A highly asymmetric sponge-like polysulfone porous membrane and its preparation method
By introducing hydrophilic molecules and catalytically active groups onto the surface of polysulfone porous membranes and combining this with a solvent-free phase separation method to prepare asymmetric sponge-like membranes, the problems of easy membrane fouling and difficult catalyst bonding have been solved, enabling the application of highly efficient and long-life membrane materials.
Patent Information
- Application Number
- CN202211342948.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-31
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-10-31
AI Technical Summary
Existing organic porous membranes suffer from problems such as easy fouling, short service life, difficulty in effectively combining with catalysts, and low catalyst recovery rate.
A highly asymmetric sponge-like polysulfone porous membrane was prepared by introducing hydrophilic molecules and/or catalytically active groups on the membrane surface and using a non-solvent-induced phase separation-assisted reverse thermal phase separation method to form a pre-filtration zone and a separation zone of the porous membrane with a gradient change in pore size.
It improves the membrane's antifouling performance and lifespan, enhances catalyst recovery and catalytic efficiency, and maintains high-flux and high-efficiency filtration performance.
Smart Images

Figure CN117983076B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of porous separation membrane technology of polymers, and in particular to a highly asymmetric sponge-like polysulfone porous membrane and its preparation method. Background Technology
[0002] Membrane separation technology is widely used in environmental, chemical, food and biopharmaceutical, and microelectronic fields due to its advantages such as low energy consumption, convenient operation, no phase change, and high separation efficiency. Common methods for preparing organic porous membranes include stretching, thermally induced phase separation, and solvent-induced phase separation. Porous membranes can be classified into symmetrical and asymmetrical membranes according to their structure. Symmetrical membranes have pore sizes that are essentially uniform along their thickness direction, while asymmetrical membranes have pore sizes that are inconsistent along their thickness direction, typically referring to membranes with a gradient change in pore size along the thickness direction.
[0003] However, the problems of membrane fouling and short service life have become technical challenges restricting their large-scale application. For example, Chinese patent CN103055724B discloses a method for preparing polysulfone polymer microporous membranes by reverse thermal phase separation. This type of membrane has defects. First, the filter membrane does not have hydrophilic groups and is a hydrophobic membrane. It has a large filtration pressure difference and is easily fouled. In addition, the membrane is a homogeneous membrane with a small flux and dirt holding capacity.
[0004] Furthermore, membrane materials, as fundamental materials, have a wide range of applications. When catalytic removal of harmful substances is required, membrane filtration and catalysis are often separated. However, the catalyst recovery rate is another issue that needs to be addressed in this approach. Currently, some researchers are improving membrane materials by coating them during the membrane fabrication process. However, the adhesion between the catalyst and the membrane material is difficult to control. If the membrane material surface is completely covered by the catalyst, it will directly affect the filtration and separation performance of the membrane material itself. If only part of the membrane material surface is covered, the catalytic efficiency will be greatly reduced.
[0005] In view of this, it is necessary to improve the organic membrane materials in the existing technology to solve the technical problems such as easy fouling, short service life, difficulty in effectively combining with catalysts, and low catalyst recovery rate. Summary of the Invention
[0006] The objective of this invention is to disclose a polysulfone porous membrane with self-cleaning and anti-fouling properties. The membrane surface contains hydrophilic molecules and / or catalytically active groups, which can effectively solve the problem of porous membranes being easily fouled.
[0007] To achieve the above objectives, the present invention provides a highly asymmetric sponge-like polysulfone porous membrane. The porous membrane includes a pre-filtration zone and a separation zone. One side of the pre-filtration zone is a first outer surface, and one side of the separation zone is a second outer surface. The average pore size of the first outer surface is 0.1–4 μm, and the average pore size of the second outer surface is 0.03–1 μm. The cross-section of the porous membrane has non-directional tortuous channels, and the average pore size from the first outer surface to the second outer surface exhibits a continuous gradient change. The porous membrane has an asymmetry factor of 1.5–15, and hydrophilic molecules and / or catalytically active groups are distributed on the outer surface of the porous membrane.
[0008] In some embodiments, the pure water flux of the porous membrane is 1–300,000 L / m³. 2 The porous membrane has a tensile strength of 4-15 MPa and an elongation at break of 5%-35%, with a hydrophilic contact angle of 20° to 85°.
[0009] The second objective of this invention is to disclose a method for preparing a highly asymmetric sponge-like polysulfone porous membrane. The polysulfone porous membrane is prepared by a non-solvent-induced phase separation assisted by a reverse thermal phase separation method, which is convenient and simple.
[0010] To achieve the above objectives, the present invention provides a method for preparing a highly asymmetric sponge-like polysulfone porous membrane, comprising the following steps:
[0011] Step 1: Dissolve the additive in a mixture of solvent and non-solvent, then add polysulfone polymer to prepare a uniform casting solution, and let it stand to remove bubbles;
[0012] Step 2: Use a scraper or slit extruder to flow the casting liquid onto the carrier. In the preforming section, control the temperature and humidity on both sides of the liquid film to produce the initial film.
[0013] Step 3: Immerse the nascent membrane in the coagulation bath to solidify and shape;
[0014] Step 4: After washing, drying, and winding, the finished product is produced;
[0015] The casting solution contains 0%–20% additives, 5%–80% solvents, 10%–80% non-solvents, and 10%–30% polysulfone polymers.
