dibutyltin dilaurate (DBTDD) was purchased from Shanghai Coklin Biochemical Technology Co., Ltd.

[0051] The technical solution of the present invention is further illustrated by the following embodiments.

[0052] Example 1

[0053] (a) preparing a hollow fiber containing a polyurethane prepolymer, comprising the following steps:

[0054] Step 1: Add 100 mL of DMF and 20 g of MDI into a four-necked round-bottom flask filled with nitrogen, and heat to 50° C. When diphenylmethane diisocyanate (MDI) is completely melted, add 80 g of PPG (Mn=2000), adjust the temperature to 75° C., and stir for 20 min to generate a polyurethane prepolymer containing -NCO end-capping; divide the generated polyurethane prepolymer into two equal parts;

[0055] Step 2: Add 2 g of dibutyltin dilaurate (DBTDL) to one of the portions, pass nitrogen under catalysis, stir and react at 75° C. for 40 min, then add 10 g of 2,2-dithiodiethanol (HEDS), and react under the same conditions until the hydroxyl group and -NCO in the system react completely to obtain a polyurethane prepolymer solution containing disulfide bonds;

[0056] Step 3: For another portion of polyurethane prepolymer, 5 g of FAm furfurylamine was added dropwise. After half an hour of ice-water bath, the reaction temperature was restored to room temperature. The FT-IR was used to detect the peaks at 2270 cm -1 The end point of the reaction was determined by the disappearance of the characteristic peak of the -NCO group, and a polyurethane prepolymer (MPF) solution containing furan end-capping was obtained; then bismaleimide (BMI) was added to MPF at a molar ratio of furan to maleimide of 1:1, and the reaction was stirred at 60°C under nitrogen for 24 hours. After cooling to room temperature, a polyurethane prepolymer solution containing DA bonds was obtained.

[0057] Step 4: Inject the prepared 25g of polyurethane prepolymer solution containing DA bonds and 25g of polyurethane prepolymer solution containing disulfide bonds into the inner cavity of 50g of polyimide hollow fiber respectively, ensuring sufficient coverage so that it can be effectively sealed.

[0058] (II) Preparation of fast-dissolving high-viscosity granules:

[0059] 1 g of graphene oxide, 20 g of cosolvent, 7.5 g of desulfurized rubber powder, 7.5 g of SBS, 1 g of antioxidant, and 2 g of C9 petroleum resin were added into a high-pressure tubular reactor via a compressor to carry out a polymerization reaction. The obtained reaction product was passed through a high-pressure separator and a low-pressure separator to obtain a polymerization product, wherein the temperature in the high-pressure separator was 220° C. and the absolute pressure was 165 MPa.

[0060] The cosolvent is composed of low molecular weight polyethylene wax and aromatic oil in a mass ratio of 2:1; the antioxidant is composed of Irganox 168 and Irganox 1010 in a mass ratio of 2:1.

[0061] (III) Preparing self-healing enhanced instant high-viscosity asphalt particles, comprising the following steps:

[0062] Weigh 25g of the instant high-viscosity particles prepared above, 7.5g of hollow fibers containing polyurethane prepolymer (containing dynamically cross-linked polyurethane prepolymer) and 75g of matrix asphalt, add them into a polytetrafluoroethylene (PTFE) mold, heat to 185°C, stir at 700r / min for 30min, cool and wait for 2h to solidify, and obtain self-healing enhanced high-viscosity asphalt particles, realize asphalt self-healing, and extend the service life of the road surface.

[0063] Example 2

[0064] The difference from Example 1 is that the weight proportions of raw materials used to prepare self-healing enhanced instant high-viscosity asphalt particles are different: 70 parts of base asphalt, 5 parts of hollow fibers containing polyurethane prepolymer, 1 part of graphene oxide, 5 parts of desulfurized rubber powder, 2 parts of SBS, 1 part of C9 petroleum resin, 15 parts of co-solvent and 1 part of antioxidant.

[0065] Other conditions are the same as in Example 1.

