TOPcon solar cell and method for manufacturing the same

By depositing a multi-layer hydrogen passivation layer and a silicon nitride layer on the back of the TOPcon solar cell, the chemical passivation performance is improved, and the problem of low conversion efficiency of TOPcon solar cell in the prior art is solved, thereby achieving efficiency improvement and hydrogen passivation .

CN118016763BActive Publication Date: 2024-11-01MIANYANG XINHAO NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410168713.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-06
Publication Date
2024-11-01
Estimated Expiration
2044-02-06

AI Technical Summary

Technical Problem

The conversion efficiency of existing TOPcon solar cells still has a large room for optimization, and surface suspension and defects require hydrogen for chemical passivation.

Method used

The tunneling layer, polysilicon layer, phosphorus diffusion layer and silicon nitride layer are deposited in sequence from inside to outside on the back of the silicon substrate. A hydrogen passivation layer is deposited on the inner side of each silicon nitride layer, and the passage is carried into the deposition chamber. Ammonia gas achieves constant pressure and deposition, and adopts a combined structure of a multi-layer hydrogen passivation layer and a silicon nitride layer to improve chemical passivation performance.

Benefits of technology

By increasing atomic hydrogen to passivate the hanging bonds on the surface of the silicon wafer, the open circuit voltage is increased, and the conversion efficiency of TOPcon solar cells is increased by more than 0.0805%. The total thickness of the back mask layer is 70nm~90nm, and the refractive index is 2.0~2.5.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118016763B_ABST
    Figure CN118016763B_ABST
Patent Text Reader

Abstract

The present application provides a TOPcon solar cell and a method for making the same, the preparation method comprising: depositing a boron diffusion layer, an aluminum oxide layer and a composite layer on the front side of a silicon substrate from the inside to the outside, and depositing a tunneling layer, a polysilicon layer, a phosphorus diffusion layer and at least one silicon nitride layer on the back side of the silicon substrate from the inside to the outside, and a hydrogen passivation layer is deposited on the inner side of each silicon nitride layer; wherein the deposition method of all hydrogen passivation layers is: firstly introducing ammonia into the deposition chamber to achieve constant pressure, and then continuing to introduce ammonia to achieve deposition. By depositing a layer of hydrogen passivation layer before depositing the silicon nitride layer, atomic hydrogen is added to passivate the dangling bonds on the surface of the silicon wafer, thereby ensuring the hydrogen passivation effect, improving the chemical passivation performance, and improving the open circuit voltage, thereby improving the conversion efficiency of the TOPcon solar cell by more than 0.0805%, and the total thickness of the back film layer is 70nm to 90nm, and the refractive index is 2.0 to 2.5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of solar cells, and more specifically, to a TOPcon solar cell with a back surface hydrogenation film passivated and a method for manufacturing the same. Background Art

[0002] A solar cell is a device that effectively absorbs solar radiation and converts light energy into electrical energy using the photovoltaic effect. When sunlight shines on the semiconductor PN junction, new hole-electron pairs are formed. Under the action of the PN junction electric field, holes flow from the N region to the P region, and electrons flow from the P region to the N region. When the circuit is connected, current is formed. Since it is a solid semiconductor device that converts solar energy into electrical energy using the photovoltaic effect of various potential barriers, it is also called a solar cell or photovoltaic cell, and is an important component of the solar cell array power supply system.

[0003] With the development of solar cells and market demand, the improvement of TOPcon cell manufacturing cost and conversion efficiency has become the industry's first choice to solve the problem. The efficiency of existing TOPcon cells still has a lot of room for optimization, and considering surface suspension and defects, hydrogen is still needed for chemical passivation. Summary of the invention

[0004] The technical problem to be solved by the present invention is: how to improve the conversion efficiency of TOPcon batteries.