[0016] The casting solution is stable and homogeneous below the critical phase separation temperature, and phase separation occurs above the critical phase separation temperature. The temperature in steps one and two is controlled below the critical phase separation temperature, and the temperature of the coagulation bath in step three is higher than the critical phase separation temperature in steps one and two.
[0017] In some embodiments, the additive is one or more of the following: a multifunctional nanomaterial or its sol, a porphyrin compound, a hydrophilic modified polysulfone polymer, or water.
[0018] In some embodiments, the multifunctional nanomaterial or its sol is one or more of ZnO, ZrO2, TiO2, Al2O3, MnO2-x, Au, Pd, Ag, Fe and their corresponding salts.
[0019] In some embodiments, the hydrophilic modified polysulfone polymer is one or more of the following: quaternized polyethersulfone, quaternized double type A polysulfone, quaternized polyphenylene sulfone, sulfonated polyethersulfone, sulfonated double type A polysulfone, sulfonated polyphenylene sulfone, hydroxylated polysulfone, hydroxylated polyphenylene sulfone, hydroxylated polyethersulfone, chlorinated polysulfone, chlorinated polyphenylene sulfone, and chlorinated polyethersulfone.
[0020] In some embodiments, the solvent is N,N-dimethylacetamide.
[0021] In some embodiments, the non-solvent is polyethylene glycol and diethylene glycol.
[0022] In some embodiments, in step one, the polysulfone polymer is one or more of polyethersulfone, polysulfone, and polyphenylsulfone.
[0023] In some embodiments, in step two, the carrier is one of the following: a glass plate, a continuously rotating annular polishing steel belt, a polishing drum, a non-woven fabric, and a release film.
[0024] In some embodiments, the temperature in steps one and two is controlled below the critical phase separation temperature, which is 15°C to 99°C.
[0025] In some embodiments, in step two, the temperature of the liquid film on the upper and lower surfaces of the preformed section is controlled separately, and the humidity of the surface in contact with air is controlled. The temperature is controlled within the range of 15℃ to 99℃, the relative humidity is controlled within the range of 45% to 95%, and the preforming time is 2s to 90s.
[0026] In some embodiments, in step three, the temperature of the coagulation bath is controlled between 16°C and 100°C, the coagulation bath is composed of 90% to 100% water and 0% to 10% N,N-dimethylacetamide, and the curing time is at least 20 seconds.
[0027] Compared with the prior art, the beneficial effects of the present invention are: (1) By adding hydrophilic additives to the casting solution, the surface properties of the membrane material are changed, its hydrophilicity is improved, and catalyst additives are added, combining catalytic technology and membrane separation technology. With the membrane material as the matrix, the catalyst penetrates into the membrane body. Due to the catalytic effect of the catalyst, the membrane material has richer functions, forming a multifunctional material with separation, antibacterial, degradation and self-cleaning properties, thereby improving the efficiency of pollution control, playing a role in mitigating membrane fouling to a certain extent, and extending the service life of the membrane material; (2) The porous membrane is integrally formed without composite process, and the process preparation is simple. Moreover, the polysulfone porous membrane is an asymmetric membrane with the pore size varying in the thickness direction, resembling a sponge. This ensures both high interception efficiency and high flux and antifouling properties. While ensuring high catalyst recovery rate, the catalytic activity is only slightly reduced; (3) The polysulfone filter membrane prepared by the present invention has good tensile strength and elongation at break, is suitable for various processing, has strong industrial applicability, and has high flux, fast and efficient filtration speed, and high economic benefits. Attached Figure Description
[0028] Figure 1 This is a scanning electron microscope image of a cross section of the highly asymmetric sponge-like polyethersulfone porous membrane shown in Example 1;
[0029] Figure 2 This is a scanning electron microscope image of the second outer surface of the highly asymmetric sponge-like polyethersulfone porous membrane shown in Example 1;
[0030] Figure 3 This is a scanning electron microscope image of the first outer surface of the highly asymmetric sponge-like polyethersulfone porous membrane shown in Example 1;
[0031] Figure 4 This is a scanning electron microscope image of a cross section of the homogeneous polyethersulfone porous membrane shown in Example 3;
[0032] Figure 5 This is a scanning electron microscope image of the second outer surface of the homogeneous polyethersulfone porous membrane shown in Example 3;
[0033] Figure 6 This is a scanning electron microscope image of the first outer surface of the homogeneous polyethersulfone porous membrane shown in Example 3. Detailed Implementation
[0034] The present invention will now be described in detail with reference to the embodiments shown in the accompanying drawings. However, it should be noted that these embodiments are not intended to limit the present invention. Equivalent changes or substitutions in function, method, or structure made by those skilled in the art based on these embodiments are all within the scope of protection of the present invention.
[0035] Example 1
[0036] like Figure 1-3 As shown, a method for preparing a highly asymmetric sponge-like polysulfone porous membrane includes the following steps:
[0037] Quaternized polyethersulfone, polyethersulfone resin (weight average molecular weight 62000), N,N-dimethylacetamide and polyethylene glycol 200 were selected in a mass ratio of 4:12:63:21.
[0038] Step 1: At 25℃, dissolve quaternized polyethersulfone in a mixture of N,N-dimethylacetamide and polyethylene glycol 200. Stir until completely dissolved, then add polyethersulfone resin and stir until the casting solution is clear and homogeneous. Let it stand for 3 hours to remove bubbles. Select a portion of the casting solution and measure the turbidity point, which is 61℃ (critical phase separation temperature). Keep the casting solution at 20℃.
