A method for extracting precious metals by integrating thiosulfate electrochemical leaching and recovery into a short process

The anodic oxidation leaching and cathodic reduction of precious metals are realized in the electrolyte through the thiosulfate electrochemical method. The integrated short-process extraction solves the problems of complex wet precious metal leaching process, long cycle and low efficiency, and achieves high efficiency. , low energy consumption precious metal extraction.

CN118007193BActive Publication Date: 2024-10-18WUHAN UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410050518.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-12
Publication Date
2024-10-18
Estimated Expiration
2044-01-12

AI Technical Summary

Technical Problem

The existing wet precious metal leaching process is complex, has long extraction cycle, low efficiency and high cost.

Method used

The short process method of thiosulfate electrochemical leaching and recovery is adopted. The thiosulfate, electrolyte and alkali solution in the electrolyte are electrolyzed in the electrolytic tank, so that the precious metals are oxidized and leached at the anode and deposited at the cathode. Anodic oxidation and cathodic reduction are carried out simultaneously, the voltage is controlled at 0.1-3V, and the pH is adjusted at 7-13.

Benefits of technology

It achieves efficient green one-step extraction of precious metals, shortens the extraction time, has a gold leaching rate of 100%, and a recovery rate of 99.8%. It also simplifies the process steps and has the advantages of high efficiency, low energy consumption, and no pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118007193B_ABST
    Figure CN118007193B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for extracting precious metals by an integrated short process of thiosulfate electrochemical leaching and recovery, including: adding alkali solution after dissolving thiosulfate and electrolyte, and stirring to obtain an electrolyte; the electrolyte is a salt that does not contain thiosulfate; the pH of the electrolyte is adjusted to 7-13, and then the electrolyte and the material containing precious metals are placed in an electrolytic cell, and an electrode system provided in the electrolytic cell is used for electrolytic operation, so that the precious metals are leached at the anode and deposited at the cathode; the voltage of the electrolytic operation is 0.1-3V; and the precious metal element deposited on the cathode is collected. The present invention can simultaneously realize anode precious metal leaching and cathode precious metal ion electrolytic deposition in a reaction device, realizes the integrated extraction of precious metals while leaching and recovering, and has the advantages of high extraction efficiency, short process flow, low reagent consumption, low energy consumption, and no pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrometallurgy, and specifically relates to a method for extracting precious metals by integrating thiosulfate electrochemical leaching and recovery in a short process. Background Art

[0002] Precious metals are strategic mineral resources that guarantee national economic and financial security. Currently, there are two main refining methods: pyrometallurgy and hydrometallurgy. Wet leaching has been widely studied due to its advantages of low carbon, environmental protection, and low energy consumption. Its leaching reaction is essentially a redox reaction, that is, the precious metal loses electrons and is oxidized to precious metal ions and enters the solution, and then the enriched precious metal ions gain electrons and are reduced to single substances for recovery. The current wet leaching process is: leaching precious metal-containing materials with leaching agents such as cyanide, thiosulfate or thiourea, then adsorbing the precious metal coordination ions in the leaching solution with activated carbon or resin, and then desorbing the gold-loaded carbon or resin to obtain precious liquid, and finally reducing the precious metal coordination ions in the precious liquid by displacement or electrolysis to obtain precious metal single substances. In the existing process, the oxidation leaching of precious metal materials and the reduction recovery of precious metal coordination ions are independent of each other, and the entire wet leaching process is complicated, resulting in problems such as long precious metal leaching cycle, low efficiency, and high cost. Summary of the invention

[0003] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for extracting precious metals by integrating thiosulfate electrochemical leaching and recovery in a short process, so as to solve the problems of complex process flow, long extraction cycle, low efficiency and high cost of current precious metal wet leaching.

[0004] To achieve the above object, the present invention is implemented through the following technical solutions:

[0005] A method for extracting precious metals by integrating thiosulfate electrochemical leaching and recovery into a short process, comprising the following steps:

[0006] S1: dissolving thiosulfate and electrolyte, adding alkali solution, and stirring evenly to obtain an electrolyte; the electrolyte is a salt that does not contain thiosulfate;

[0007] S2: adjusting the pH of the electrolyte to 7-13, then placing the electrolyte and the material containing the precious metal in an electrolytic cell, and performing electrolysis using an electrode system in the electrolytic cell, so that the precious metal is leached at the anode and deposited at the cathode; the voltage of the electrolytic operation is 0.1-3V;

[0008] S3: Collect the precious metal element deposited on the cathode.