[0005] The technical solution of the present invention is:

[0006] A method for manufacturing a TOPcon solar cell with a back surface hydrogenation film passivated, comprising:

[0007] A boron diffusion layer, an aluminum oxide layer and a composite layer are sequentially deposited on the front side of the silicon substrate from the inside to the outside, and a tunneling layer, a polysilicon layer, a phosphorus diffusion layer and at least one silicon nitride layer are sequentially deposited on the back side of the silicon substrate from the inside to the outside, and a hydrogen passivation layer is deposited on the inner side of each silicon nitride layer;

[0008] Among them, the deposition methods of all hydrogen passivation layers are: firstly, ammonia gas is introduced into the deposition chamber to achieve constant pressure, and then ammonia gas is continued to be introduced to achieve deposition.

[0009] As a possible design, the hydrogen passivation layer has a total of four layers, and the silicon nitride layer has a total of four layers, and the order of the hydrogen passivation layer and the silicon nitride layer is: the first hydrogen passivation layer, the first silicon nitride layer, the second hydrogen passivation layer, the second silicon nitride layer, the third hydrogen passivation layer, the third silicon nitride layer, the fourth hydrogen passivation layer and the fourth silicon nitride layer, and the first hydrogen passivation layer is adjacent to the phosphorus diffusion layer.

[0010] As a possible design, when depositing the first hydrogen passivation layer, the flow rate of ammonia required for constant pressure is 11000-12500 ml / min, the time required is 15-25 s, and the flow rate of ammonia required for deposition is 11000-12500 ml / min, the time required is 55-65 s.

[0011] As a possible design, when depositing the second hydrogen passivation layer, the ammonia flow rate required for constant pressure is 15000-17000 ml / min, the required time is 15-25 s, and the ammonia flow rate required for deposition is 15000-17000 ml / min, the required time is 55-65 s.

[0012] As a possible design, when depositing the third hydrogen passivation layer and the fourth hydrogen passivation layer, the flow rate of ammonia required for constant pressure is 17500-19000 ml / min, the time required is 15-25 s, and the flow rate of ammonia required for deposition is 17500-19000 ml / min, the time required is 55-65 s.

[0013] As a possible design, when depositing the first hydrogen passivation layer and the second hydrogen passivation layer, the discharge power of the deposition chamber during deposition is 14200-14500 kw.

[0014] As a possible design, when depositing the third hydrogen passivation layer and the fourth hydrogen passivation layer, the discharge power of the deposition chamber during deposition is 15200-15500 kw.

[0015] The beneficial effects of the present invention are:

[0016] The present invention deposits a hydrogen passivation layer before depositing the silicon nitride layer, thereby adding atomic hydrogen to passivate the dangling bonds on the surface of the silicon wafer, ensuring the hydrogen passivation effect, improving the chemical passivation performance, and improving the open circuit voltage, thereby improving the conversion efficiency of the TOPcon solar cell by more than 0.0805%. The total thickness of the back film layer is 70nm to 90nm, and the refractive index is 2.0 to 2.5. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0018] Figure 1 It is a schematic diagram of the structure of an existing TOPcon solar cell;

[0019] Figure 2This is a schematic diagram of the structure of a TOPcon solar cell prepared in Example 1;

[0020] Among them, the reference numerals in the figure are:

[0021] 1-silicon substrate, 2-boron diffusion layer, 3-aluminum oxide layer, 4-composite layer, 5-metal electrode, 6-tunneling layer, 7-polysilicon layer, 8-phosphorus diffusion layer, 9-first hydrogen passivation layer, 10-first silicon nitride layer, 11-second hydrogen passivation layer, 12-second silicon nitride layer, 13-third hydrogen passivation layer, 14-third silicon nitride layer, 15-fourth hydrogen passivation layer, 16-fourth silicon nitride layer. DETAILED DESCRIPTION

[0022] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0023] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.