[0039] Step 2: Use a scraper to cast the casting liquid onto the polishing drum for pre-forming. The casting thickness is 300 μm, and the drum temperature is 47°C. In the pre-forming section, the temperature and humidity of both sides of the liquid film are controlled to produce the initial film. In this embodiment, it is preferred that the side of the liquid film exposed to air is controlled by a constant temperature and humidity chamber with a temperature of 20°C and a humidity of 85%.
[0040] Step 3: Immerse the nascent membrane in a coagulation bath to solidify and shape it. In this embodiment, preferably, the liquid membrane is pre-shaped for 25 seconds and then further shaped in a coagulation tank at 70°C.
[0041] Step 4: After washing with pure water and / or ethanol, drying at 70°C, and finally rolling up to form the finished product.
[0042] The casting solution contains 0%–20% additives, 5%–80% polar solvents, 10%–80% non-polar solvents, and 10%–30% polysulfone polymers.
[0043] The polyethersulfone porous membrane prepared in this embodiment has an average pore size of 3.34 μm on the first outer surface, an average pore size of 0.33 μm on the second outer surface, a porosity of 86%, a median pore size of 0.29 μm measured by PMI, and a pure water flux of 25000 L / m³. 2 .h.bar, contact angle 58°, tensile strength 5.6MPa, elongation at break 30.2%.
[0044] (1) Endotoxin removal test of polyethersulfone porous membrane: Different endotoxins have relative molecular masses ranging from several thousand to tens of thousands. However, due to their amphiphilic nature, endotoxins can form associative compounds in water, with relative molecular masses reaching 400,000 to 1,000,000. Dead-end filtration was used. Endotoxin solutions prepared with purified water and deionized water were delivered at a constant flow rate using a peristaltic pump. The initial endotoxin concentration was 400 EU / mL. The solutions were passed through a porous membrane prepared with a mass of 34 mg. The endotoxin concentration of the permeate was sampled at regular intervals to analyze the endotoxin removal effect.
[0045] Results: For endotoxin solutions prepared with 1000ml of pure water, the endotoxin removal rate reached over 99.7%, after which the removal rate slowly decreased. Throughout the process, the pressure difference remained relatively constant at 0.01MPa. Therefore, the porous membrane did not experience clogging due to the trapping of particles and large aggregates. Removal was achieved solely through the affinity adsorption of endotoxins by positively charged quaternary ammonium groups. For endotoxin solutions prepared with 6000ml of deionized water, the total endotoxin removal rate reached over 98.5%, after which... When the membrane pressure difference becomes too large and reaches the upper pressure limit, it is no longer suitable for use. The pressure change indicates that during the treatment of endotoxin solutions prepared with deionized water, the porous membrane is gradually contaminated and clogged due to the trapping of particles, bacteria, or large aggregates. The reason why its treatment capacity is significantly greater than that of endotoxin solutions prepared with pure water and why it maintains a high endotoxin removal rate is that at this point, due to the blockage of membrane pores and the reduction in pore size, the membrane will rely on the sieving principle to trap endotoxin aggregates, so that the removal rate no longer decreases. In this process, both affinity adsorption and sieving mechanisms contribute to the removal of endotoxins.
[0046] (2) The polyethersulfone porous membrane was tested for bacterial challenge and its bacterial challenge level was ≥7log / cm2 (Brev.Dim.). The bacterial challenge test method was performed in accordance with YY / T0918.
[0047] Example 2
[0048] A method for preparing a highly asymmetric sponge-like polysulfone porous membrane includes the following steps:
[0049] A mixture of polyethersulfone resin (weight average molecular weight 62000), N,N-dimethylacetamide, and polyethylene glycol 200 in a mass ratio of 16:63:21 was selected.
[0050] Step 1: At 23℃, dissolve polyethersulfone resin in a mixture of N,N-dimethylacetamide and polyethylene glycol 200, stir until completely dissolved and the casting solution becomes clear and homogeneous, and let it stand for 3 hours to remove bubbles; select a portion of the casting solution and measure the turbidity point, which is 54℃ (critical phase separation temperature), and keep the casting solution at 20℃.
[0051] Step 2: Use a scraper to cast the casting liquid onto the polishing drum for pre-forming. The casting thickness is 300 μm, and the polishing drum temperature is 47°C. In the pre-forming section, the temperature and humidity of both sides of the liquid film are controlled to produce the initial film. In this embodiment, it is preferred that the side of the liquid film exposed to air is controlled by a constant temperature and humidity chamber with a temperature of 20°C and a humidity of 85%.
[0052] Step 3: Immerse the nascent membrane in a coagulation bath to solidify and shape it. In this embodiment, preferably, the liquid membrane is pre-shaped for 25 seconds and then further shaped in a coagulation tank at 70°C.
[0053] Step 4: After washing with pure water and / or ethanol, drying at 60°C, and finally rolling up to form the finished product.
[0054] The polyethersulfone porous membrane prepared in this embodiment has an average pore size of 2.81 μm on the first outer surface, an average pore size of 0.28 μm on the second outer surface, a porosity of 84%, a median pore size of 0.26 μm measured by PMI, and a pure water flux of 13000 L / m³. 2 .h.bar, contact angle 92°, tensile strength 5.5MPa, elongation at break 31.5%.