[0009] Preferably, the concentration of thiosulfate in the electrolyte is 0.1-0.5M, the concentration of electrolyte is 0.1-0.5M, and the concentration of alkali solution is 0.3-1.5M.

[0010] Preferably, the concentration of thiosulfate in the electrolyte is 0.2-0.3M, and the concentration of electrolyte is 0.3-0.4M.

[0011] Preferably, in step S2, the pH of the electrolyte is adjusted to 10-11.

[0012] Preferably, the thiosulfate is one or more of sodium thiosulfate, ammonium thiosulfate, and potassium thiosulfate; and the alkali solution is one or more of ammonia water, sodium hydroxide, and potassium hydroxide.

[0013] Preferably, the electrolyte is one or two of chloride, sulfate and carbonate.

[0014] Preferably, the material containing precious metals is pure gold flakes, silver flakes or waste circuit boards.

[0015] Preferably, the cathode of the electrolysis system is a titanium plate or a copper plate, and the anode is one of platinum, titanium, copper, lead, glassy carbon, silicon carbide, stainless steel, graphite electrode, and graphite felt.

[0016] Preferably, a diaphragm is provided in the electrolytic cell, and the diaphragm divides the electrolytic cell into a cathode chamber and an anode chamber.

[0017] Preferably, the diaphragm is an acid- and alkali-resistant filter cloth or nylon mesh with a mesh size of 600-800.

[0018] The beneficial effects of the present invention are:

[0019] 1. The present invention realizes the integrated short-process extraction of precious metals by thiosulfate electrochemical leaching and recovery, that is, the cathode is reduced while the anodic oxidation leaching occurs. Within 24 hours, the leaching rate of gold is 100% and the recovery rate is 99.8%;

[0020] 2. The present invention greatly shortens the extraction time. Compared with the traditional extraction process, the extraction time of precious metals is shortened from 65h to 24h;

[0021] 3. The present invention simplifies the precious metal extraction process steps, has the advantages of high efficiency, low energy consumption, short flow path, and no pollution, and can achieve efficient and green one-step extraction of precious metals. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the process of extracting precious metals by traditional technology;

[0023] Figure 2 Schematic diagram of the electrochemical leaching-recovery integrated precious metal extraction process of the present invention;

[0024] Figure 3 This is a diagram showing the effect of extracting precious metals in one step by leaching and recovering in Example 1;

[0025] Figure 4 This is a diagram showing the effect of extracting gold from PCBs by integrated leaching and recovery in Example 2;

[0026] Figure 5 Is different S2O3 2- The effect of concentration on the integrated extraction of gold from PCBs by leaching and recovery;

[0027] Figure 6 This is a diagram showing the integrated extraction effect of leaching and recovery of gold from PCBs at different KCl concentrations;

[0028] Figure 7 This is a diagram showing the effects of different initial pH on the integrated leaching-recovery of gold in PCBs. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] like Figure 1 As shown, when copper ammonia-thiosulfate is used to leach gold, the leaching liquid after solid-liquid separation needs to be recycled through processes such as adsorption, desorption and reduction to recover precious metals. The traditional process has problems such as low efficiency, high reagent consumption, high cost and long time consumption.

[0031] Based on this, the present invention creatively proposes a method for extracting precious metals by integrating electrochemical leaching and recovery of thiosulfate in a short process, which dissolves precious metals by electrochemical anode oxidation at a low voltage, and effectively combines the cathode for reduction and recovery of the leachate, and can simultaneously realize the integrated reaction of anode mineral metal leaching and cathode leachate electrolytic deposition in one reaction device, achieving an integrated extraction effect of leaching and recovery, with the advantages of high extraction efficiency, short process flow, low reagent consumption, low energy consumption, and no pollution, making the metal extraction process safer and more cost-effective. Specifically, the method for extracting precious metals by integrating electrochemical leaching and recovery of thiosulfate provided by the present invention, such as Figure 2 As shown, the following steps are included:

[0032] S1: preparing electrolyte: dissolving thiosulfate and chloride, adding alkali solution, stirring evenly to obtain electrolyte; the concentration of thiosulfate in the electrolyte is 0.1-0.5M, preferably 0.2-0.3M; the concentration of electrolyte is 0.1-0.5M, preferably 0.3-0.4M; the concentration of alkali solution is 0.3-1.5M. The type of thiosulfate is not limited, and it can be one or more of sodium thiosulfate, ammonium thiosulfate, and potassium thiosulfate; the type of alkali solution is not limited, including but not limited to one or more of ammonia water, sodium hydroxide, and potassium hydroxide; the electrolyte is a salt that does not contain thiosulfate, for example, it can be one or two of chloride, sulfate, and carbonate.