[0024] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0025] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0026] The structure of existing TOPcon solar cells is as follows Figure 1 As shown by Figure 1It can be seen that the existing TOPcon solar cell includes a silicon substrate, on the front side of which a boron diffusion layer, an aluminum oxide layer and a composite layer are deposited in sequence from the inside to the outside; on the back side of the silicon substrate, a tunneling layer, a polysilicon layer, a phosphorus diffusion layer and a multi-layer silicon nitride layer are deposited in sequence from the inside to the outside.

[0027] It should be noted that in the aforementioned “inside to outside”, the inside refers to the side close to the silicon substrate, and the outside refers to the side away from the silicon substrate.

[0028] The structure of the TOPcon solar cell disclosed in the present invention is as follows Figure 2 As shown by Figure 2 It can be seen that the TOPcon solar cell includes a silicon substrate, on the front side of which a boron diffusion layer 2, an aluminum oxide layer 3 and a composite layer 4 are sequentially deposited from the inside to the outside; on the back side of the silicon substrate, a tunneling layer 6, a polysilicon layer 7, a phosphorus diffusion layer 8 and at least one silicon nitride layer are sequentially deposited from the inside to the outside, and a hydrogen passivation layer is deposited on the inner side of each silicon nitride layer;

[0029] Among them, the deposition methods of all hydrogen passivation layers are: firstly, ammonia gas is introduced into the deposition chamber to achieve constant pressure, and then ammonia gas is continued to be introduced to achieve deposition.

[0030] It should be noted that the inner side of the silicon nitride layer refers to the side of the silicon nitride layer close to the silicon substrate. By depositing a hydrogen passivation layer on the inner side of the silicon nitride layer, atomic hydrogen is added to passivate the dangling bonds on the surface of the silicon wafer, ensuring the hydrogen passivation effect, improving the chemical passivation performance, and increasing the open circuit voltage, thereby improving the conversion efficiency of the TOPcon solar cell.

[0031] Generally, the number of silicon nitride layers is selected according to actual needs, so the number of hydrogen passivation layers is the same as the number of silicon nitride layers.

[0032] In the present invention, the number of silicon nitride layers is 4, so the number of hydrogen passivation layers is also 4, namely the first hydrogen passivation layer 9, the second hydrogen passivation layer 11, the third hydrogen passivation layer 13 and the fourth hydrogen passivation layer 15. The arrangement order of the 4 hydrogen passivation layers and the 4 silicon nitride layers is: the first hydrogen passivation layer 9, the first silicon nitride layer 10, the second hydrogen passivation layer 11, the second silicon nitride layer 12, the third hydrogen passivation layer 13, the third silicon nitride layer 14, the fourth hydrogen passivation layer 15 and the fourth silicon nitride layer 16, and the first hydrogen passivation layer 9 is adjacent to the phosphorus diffusion layer 8.

[0033] In practical applications, the thickness of each hydrogen passivation layer may be the same or different, and the thickness is selected according to the actual situation.

[0034] It should be noted that except for the hydrogen passivation layer, the thickness and manufacturing process of other layers are Figure 1The manufacturing process of the existing TOPcon solar cells shown is the same, for example: a conventional texturing process, which will not be described in detail here.

[0035] All the manufacturing processes of hydrogen passivation layers are carried out by deposition, and the medium used for deposition is ammonia. When depositing the first hydrogen passivation layer 9, the flow rate of ammonia required for constant pressure is 11000-12500ml / min, for example: 11000ml / min, 11200ml / min, 11500ml / min, 11800ml / min, 12000ml / min, 12200ml / min, 12500ml / min and any value between any two values, preferably 12500ml / min; the required time is 15-25s, for example: 15s, 18s, 20s, 23s, 25s and any value between any two values, preferably 20s. The flow rate of ammonia required for deposition is 11000-12500 ml / min, for example: 11000 ml / min, 11200 ml / min, 11500 ml / min, 11800 ml / min, 12000 ml / min, 12200 ml / min, 12500 ml / min and any value between any two values, preferably 12500 ml / min; the time required is 55-65 s, for example: 55 s, 58 s, 60 s, 62 s, 65 s and any value between any two values, preferably 60 s.