[0055] (1) Endotoxin removal test of polyethersulfone porous membrane: The results showed that the endotoxin removal rate of the endotoxin solution prepared with pure water was almost 0%; the total endotoxin removal rate of the endotoxin solution prepared with 4300ml of deionized water was only about 84.2%. After that, due to the excessive membrane pressure difference reaching the pressure limit, it was no longer suitable for use.
[0056] (2) The polyethersulfone porous membrane was tested for bacterial challenge and its bacterial challenge level was ≥7log / cm2 (Brev.Dim.). The bacterial challenge test method was performed in accordance with YY / T0918.
[0057] Example 3 (Comparative Example)
[0058] A method for preparing a homogeneous polysulfone porous membrane includes the following steps:
[0059] A mixture of polyethersulfone resin (weight average molecular weight 62000), N,N-dimethylacetamide, and polyethylene glycol 200 in a mass ratio of 16:63:21 was selected.
[0060] Step 1: At room temperature, dissolve polyethersulfone resin in a mixture of N,N-dimethylacetamide and polyethylene glycol 200, stir until the casting solution is clear and homogeneous, and let it stand for 3 hours to remove bubbles; select a portion of the casting solution and measure the turbidity point, which is 54℃ (critical phase separation temperature), and keep the casting solution at 20℃.
[0061] Step 2: Use a scraper to cast the film liquid onto the polishing drum for pre-forming. The casting thickness is 300 μm, and the drum temperature is 20°C. In the pre-forming section, the temperature and humidity of both sides of the liquid film are controlled to produce the initial film. In this embodiment, it is preferred that the side of the liquid film exposed to air is controlled by a constant temperature and humidity chamber with a temperature of 20°C and a humidity of 85%.
[0062] Step 3: Immerse the nascent membrane in a coagulation bath to solidify and shape it. In this embodiment, preferably, the liquid membrane is pre-shaped for 25 seconds and then further shaped in a coagulation tank at 70°C.
[0063] Step 4: After washing with pure water and / or ethanol, drying at 60°C, and finally rolling up to form the finished product.
[0064] The polyethersulfone porous membrane prepared in this embodiment has an average pore size of 0.29 μm on the first outer surface, an average pore size of 0.28 μm on the second outer surface, a porosity of 79%, a median pore size of 0.25 μm measured by PMI, and a pure water flux of 9800 L / m³. 2 .h.bar, contact angle 93°, tensile strength 6MPa, elongation at break 28.6%.
[0065] (1) Endotoxin removal test of polyethersulfone porous membrane: The results showed that the endotoxin removal rate of the endotoxin solution prepared with pure water was almost 0%; the total endotoxin removal rate of the endotoxin solution prepared with 3500ml of deionized water was only about 83.3%. After that, the membrane pressure difference was too large and reached the pressure limit, so it was not suitable for further use.
[0066] (2) The polyethersulfone porous membrane was tested for bacterial challenge and its bacterial challenge level was ≥7log / cm2 (Brev.Dim.). The bacterial challenge test method was performed in accordance with YY / T0918.
[0067] Table 1 Comparison of experimental data for polyethersulfone porous membranes prepared in Examples 1-3
[0068]
[0069] As can be seen from the comparison of Examples 1, 2 and 3, the asymmetric positively charged polyethersulfone porous membrane (Example 1) has significantly improved hydrophilicity, flux and dirt holding capacity compared to the asymmetric hydrophobic polyethersulfone porous membrane (Example 2) and the homogeneous polyethersulfone porous membrane (Example 3). At the same time, due to the charging effect, the endotoxin removal rate is also significantly improved. Compared with the traditional non-solvent-induced phase separation method, thermal phase separation method and stretching method, the reverse thermal phase separation method is simpler in process and has lower membrane production energy consumption, which meets the needs of practical development and application.
[0070] Example 4
[0071] A method for preparing a highly asymmetric sponge-like polysulfone porous membrane includes the following steps:
[0072] Fe(Ⅲ)-TiO2 visible light catalyst powder, polyethersulfone resin (weight average molecular weight 77000), N,N-dimethylacetamide and polyethylene glycol 300 were selected in a mass ratio of 1:18:11.7:70.3.
[0073] Step 1: Add Fe(Ⅲ)-TiO2 visible light catalyst powder to N,N-dimethylacetamide, disperse it evenly by ultrasonication, and then mix it with polyethersulfone resin and polyethylene glycol 300 to prepare casting solution. The ultrasonic temperature is controlled at 20℃ and stirred for 4-6 hours. After ultrasonic degassing for 1-2 hours, let it stand. Select a portion of the casting solution and measure the turbidity point, which is 74℃ (critical phase separation temperature). The casting solution is kept at 20℃.
[0074] Step 2: Use a scraper to cast the casting liquid onto a continuously rotating annular polishing steel belt for pre-forming. The casting thickness is 300 μm, and the temperature of the continuously rotating annular polishing steel belt is 50°C. In the pre-forming section, the temperature and humidity of both sides of the liquid film are controlled to produce the initial film. In this embodiment, it is preferred that the side of the liquid film exposed to air is controlled by a constant temperature and humidity chamber with a temperature of 20°C and a humidity of 80%.