[0033] S2: Adjust the pH of the electrolyte to 7-13, preferably 10-11; then place the electrolyte and the material containing precious metals in an electrolytic cell, and use the electrode system provided in the electrolytic cell to perform electrolysis operation, so that the precious metals are leached at the anode and deposited at the cathode; the voltage of the electrolysis operation is 0.1-3V; the material containing precious metals can be pure gold sheets, silver sheets or discarded circuit boards. The cathode of the electrolysis system is a metal electrode with good conductivity such as a titanium plate or a copper plate, which needs to be polished and put into use, and the anode is an electrode material with good conductivity such as platinum, titanium, copper, lead, glassy carbon, silicon carbide, stainless steel, graphite electrode and graphite felt. Preferably, a diaphragm is provided in the electrolytic cell, which divides the electrolytic cell into a cathode chamber and an anode chamber. The diaphragm can be a 600-800 mesh acid and alkali resistant filter cloth or nylon mesh to prevent solid minerals or impurities in the anode chamber from entering the cathode.

[0034] S3: Collect the precious metal element deposited on the cathode.

[0035] The present invention is a novel thiosulfate electrochemical oxidation system (S2O3 2- - electrolyte - alkali solution) can realize the reduction of cathode metal ions while anodic oxidation leaching. The reaction of precious metal wet leaching is essentially a redox reaction, that is, the precious metal loses electrons and is oxidized to precious metal ions. In the anodic process, the metal mineral collides with the anode and loses electrons to be electrochemically oxidized and reacts with S2O3 2- Complexation is used to achieve leaching, and the leached Au(S2O3 2- )2 3- Under the action of concentration diffusion and convection, it reaches the cathode, where it obtains electrons for reduction, thereby achieving leaching and recovery. In the present invention, thiosulfate is a leaching complexing agent, and the presence of alkali solution (such as ammonia water) can prevent the insoluble products of thiosulfate from precipitating on the gold surface during the dissolution process, such as elemental sulfur. When the alkali solution is ammonia water, the complex M(S2O3)(NH)3 - The formation of can prevent the oxidation / disproportionation of unstable thiosulfate. The reaction formula is as follows:

[0036] Anode: Au+2S2O32- -e - =Au(S2O3 2- )2 3-

[0037] Cathode: Au(S2O3 2- )2 3- +e - =Au 0 +2S2O3 2-

[0038] The present invention is described in detail below with reference to specific embodiments.

[0039] The calculation formulas for the leaching rate and recovery rate of precious metals in the present invention are as follows:

[0040]

[0041]

[0042] Example 1

[0043] The electrolyte composition is 0.2M Na2S2O3, 0.2M KCl, 0.5M NH3, and is adjusted to pH 0=10 with sodium hydroxide.

[0044] S2O3 2- -KCl-NH3 system reaction electrolyte is poured into a cylindrical electrolytic cell. The anode is a pure mineral gold sheet, and the cathode is a titanium plate of the same size as the anode. Connect a DC power supply, adjust the voltage to 0.6V, adjust the speed to 500rpm for reaction, and take samples at different times. Atomic absorption spectroscopy is used to detect the gold concentration in the electrolytic cell at different time points. After 24 hours, the anode and cathode plates are collected and cleaned and dried. The quality of the anode and cathode plates before and after the reaction is compared, and the cathode plate morphology is photographed with a scanning electron microscope. Combined with the gold concentration in the solution and the cathode SEM image, the electrochemical oxidation leaching and electrodeposition reduction effects are evaluated. The experimental results are as follows: Figure 3 As shown, from Figure 3 (A) It can be seen that the gold concentration in the solution remains at around 63 mg / L from 10 h to 24 h. Figure 3 (B) The titanium plate at the cathode changes from silver to a smooth golden yellow, and a large amount of gold is deposited and covered, indicating that the gold flakes are leached at the anode while the cathode plays a reducing role. The leaching and reduction of gold can be achieved in the same system and device.