[0036] When depositing the second hydrogen passivation layer 11, the flow rate of ammonia required for constant pressure is 15000-17000 ml / min, for example: 15000 ml / min, 15500 ml / min, 16000 ml / min, 16500 ml / min, 17000 ml / min and any value between any two values, preferably 16500 ml / min; the required time is 15-25 s, for example: 15 s, 18 s, 20 s, 22 s, 24 s, 25 s and any value between any two values. value, preferably 20s; the flow rate of ammonia required for deposition is 15000-17000ml / min, for example: 15000ml / min, 15500ml / min, 16000ml / min, 16500ml / min, 17000ml / min and any value between any two values, preferably 16500ml / min; the time required is 55-65s, for example: 55s, 58s, 60s, 62s, 65s and any value between any two values, preferably 60s.

[0037] When depositing the third hydrogen passivation layer 13 and the third hydrogen passivation layer 13, the flow rate of ammonia required for constant pressure is 17500-19000ml / min, for example: 17500ml / min, 17800ml / min, 18000ml / min, 18500ml / min, 18300ml / min, 18500ml / min, 18800ml / min, 19000ml / min and any value between any two values, preferably 18500ml / min; the time required is 15-25s, for example: 15s, 18s, 20s, 23s, 25s and any value between any two values, preferably 20s.

[0038] The control of the discharge power of ammonia gas required for deposition is very important, which is related to the thickness of the hydrogen passivation layer and the adjacent film layers are not excessively damaged.

[0039] Generally, when depositing the first hydrogen passivation layer 9 and the second hydrogen passivation layer 11, the discharge power of the deposition chamber is 14200-14500 kw, for example: 14200 kw, 14300 kw, 14400 kw, 14500 kw and any value between any two values, preferably 14500 kw.

[0040] When depositing the third hydrogen passivation layer 13 and the fourth hydrogen passivation layer 15, the discharge power of the deposition chamber is 15200-15500 kw, for example, 15200 kw, 15300 kw, 15400 kw, 15500 kw and any value between any two values, preferably 15500 kw.

[0041] Example 1

[0042] The production of TOPcon solar cells includes the following steps:

[0043] S1. Using a conventional texturing process, the n-type original silicon wafer is immersed in a mixed solution of 2% by mass NaOH and 6% by mass H2O2 at a temperature of 65°C to 70°C to remove the damaged layer, and then a mixed solution of 1% by mass KOH or NaOH solution and a certain amount of isopropanol or a texturing additive is used to texturize the double sides;

[0044] S2. Load the textured silicon wafer obtained after double-sided texturing (back-to-back double insertion) into a tubular low-pressure boron diffusion furnace tube, and then keep the temperature constant at 900°C to 920°C for 100 minutes to complete the preparation of the front boron diffusion layer 2;

[0045] S3. The borosilicate glass layer on the back surface of the silicon substrate 1 is removed on one side using an HF solution, and then the back surface is polished using a mixed solution of NaOH and an additive;

[0046] S4. On the back surface, a tunneling layer 6, a polysilicon layer 7 and a phosphorus diffusion layer 8 are grown in sequence by using LPCVD equipment at a temperature of 560° C. to 580° C. The growth pressure of the tunneling layer 6 is 760 torr.

[0047] S5. Using HF solution to remove the borosilicate glass layer on the front surface of the silicon substrate 1 on one side, then using KOH (or NaOH) and an additive mixed solution to remove the polysilicon coating layer produced on the front surface, and finally using HF solution to remove the borosilicate glass and borosilicate glass layer on the front and back sides of the silicon substrate 1;

[0048] S6. A layer of 8nm Al2O3 is grown on the front surface using atomic layer deposition technology, and then a layer of 85nm thick SiN is plated on the front surface of the battery using PECVD equipment. x +SiON x +SiO2 composite film layer, the flow ratio of SiH4 and NH3 during the coating process is about 1:4, and the coating temperature is set at 480-550℃;

[0049] S7. The product obtained in step S6 is placed in a deposition chamber using PECVD equipment to deposit the first hydrogen passivation layer 9. Before deposition, ammonia gas is introduced into the deposition chamber at a flow rate of 12500 ml / min for 20 seconds to achieve a constant pressure effect, and then ammonia gas is introduced at a flow rate of 12500 ml / min for 60 seconds. The first hydrogen passivation layer 9 is deposited at a discharge power of 14000 kW.