[0075] Step 3: Immerse the nascent membrane in a coagulation bath to solidify and shape it. In this embodiment, preferably, the liquid membrane is pre-shaped for 15 seconds and then further shaped in a coagulation tank at 80°C.
[0076] Step 4: After washing with pure water and / or ethanol, drying at 80℃, and finally rolling up to form the finished product, a highly asymmetric sponge-like composite porous membrane of Fe(Ⅲ)-TiO2 / PES is obtained, which has both filtration and photocatalytic functions.
[0077] The polyethersulfone porous membrane prepared in this embodiment has an average pore size of 0.71 μm on the first outer surface, an average pore size of 0.075 μm on the second outer surface, a porosity of 80%, a median pore size of 0.065 μm measured by PMI, and a pure water flux of 2100 L / m³. 2 .h.bar, contact angle 64°, tensile strength 7.4MPa, elongation at break 18.5%.
[0078] The preparation method of the above Fe(Ⅲ)-TiO2 visible light catalyst powder is as follows: Weigh 0.5 g of P25-TiO2 and 0.0126 g of Fe(NO3)3·9H2O into a beaker, add 20 mL of deionized water to dissolve, and stir magnetically for 30 min. Transfer the stirred suspension to a microwave reactor, rinse the beaker with 10 mL of deionized water, and pour the rinsing solution into the reactor. The catalyst is synthesized by microwave hydrothermal method. The microwave hydrothermal method uses programmed temperature rise (120℃ for 5 min; 160℃ for 5 min; 190℃ for 3 min) to the set temperature of 190℃, and the reaction time is 90 min. The reacted material is centrifuged at 5000 r / min for 20 min, washed twice with deionized water and anhydrous ethanol, and then dried in a vacuum drying oven at 50℃ for 8 h. After grinding and sieving, Fe(Ⅲ)-TiO2 particles with uniformity are obtained.
[0079] (1) Photocatalytic performance test:
[0080] BPA (molecular formula C) 15 H 16 O2 (an endocrine disruptor) is commonly used in the production of polycarbonate plastics and epoxy resins used in many consumer products. As one of the world's most produced chemicals, it has acute toxicity in the range of 1-10 mg / L. If it dissolves or seeps into the ecological environment through waste, it will affect human and biological health. However, BPA can be decomposed through photocatalytic conversion to generate inorganic small molecules such as CO2 and H2O, and the products conform to the principles of green chemistry.
[0081] A 10 mg / L BPA solution was prepared as the target pollutant. 250 mL of solution was used for each degradation attempt. A 500W long-arc xenon lamp was used as the visible light source, and the experiment was conducted using a photocatalytic reactor. When testing catalyst performance, 0.2 g of Fe(Ⅲ)-TiO2 (catalyst concentration 0.8 g / L) was added. When testing membrane performance, a 2.2 g porous membrane (containing 0.2 g of catalyst) was cut and wrapped around the outside of a quartz cold trap, then immersed in the BPA solution to be degraded. The xenon lamp was inserted into the reactor cold trap, a rotor was added, and magnetic stirring was turned on. After a 30-minute dark reaction, the xenon lamp and condensate were turned on. The reaction time was 3 hours, with samples taken every 30 minutes. A clear, transparent solution was obtained by filtering with a disposable filter. The absorbance of the solution at different sampling times was measured using a UV-Vis spectrophotometer adjusted to 278 nm. The concentration and removal rate of BPA were calculated according to the standard curve formula.
[0082] In this embodiment, the asymmetric polyethersulfone porous membrane achieves a BPA removal rate of up to 85.3%, with a catalyst recovery rate of up to 99%.
[0083] (2) Filtration performance test: Prepare a bovine serum albumin (BSA) solution with a mass concentration of 100 mg / L and refrigerate overnight before use. Select a complete membrane and cut it into a circle. Place the cut membrane in the ultrafiltration device and tighten the screw. Add 400 mL of BSA solution to a beaker, pre-pressurize at 0.1 MPa for 30 min, and measure 10 mL of the outflowing BSA solution. Measure the absorbance of the BSA solution before and after filtration using a UV-Vis spectrophotometer at 278.5 nm. Calculate the rejection rate according to the standard curve and formula.
[0084] The asymmetric polyethersulfone porous membrane of this embodiment has a BSA rejection rate of up to 95%.
[0085] Example 5 (Comparative Example)
[0086] A method for preparing a highly asymmetric sponge-like polysulfone porous membrane includes the following steps:
[0087] Polyethersulfone resin (weight average molecular weight 77,000), N,N-dimethylacetamide, and polyethylene glycol 300 were selected in a mass ratio of 18:11.7:70.3.
[0088] Step 1: Add polyethersulfone resin to a mixed solution of N,N-dimethylacetamide and polyethylene glycol 300, mix and ultrasonically disperse to obtain a casting solution. The ultrasonic temperature is controlled at 20℃ and stirred for 4-6 hours. After ultrasonic degassing for 1-2 hours, let it stand. After degassing, select a portion of the casting solution and measure the turbidity point, which is 69℃ (critical phase separation temperature). The casting solution is kept at 20℃.
[0089] Step 2: Use a scraper to cast the casting liquid onto a continuously rotating annular polishing steel belt for pre-forming. The casting thickness is 300 μm, and the temperature of the continuously rotating annular polishing steel belt is 50°C. In the pre-forming section, the temperature and humidity of both sides of the liquid film are controlled to produce the initial film. In this embodiment, it is preferred that the side of the liquid film exposed to air is controlled by a constant temperature and humidity chamber with a temperature of 20°C and a humidity of 80%.