[0045] Example 2

[0046] A thiosulfate electrochemical leaching-recovery integrated extraction of gold from PCBs, the steps are as follows:

[0047] The electrolyte composition is 0.2M Na2S2O3, 0.3M KCl, 0.5M NH3, and is adjusted to pH 0=10 with sodium hydroxide.

[0048] The middle of the electrolytic cell is separated by a 600-mesh nylon mesh to prevent PCBs solid minerals from entering the cathode and to divide the electrolytic cell into anode and cathode chambers. 2- -KCl-NH3 system reaction electrolyte is poured into the anode and cathode chambers of the electrolytic cell, and the liquid levels in the two chambers are kept level. Put the PCBs powder sample in the anode chamber, connect the anode and cathode electrodes, the anode is graphite felt (GF), and the cathode is a titanium plate of the same size as the anode. Adjust the speed to 800rpm, connect the DC power supply, adjust the voltage to 0.6V and then react. After the reaction is completed, collect the solid slag in the anode chamber to measure the gold content, collect the cathode plate, dry and weigh it, and calculate the leaching rate and recovery rate. The experimental results are as follows Figure 4 As shown, under this system, the gold leaching rate is 100% and the recovery rate is 99.8%.

[0049] Example 3

[0050] A thiosulfate electrochemical leaching-recovery integrated extraction of gold from PCBs (different S2O3 2- concentration)

[0051] Prepare 5 different S2O3 2- Concentration of S2O3 2- -KCl-NH3 system reaction electrolyte, S2O3 2- The concentrations are 0.1, 0.2, 0.3, 0.4, and 0.5 M respectively, and the other reagents are 0.3 M KCl and 0.5 M NH3 respectively. The pH of the electrolyte is 0=10.

[0052] The middle of the electrolytic cell is separated by a 600-mesh nylon mesh to prevent PCBs solid minerals from entering the cathode, and the electrolytic cell is divided into anode and cathode chambers. The prepared electrolyte is poured into 5 electrolytic cells respectively, and the liquid levels of the anode and cathode chambers are kept level. The same mass of PCBs powder samples are placed in the anode chamber respectively, and the anode and cathode electrodes are connected. The anode is GF and the cathode is a titanium plate of the same size as the anode. The rotation speed is adjusted to 800rpm, and a DC power supply is connected. The voltage is adjusted to 0.6V for reaction. After the reaction is completed, the solid slag in the anode chamber is collected to measure the gold content, and the cathode plate is collected, dried and weighed, and the leaching rate and recovery rate are calculated. The experimental results are as follows Figure 5 As shown, it can be seen that different S2O3 2- The concentration has a certain influence on the leaching rate and recovery rate. 2- The best effect was achieved when the concentration was 0.3 M, with a gold leaching rate of 100% and a recovery rate of 100%.

[0053] Example 4

[0054] A thiosulfate electrochemical leaching-recovery integrated extraction of gold from PCBs (different KCl concentrations)

[0055] Prepare 5 S2O3 solutions with different KCl concentrations 2- -KCl-NH3 system reaction electrolyte, KCl concentrations are 0.1, 0.2, 0.3, 0.5, 0.7, and the other reagents are 0.2M S2O3 2- , 0.5M NH3, pH of the electrolyte is 0=10.

[0056] The middle of the electrolytic cell is separated by a 600-mesh nylon mesh to prevent PCBs solid minerals from entering the cathode, and the electrolytic cell is divided into anode and cathode chambers. The prepared electrolyte is poured into 5 electrolytic cells respectively, and the liquid levels of the anode and cathode chambers are kept level. The same mass of PCBs powder samples are placed in the anode chamber respectively, and the anode and cathode electrodes are connected. The anode is GF and the cathode is a titanium plate of the same size as the anode. The rotation speed is adjusted to 800rpm, and a DC power supply is connected. The voltage is adjusted to 0.6V for reaction. After the reaction is completed, the solid slag in the anode chamber is collected to measure the gold content, and the cathode plate is collected, dried and weighed, and the leaching rate and recovery rate are calculated. The experimental results are as follows Figure 6 As shown, it can be seen that different KCl concentrations have a great influence on the leaching rate and recovery rate. The leaching-recovery effect is best when the KCl concentration is 0.3 M, the gold leaching rate is 100%, and the recovery rate is 99.8%.