[0066] Example 3

[0067] The difference from Example 1 is that the weight proportions of raw materials used to prepare self-healing enhanced instant high-viscosity asphalt particles are different: 75 parts of base asphalt, 7 parts of hollow fibers containing polyurethane prepolymer, 2 parts of graphene oxide, 8 parts of desulfurized rubber powder, 8 parts of SBS, 2 parts of C9 petroleum resin, 18 parts of co-solvent and 3 parts of antioxidant.

[0068] Other conditions are the same as in Example 1.

[0069] Example 4

[0070] The difference from Example 1 is that the weight proportions of raw materials used to prepare self-healing enhanced instant high-viscosity asphalt particles are different: 80 parts of base asphalt, 10 parts of hollow fibers containing polyurethane prepolymer, 3 parts of graphene oxide, 10 parts of desulfurized rubber powder, 10 parts of SBS, 3 parts of C9 petroleum resin, 20 parts of co-solvent and 3 parts of antioxidant.

[0071] Other conditions are the same as in Example 1.

[0072] Comparative Example 1 (Ordinary High Viscosity Modified Asphalt)

[0073] 1) Preheat 100g of base asphalt to 180°C in an oven and soften it for later use. Weigh 7.5g of SBS according to the required mass for later use.

[0074] 2) Heat the base asphalt to 175°C, add 5g of aromatic oil to the base asphalt, add SBS to the hot asphalt in batches, stir for 2min each time, and use a shearing machine to shear at a low speed of 2000r / min for 20min; then increase the speed to 5000r / min and shear at a high speed for 1h;

[0075] 3) After high-speed shearing is completed, add 0.75% wt PPA (as a stabilizer to help form a dynamic cross-linking network, which needs to be melted in a water bath in advance) and high-speed shear at 5000r / min for 5 minutes; after the stabilizer shearing is completed, add 0.6% wt Evotherm3G and high-speed shear for 10 minutes.

[0076] 4) After the shearing is completed, the temperature is reduced to 175°C, and a four-blade mixer is used to stir at a low speed (600r / min) for 30 minutes to defoam. The mixture is taken out and placed in a 175°C oven to swell and develop for 30 minutes before being molded and packaged.

[0077] Comparative Example 2

[0078] The difference between Comparative Example 2 and Example 1 is that hollow fibers containing polyurethane prepolymer and graphene oxide are not added during the preparation of high-viscosity asphalt particles, and the rest is the same as Example 1.

[0079] Comparative Example 3

[0080] The difference between Comparative Example 3 and Example 1 is that the hollow fiber containing polyurethane prepolymer and the high-viscosity particle binder (including desulfurized rubber powder, SBS, cosolvent, antioxidant, C9 petroleum resin) are not added, and the rest is the same as Example 1.

[0081] Comparative Example 4

[0082] The difference between Comparative Example 4 and Example 1 is that no quick-dissolving high-viscosity particles (including graphene oxide, desulfurized rubber powder, SBS, co-solvent, antioxidant, C9 petroleum resin) are added, and the rest is the same as Example 1.

[0083] Performance test

[0084] To illustrate the beneficial effects of the present invention, the high-viscosity modified asphalt prepared in Example 1 and Comparative Examples 1-4 was tested for high-temperature rheological properties, fatigue resistance and self-healing properties before and after aging using a dynamic shear rheometer. All tests were performed in accordance with the Highway Asphalt Pavement Design Specification (JTG D50-2017). The aging test was performed according to the standard thin film oven (TFOT) aging test. Among them, the elastic recovery rate was obtained in the MSCR test at 64°C, the zero shear viscosity was measured in the ZSV at 60°C, the fatigue life was obtained in the LAS test at 20°C, and the self-healing index was tested by a 20°C linear amplitude sweep self-healing test to test the percentage of damage self-healing based on the damage variable index. The test results are shown in Table 1.