[0090] Step 3: Immerse the nascent membrane in a coagulation bath to solidify and shape it. In this embodiment, preferably, the liquid membrane is pre-shaped for 15 seconds and then further shaped in a coagulation tank at 80°C.
[0091] Step 4: After washing with pure water and / or ethanol, drying at 80°C, and finally rolling up to form the finished product, a highly asymmetric sponge-like composite porous membrane is obtained.
[0092] The polyethersulfone porous membrane prepared in this embodiment has an average pore size of 0.62 μm on the first outer surface, an average pore size of 0.066 μm on the second outer surface, a porosity of 76%, a median pore size of 0.06 μm measured by PMI, and a pure water flux of 1400 L / m³. 2.h.bar, contact angle 92°, tensile strength 7.1MPa, elongation at break 19.3%
[0093] (1) Photocatalytic performance test: The asymmetric polyethersulfone porous membrane in this embodiment has a BPA removal rate of only 53.8%.
[0094] (2) Filtration performance test: The asymmetric polyethersulfone porous membrane of this embodiment can achieve a BSA rejection rate of up to 96%.
[0095] Table 2 Comparison of experimental data for polyethersulfone porous membranes prepared in Examples 4-5
[0096]
[0097] It is evident that the BPA removal rate of pure catalyst Fe(III)-TiO2 is higher than that of Fe(III)-TiO2 / PES. This is because some of the Fe(III)-TiO2 catalyst in the Fe(III)-TiO2 / PES membrane cannot catalyze the decomposition of BPA within the membrane pores. In contrast, the pure PES membrane still exhibits some BPA removal efficiency, primarily due to the electrostatic adsorption effect of the membrane pores. The photocatalytic reaction of pure catalyst Fe(III)-TiO2 involves directly adding the catalyst to the reaction solution, resulting in a low catalyst yield of only 84%. However, when using the composite Fe(III)-TiO2 / PES, the catalyst is almost entirely preserved throughout the photocatalytic process due to the anchoring effect of the PES membrane on the Fe(III)-TiO2, achieving a recovery rate exceeding 99%. Furthermore, recovery is simple; the membrane can be directly removed from the reaction solution. After adding Fe(Ⅲ)-TiO2, the rejection rate of the composite porous membrane did not change significantly compared with the pure membrane, remaining at around 85%, indicating that the addition of Fe(Ⅲ)-TiO2 did not significantly change the membrane pore size; however, the pure water flux of Fe(Ⅲ)-TiO2 / PES was significantly greater than that of the pure PES membrane, indicating that the hydrophilic modification of the PES membrane by Fe(Ⅲ)-TiO2 had a significant effect on increasing the flux.
[0098] Example 6
[0099] A method for preparing a highly asymmetric sponge-like polysulfone porous membrane includes the following steps:
[0100] Nano ZnO powder, polysulfone resin (PSF), N,N-dimethylacetamide, and polyethylene glycol 600 were selected in a mass ratio of 2:18:31.5:50.5.
[0101] Step 1: Add nano ZnO powder to N,N-dimethylacetamide, disperse it evenly by ultrasonication, and then mix it with polysulfone resin (PSF) and polyethylene glycol 600 to prepare a casting solution. The ultrasonic temperature is controlled at 18℃ and stirred for 4-6 hours. After ultrasonic degassing for 1-2 hours, it is allowed to stand. A portion of the casting solution is selected and the turbidity point is measured to be 64℃ (critical phase separation temperature). The casting solution is kept at 18℃.
[0102] Step 2: Use a scraper to cast the casting liquid onto a glass plate for preforming. The casting thickness is 300 μm, and the glass plate temperature is 45°C. In the preforming section, the temperature and humidity of both sides of the liquid film are controlled to produce the initial film. In this embodiment, the side of the liquid film exposed to air is preferably controlled by a constant temperature and humidity chamber with a temperature of 18°C and a humidity of 80%.
[0103] Step 3: Immerse the nascent membrane in a coagulation bath to solidify and shape it. In this embodiment, preferably, the liquid membrane is pre-shaped for 7 seconds and then further shaped in a coagulation tank at 70°C.
[0104] Step 4: After washing with pure water and / or ethanol, drying at 70°C, and finally winding up to form the finished product, a ZnO / PSF highly asymmetric gradient sponge-like composite porous membrane is obtained.
[0105] The polysulfone porous membrane prepared in this embodiment has an average pore size of 0.35 μm on the first outer surface, an average pore size of 0.054 μm on the second outer surface, a porosity of 78%, a median pore size of 0.048 μm measured by PMI, and a pure water flux of 500 L / m³. 2 .h.bar, contact angle 69°, tensile strength 6.6MPa, elongation at break 22.7%.
[0106] The above-mentioned method for preparing nano-ZnO powder is as follows: Nano-zinc oxide (ZnO) is prepared by the sol-gel method. Zinc acetate (135 mg) is used as a precursor and dissolved in 250 mL of distilled water. Ammonia solution (50% v / v) is added to the above solution, and the mixture is stirred continuously until the pH of the solution reaches 8.5. The reaction mixture is stored at room temperature until a gel is formed. The gel is washed with 0.1 M ammonium nitrate solution, filtered, dried in an oven at 90 °C, and finally calcined in a muffle furnace at 400 °C for 5 h to obtain nano-ZnO.