[0057] Example 5

[0058] A thiosulfate electrochemical leaching-recovery integrated extraction of gold from PCBs (different pH0)

[0059] Preparation of 6 different initial pH S2O3 2- -KCl-NH3 system reaction electrolyte, initial pH is 7, 8, 9, 10, 11, 12, and the other reagents are 0.2M S2O3 2- , 0.3M KCl, 0.5M NH3

[0060] The middle of the electrolytic cell is separated by a 600-mesh nylon mesh to prevent PCBs solid minerals from entering the cathode, and the electrolytic cell is divided into anode and cathode chambers. The prepared electrolyte is poured into 6 electrolytic cells respectively, and the liquid levels of the anode and cathode chambers are kept level. The same mass of PCBs powder samples are placed in the anode chamber respectively, and the anode and cathode electrodes are connected. The anode is GF and the cathode is a titanium plate of the same size as the anode. The speed is adjusted to 800rpm, and a DC power supply is connected. The voltage is adjusted to 0.6V for reaction. After the reaction is completed, the solid slag in the anode chamber is collected to measure the gold content, and the cathode plate is collected, dried and weighed, and the leaching rate and recovery rate are calculated. The experimental results are as follows Figure 7As shown, it can be seen that different pH0 has a great influence on the leaching rate and recovery rate, among which the leaching recovery effect is optimal when pH0=10.

[0061] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.

[0062] The above-mentioned embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for extracting precious metals by integrating thiosulfate electrochemical leaching and recovery into a short process, characterized in that: The steps include: S1: dissolving thiosulfate and electrolyte, adding alkali solution, and stirring evenly to obtain an electrolyte; the electrolyte is potassium chloride; the alkali solution is ammonia water; S2: adjusting the pH of the electrolyte to 7-13, then placing the electrolyte and the material containing the precious metal in an electrolytic cell, and performing electrolysis using an electrode system disposed in the electrolytic cell, so that the precious metal is leached at the anode and deposited at the cathode; the voltage of the electrolysis operation is 0.1-3V; the material containing the precious metal is a pure gold sheet or a waste circuit board; S3: Collect the precious metal element deposited on the cathode.

2. The method for extracting precious metals by thiosulfate electrochemical leaching-recovery integrated short process according to claim 1, characterized in that: The concentration of thiosulfate in the electrolyte is 0.1-0.5M, the concentration of the electrolyte is 0.1-0.5M, and the concentration of the alkali solution is 0.3-1.5M.

3. The method for extracting precious metals by thiosulfate electrochemical leaching-recovery integrated short process according to claim 2, characterized in that: The concentration of thiosulfate in the electrolyte is 0.2-0.3M, and the concentration of the electrolyte is 0.3-0.4M.

4. The method for extracting precious metals by thiosulfate electrochemical leaching-recovery integrated short process according to claim 1, characterized in that: In step S2, the pH of the electrolyte is adjusted to 10-11.

5. The method for extracting precious metals by thiosulfate electrochemical leaching-recovery integrated short process according to claim 1, characterized in that: The thiosulfate is one or more of sodium thiosulfate, ammonium thiosulfate and potassium thiosulfate.

6. The method for extracting precious metals by thiosulfate electrochemical leaching-recovery integrated short process according to claim 1, characterized in that: The cathode of the electrode system is a titanium plate or a copper plate, and the anode is one of platinum, titanium, copper, lead, glassy carbon, silicon carbide, stainless steel, graphite electrode, and graphite felt.

7. The method for extracting precious metals by thiosulfate electrochemical leaching-recovery integrated short process according to claim 1, characterized in that: A diaphragm is arranged in the electrolytic cell, and the diaphragm divides the electrolytic cell into a cathode chamber and an anode chamber.

8. The method for extracting precious metals by integrating thiosulfate electrochemical leaching and recovery in a short process according to claim 7, characterized in that: The diaphragm is 600-800 mesh acid and alkali resistant filter cloth or nylon mesh.

Citation Information

Patent Citations

  • Method for electrolyzing and recovering silver from silver-plated connector waste material

    CN109735710A

  • Simultaneous leaching and electrodeposition of precious metals

    US4510027A