[0085] Table 1 Performance test results of high viscosity modified asphalt

[0086]

[0087] Conclusion: It can be seen from Table 1 that the self-healing enhanced instant high-viscosity asphalt particles prepared by the embodiment of the present invention are superior to those of Comparative Examples 1-4 in terms of high-temperature rheology, fatigue resistance and self-healing performance. It can be seen from Comparative Examples 1 and 2 that the high-viscosity particle binder prepared by the present invention can effectively improve the elastic recovery performance of asphalt, and is higher than that of ordinary high-viscosity modified asphalt; according to Example 1 and Comparative Example 3, it can be found that the addition of graphene oxide significantly improves the high-temperature deformation resistance and elastic deformation recovery of asphalt; according to Example 1 and Comparative Example 4, it can be seen that this is because dynamic reversible chemical bonds are introduced into the isocyanate prepolymer, and the hollow fiber is used to seal it to ensure the effect time. When the material is subjected to external force, the hollow fiber ruptures to release the internal core material, and the dynamic chemical bonds will undergo a reversible cleavage-exchange reaction before the main chain of the polymer modifier is destroyed, inducing the polymer network structure inside the material to achieve dynamic adjustment, thereby achieving a significant enhancement of the material toughness and giving the high-viscosity modified asphalt the ability to self-heal.

[0088] Figure 2 The fluorescence microscopy results of the self-healing enhanced instant high-viscosity asphalt prepared in Example 1 and the asphalt prepared in Comparative Example 1 are compared, wherein (a) is that of Example 1 and (b) is that of Comparative Example 1. Figure 2 The fluorescence microscopy results can more intuitively show the different substances and distribution in the prepared samples. Compared with ordinary high-viscosity asphalt, Example 1 forms a significant and uniform polymer cross-linked network, which shows that the high-viscosity modified particles prepared in the example have good compatibility with asphalt and achieve significant enhancement of material performance.

[0089] The above are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A self-healing enhanced instant high-viscosity asphalt granule, characterized in that: The raw material components include, by weight: 70-80 parts of base asphalt, 5-10 parts of hollow fibers containing polyurethane prepolymer, and 25-50 parts of quick-dissolving high-viscosity particles; Wherein, the mass ratio of the polyurethane prepolymer to the hollow fiber in the hollow fiber containing the polyurethane prepolymer is 2:(1.8-2.1); The hollow fiber is a polyimide hollow fiber; The polyurethane prepolymer is a polyurethane prepolymer containing a dynamic disulfide bond and a polyurethane prepolymer containing a DA bond; The fast-dissolving high-viscosity particles include graphene oxide and a high-viscosity particle binder.

2. The self-healing enhanced fast-dissolving high-viscosity asphalt granules according to claim 1, characterized in that: The polyurethane prepolymer containing dynamic disulfide bonds is prepared by reacting diphenylmethane diisocyanate, polypropylene glycol and 2,2-dithiodiethanol in a molar ratio of 1:(0.5-1):(1.2-2).

3. The self-healing enhanced instant high-viscosity asphalt granules according to claim 1, characterized in that: The polyurethane prepolymer containing DA bonds is prepared by reacting diphenylmethane diisocyanate, polypropylene glycol, furfurylamine and bismaleimide in a molar ratio of 1:(0.5-1):1.25:1.

25.

4. The self-healing enhanced instant high-viscosity asphalt granules according to claim 1, characterized in that: The high-viscosity particle binder consists of desulfurized rubber powder, SBS, C9 petroleum resin, co-solvent and antioxidant.

5. The self-healing enhanced instant high-viscosity asphalt granules according to claim 4, characterized in that: The raw materials include the following components in parts by weight: 70-80 parts of base asphalt, 5-10 parts of hollow fibers containing polyurethane prepolymer, 1-3 parts of graphene oxide, 5-10 parts of desulfurized rubber powder, 5-10 parts of SBS, 1-3 parts of C9 petroleum resin, 15-20 parts of cosolvent and 1-3 parts of antioxidant.

6. A method for preparing self-healing enhanced instant high-viscosity asphalt particles, characterized in that: The following steps are involved: (1) Weigh the amount of the raw material components according to any one of claims 1 to 5 for use; (2) Adding the hollow fiber containing the polyurethane prepolymer and the instant high-viscosity particles into the matrix asphalt, heating and stirring, cooling and solidifying, and obtaining the self-healing enhanced instant high-viscosity asphalt particles.

7. The method for preparing self-healing enhanced instant high-viscosity asphalt particles according to claim 6, characterized in that: The temperature of the heating and stirring in step (2) is 180-190° C., the speed of the heating and stirring is 700 r / min, and the stirring time is 30 min.