[0107] (1) Photocatalytic degradation performance test:
[0108] Textile industry wastewater, classified as organic pollutant, pollutes water sources worldwide, posing a serious environmental problem. Reactive dyes are among the most important and commonly used dyes in textile products. During the dyeing process, approximately 10-15% of the dye is released into the environment, resulting in wastewater with a bright but unattractive color. Traditional treatment methods, such as biological treatment, adsorption, and coagulation, have been used to treat dyes, but these methods generate secondary pollution. Therefore, rapid non-selective oxidation technology based on advanced oxidation processes (AOP) for organic dyes has been widely applied to the treatment of dyes (Reactive Red 11 is a common example). Solar-powered heterogeneous photocatalytic oxidation technology, developed in the 1970s, is a novel AOP technology that has attracted significant attention. These processes generate hydroxyl radicals (HO radicals) when a photocatalyst absorbs light radiation upon contact with water and oxygen. - ) and superoxide anion (O2) - )conduct.
[0109] The prepared ZnO / PSF membrane (9.1 g) and 90 mL of the prepared Reactive Red 11 dye solution (100 mg / L) were placed in a Bukner funnel and kept under sunlight for different time intervals (10–60 min). 0.1 g of ZnO was added when testing the catalyst performance. After the photocatalytic reaction, the filtrate was collected using a suction pump, and samples were taken at different time intervals to analyze the dye concentration. Using a UV-Vis spectrophotometer adjusted to an absorption wavelength of 555 nm, the absorbance of the solution at different sampling times was measured, and the concentration of Reactive Red 11 in the sample was calculated according to the standard curve formula.
[0110] In this embodiment, the asymmetric polysulfone porous membrane achieves a removal rate of 96.5% for Active Red 11 and a catalyst recovery rate of 98%.
[0111] Example 7 (Comparative Example)
[0112] A method for preparing a highly asymmetric sponge-like polysulfone porous membrane includes the following steps:
[0113] Polysulfone resin (PSF), N,N-dimethylacetamide, and polyethylene glycol 600 were selected in a mass ratio of 18:31.5:50.5.
[0114] Step 1: Add polysulfone resin (PSF) to a mixed solution of N,N-dimethylacetamide and polyethylene glycol 600, and disperse it evenly by ultrasonication to obtain a casting solution. The ultrasonic temperature is controlled at 18℃ and stirred for 4-6 hours. After ultrasonic degassing for 1-2 hours, let it stand. After degassing, select a portion of the casting solution and measure the turbidity point, which is 61℃ (critical phase separation temperature). The casting solution is kept at 18℃.
[0115] Step 2: Use a scraper to cast the casting liquid onto a glass plate for preforming. The casting thickness is 300 μm, and the glass plate temperature is 45°C. In the preforming section, the temperature and humidity of both sides of the liquid film are controlled to produce the initial film. In this embodiment, the side of the liquid film exposed to air is preferably controlled by a constant temperature and humidity chamber with a temperature of 18°C and a humidity of 80%.
[0116] Step 3: Immerse the nascent membrane in a coagulation bath to solidify and shape it. In this embodiment, preferably, the liquid membrane is pre-shaped for 7 seconds and then further shaped in a coagulation tank at 70°C.
[0117] Step 4: After washing with pure water and / or ethanol, drying at 70°C, and finally winding up to form the finished product, a highly asymmetric gradient sponge-like polysulfone porous membrane is obtained.
[0118] The polysulfone porous membrane prepared in this embodiment has an average pore size of 0.31 μm on the first outer surface, an average pore size of 0.051 μm on the second outer surface, a porosity of 75%, a median pore size of 0.045 μm measured by PMI, and a pure water flux of 320 L / m³. 2 .h.bar, contact angle 94°, tensile strength 6.3MPa, elongation at break 25.3%.
[0119] (1) Photocatalytic degradation performance test:
[0120] In this embodiment, the asymmetric polysulfone porous membrane has a removal rate of only 38.6% for Active Red 11.
[0121] Table 3 Comparison of experimental data for polysulfone porous membranes prepared in Examples 6-7
[0122]
[0123] It is evident that the removal rate of Reactive Red 11 by pure ZnO catalyst is slightly higher than that of ZnO / PSF (and also by polysulfone porous membranes with nano-zinc oxide). This is because some of the ZnO catalyst in the hybrid PSF membrane cannot exert its catalytic effect within the membrane pores, while the pure PSF membrane still has a certain removal effect on Reactive Red 11, mainly relying on the electrostatic adsorption of the membrane pores. The photocatalytic reaction of pure ZnO catalyst material involves directly adding the catalyst to the dye solution, resulting in a low catalyst yield of only 80%. However, in the catalyst hybrid PSF membrane, due to the anchoring effect of the PSF membrane on ZnO, the catalyst is almost not lost throughout the entire photocatalytic process, and the recovery rate can reach over 98%. After adding ZnO, the pore size of the composite porous membrane ZnO / PSF did not change significantly compared with the pure PSF membrane, indicating that the addition of ZnO did not significantly change the membrane pore size. However, the pure water flux of ZnO / PSF was significantly greater than that of the pure PSF membrane, indicating that the hydrophilic modification of the PSF membrane by ZnO had a significant effect on increasing the flux.