[0050] S8. The product obtained in step S7 is treated with PECVD equipment using low-temperature plasma as an energy source. The silicon wafer is placed on the cathode of glow discharge under low pressure. The silicon wafer is heated to a predetermined temperature by glow discharge (or with a heating element). Then, an appropriate amount of SiH4 and NH3 are introduced. After a series of chemical reactions and plasma reactions, a solid film is formed on the surface of the sample. Specifically, SiN x Membrane layer.

[0051] S9. The product obtained in step S8 is placed in a deposition chamber to deposit a second hydrogen passivation layer 11. Before deposition, ammonia gas is introduced into the deposition chamber at a flow rate of 16500 ml / min for 20 seconds to achieve a constant pressure effect, and then ammonia gas is introduced at a flow rate of 16500 ml / min for 60 seconds. The discharge power is 14500 kw to deposit the second hydrogen passivation layer 11;

[0052] S10. Continue to coat another layer of SiN on the positive surface of the battery in the PECVD equipment. x The flow ratio of SiH4 to NH3 during the coating process is about 1:4, and the coating temperature is set at 480-550°C.

[0053] S11. The product obtained in step S10 is placed in a deposition chamber to deposit a third hydrogen passivation layer 13. Before deposition, ammonia is introduced into the deposition chamber at a flow rate of 18500 ml / min for 20 seconds to achieve a constant pressure effect, and then ammonia is introduced at a flow rate of 18500 ml / min for 60 seconds, and the discharge power is 15500 kw to deposit the third hydrogen passivation layer 13;

[0054] S12. The product obtained in step S11 is further treated in the PECVD device to coat a layer of SiN on the positive surface of the battery. x The flow ratio of SiH4 to NH3 during the coating process is about 1:4, and the coating temperature is set at 480-550°C.

[0055] S13. The product obtained in step S12 is placed in a deposition chamber to deposit a fourth hydrogen passivation layer 15. Before deposition, ammonia is introduced into the deposition chamber at a flow rate of 18500 ml / min for 20 seconds to achieve a constant pressure effect, and then ammonia is introduced at a flow rate of 18500 ml / min for 60 seconds, and the discharge power is 15500 kw to deposit the fourth hydrogen passivation layer 15;

[0056] S14. Continue to coat another layer of SiN on the positive surface of the battery in the PECVD equipment. x The flow ratio of SiH4 to NH3 during the coating process is about 1:4, and the coating temperature is set at 480-550°C.

[0057] It should be noted that the total thickness of all film layers on the back surface of the silicon substrate 1 is 85 nm.

[0058] S15. The front and back sides of the coated battery structure are screen-printed respectively, and then sintered at a high temperature to complete the metallization process of the front and back sides of the battery structure.

[0059] The structure of the TOPcon solar cell obtained in this embodiment is as follows Figure 2 As shown by Figure 2 It can be seen that the TOPcon solar cell includes a silicon substrate, on the front side of which a boron diffusion layer 2, an aluminum oxide layer 3 and a composite layer 4 are deposited in sequence from the inside to the outside, and on the back side of the silicon substrate, a tunneling layer 6, a polysilicon layer 7, a phosphorus diffusion layer 8, a first hydrogen passivation layer 9, a first silicon nitride layer 10, a second hydrogen passivation layer 11, a second silicon nitride layer 12, a third hydrogen passivation layer 13, a third silicon nitride layer 14, a fourth hydrogen passivation layer 15 and a fourth silicon nitride layer 16 are deposited in sequence from the inside to the outside, and the first hydrogen passivation layer 9 is adjacent to the phosphorus diffusion layer 8.

[0060] Comparative Example

[0061] This comparative example discloses an existing TOPcon solar cell, whose structure is as follows Figure 1 shown.

[0062] Now Figure 1 The conversion efficiency of the TOPcon solar cells obtained in the embodiment 1 and the embodiment 2 is tested, and the results are 25.42% and 25.50% respectively. It can be seen that the conversion efficiency of the cell is significantly improved by adding the hydrogen passivation layer.

[0063] Figure 1 The opening voltages of the TOPcon solar cells shown and obtained in Example 1 are 0.7239 and 0.7251, respectively.

[0064] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for manufacturing a TOPcon solar cell with a back surface hydrogenation film passivated, It is characterized in that The preparation method comprises: A boron diffusion layer, an aluminum oxide layer and a composite layer are sequentially deposited on the front side of the silicon substrate from the inside to the outside, and a tunneling layer, a polysilicon layer, a phosphorus diffusion layer and at least one silicon nitride layer are sequentially deposited on the back side of the silicon substrate from the inside to the outside, and a hydrogen passivation layer is deposited on the inner side of each silicon nitride layer; Among them, the deposition methods of all hydrogen passivation layers are: firstly, ammonia gas is introduced into the deposition chamber to achieve constant pressure, and then ammonia gas is continuously introduced to achieve deposition; There are four hydrogen passivation layers in total, and there are four silicon nitride layers in total. The order of the hydrogen passivation layers and the silicon nitride layers is: the first hydrogen passivation layer, the first silicon nitride layer, the second hydrogen passivation layer, the second silicon nitride layer, the third hydrogen passivation layer, the third silicon nitride layer, the fourth hydrogen passivation layer and the fourth silicon nitride layer, and the first hydrogen passivation layer is adjacent to the phosphorus diffusion layer. When depositing the first hydrogen passivation layer, the flow rate of ammonia required for constant pressure is 11000~12500ml / min, and the time required is 15~25s. The flow rate of ammonia required for deposition is 11000~12500ml / min, and the time required is 55~65s; when depositing the second hydrogen passivation layer, the flow rate of ammonia required for constant pressure is 15000~17000ml / min, the time required is 15~25s, and the flow rate of ammonia required for deposition is 15000~17000ml / min, and the time required is 55~65s; when depositing the third hydrogen passivation layer and the fourth hydrogen passivation layer, the flow rate of ammonia required for constant pressure is 17500~19000ml / min, the time required is 15~25s, and the flow rate of ammonia required for deposition is 17500~19000ml / min, and the time required is 55~65s.

2. The method for manufacturing a TOPcon solar cell with a back surface hydrogenation film passivated according to claim 1, It is characterized in that When depositing the first hydrogen passivation layer and the second hydrogen passivation layer, the discharge power of the deposition chamber is 14200-14500 kw.

3. The method for manufacturing a TOPcon solar cell with a back surface hydrogenation film passivated according to claim 2, It is characterized in that When depositing the third hydrogen passivation layer and the fourth hydrogen passivation layer, the discharge power of the deposition chamber during deposition is 15200-15500 kw.

4. A method for manufacturing a TOPcon solar cell with a back surface hydrogenation film passivated as claimed in any one of claims 1 to 3 to produce a TOPcon solar cell.

5. The TOPcon solar cell according to claim 4, It is characterized in that The tunneling layer, polysilicon layer, phosphorus diffusion layer, first hydrogen passivation layer, silicon nitride layer, second hydrogen passivation layer, silicon nitride layer, third hydrogen passivation layer, silicon nitride layer, fourth hydrogen passivation layer and silicon nitride layer form a back film layer, and the total thickness of the back film layer is 70nm~90nm.

6. The TOPcon solar cell according to claim 5, It is characterized in that The refractive index of the back film layer is 2.0-2.5.