[0124] Table 4. Pore sizes of polysulfone porous membranes prepared in Examples 1-7
[0125]
[0126] As can be seen from Table 4 and Figure 1-3 It can be seen that the polysulfone porous membranes prepared in Examples 1-7 of the present invention (excluding Example 3) all have ideal membrane structures. The porous membranes are integrally formed without composite processes, and the preparation process is simple. Moreover, the polysulfone porous membrane is an asymmetric membrane with a gradient change in pore size in the thickness direction, exhibiting a sponge-like structure. This ensures both high interception efficiency and high flux and antifouling properties. While ensuring a high catalyst recovery rate, the catalytic activity is only slightly reduced.
[0127] Table 5. Basic properties of polysulfone porous membranes prepared in Examples 1-7
[0128]
[0129] As can be seen from Table 5, the polysulfone filter membranes prepared in Examples 1-7 have good tensile strength and elongation at break, are suitable for various processing, have strong industrial applicability, and also have high throughput, fast and efficient filtration speed, and high economic benefits.
[0130] The detailed descriptions listed above are merely specific descriptions of feasible embodiments of the present invention, and are not intended to limit the scope of protection of the present invention. All equivalent embodiments or modifications made without departing from the spirit of the present invention should be included within the scope of protection of the present invention.
[0131] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A method for preparing a highly asymmetric sponge-like polysulfone porous membrane, characterized in that, Includes the following steps: Step 1: Dissolve the additive in a mixture of solvent and non-solvent, then add polysulfone polymer to prepare a uniform casting solution, and let it stand to remove bubbles; Step 2: Use a scraper or slit extruder to extend the casting liquid onto the carrier. In the preforming section, control the temperature and humidity on both sides of the liquid film to make the temperature and humidity on both sides of the liquid film different, so as to generate the initial film. Step 3: Immerse the nascent membrane in the coagulation bath to solidify and shape; Step 4: After washing, drying, and winding, the finished product is produced; The casting solution contains 0%–20% additives, 5%–80% solvents, 10%–80% non-solvents, and 10%–30% polysulfone polymers. The casting solution is stable and homogeneous below the critical phase separation temperature, and phase separation occurs above the critical phase separation temperature. The temperature in steps one and two is controlled below the critical phase separation temperature, and the temperature of the coagulation bath in step three is higher than the critical phase separation temperature in steps one and two.
2. The method for preparing a highly asymmetric sponge-like polysulfone porous membrane according to claim 1, characterized in that, The additive is one or more of the following: multifunctional nanomaterials or their sols, porphyrin compounds, hydrophilic modified polysulfone polymers, or water.
3. The method for preparing a highly asymmetric sponge-like polysulfone porous membrane according to claim 2, characterized in that, The multifunctional nanomaterial or its sol is one or more of ZnO, ZrO2, TiO2, Al2O3, MnO2-x, Au, Pd, Ag, Fe and their corresponding salts.
4. The method for preparing a highly asymmetric sponge-like polysulfone porous membrane according to claim 2, characterized in that, The hydrophilic modified polysulfone polymer is one or more of the following: quaternized polyethersulfone, quaternized polyphenylsulfone, sulfonated polyethersulfone, sulfonated polyphenylsulfone, hydroxylated polysulfone, hydroxylated polyphenylsulfone, hydroxylated polyethersulfone, chlorinated polysulfone, chlorinated polyphenylsulfone, and chlorinated polyethersulfone.
5. The method for preparing a highly asymmetric sponge-like polysulfone porous membrane according to claim 2, characterized in that, The solvent is N,N-dimethylacetamide.
6. The method for preparing a highly asymmetric sponge-like polysulfone porous membrane according to claim 2, characterized in that, The non-solvents are polyethylene glycol and diethylene glycol.
7. The method for preparing a highly asymmetric sponge-like polysulfone porous membrane according to claim 1, characterized in that, In step one, the polysulfone polymer is one or more of polyethersulfone, polysulfone, and polyphenylsulfone.
8. The method for preparing a highly asymmetric sponge-like polysulfone porous membrane according to claim 1, characterized in that, In step two, the carrier is one of the following: a glass plate, a continuously rotating annular polishing steel belt, a polishing drum, non-woven fabric, and a release film.
9. The method for preparing a highly asymmetric sponge-like polysulfone porous membrane according to claim 1, characterized in that, In steps one and two, the temperature is controlled below the critical phase separation temperature, which is 15℃ to 99℃.
10. The method for preparing a highly asymmetric sponge-like polysulfone porous membrane according to claim 9, characterized in that, In step two, the liquid film of the preformed section is individually temperature-controlled on both the upper and lower surfaces, and the humidity is controlled on the surface in contact with air. The temperature is controlled within the range of 15℃ to 99℃, the relative humidity is controlled within the range of 45% to 95%, and the preformation time is 2s to 90s.
11. The method for preparing a highly asymmetric sponge-like polysulfone porous membrane according to claim 10, characterized in that, In step three, the temperature of the coagulation bath is controlled between 16°C and 100°C. The coagulation bath consists of 90% to 100% water and 0% to 10% N,N-dimethylacetamide. The curing time is at least 20 seconds.
Citation Information
Patent Citations
Method for preparing polysulfones polymer microporous membrane by counter-current thermally induced phase separation method
CN103055724B
Asymmetric PES filter membrane for removing viruses, and preparation method thereof
CN113842792A