A multi-component alloy, its preparation method and its application
By preparing a multi-component alloy with the chemical formula Cr1.3Fe2Ni2(AlTi)x, the limitations of multi-component alloys in marine and nuclear power environments have been addressed, achieving a combination of high strength and corrosion resistance, and expanding its industrial application scope.
Patent Information
- Application Number
- CN202410195687.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-02-22
AI Technical Summary
Multicomponent alloys are rarely used in marine and nuclear power environments, and existing technologies are insufficient to meet the mechanical properties and corrosion resistance requirements under extreme conditions.
Using a multi-component alloy with the chemical formula Cr1.3Fe2Ni2(AlTi)x, a BCC+FCC dual-phase structure was formed by controlling the molar ratio of each component raw material and the melting process parameters through a high-vacuum electric arc melting method. Combined with the lattice distortion effect of Al and Ti elements, an alloy with excellent mechanical properties and corrosion resistance was prepared.
The alloy exhibits high tensile strength and elongation after fracture, and its self-corrosion potential and current density are superior to those of common alloys. It is low in cost and widely applicable to extreme environments such as nuclear power and marine environments, thus broadening the scope of industrial applications.
Smart Images

Figure CN118028683B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of metallic materials, and in particular to a multi-component alloy, its preparation method, and its application. Background Technology
[0002] Multicomponent alloys are a class of alloy systems composed of five or more alloying elements. Compared with traditional crystalline alloys, multicomponent alloys exhibit four typical characteristic effects that result in higher strength and hardness, better corrosion and fatigue resistance, better thermal stability, and better resistance to neutron radiation. Therefore, multicomponent alloys are considered to have great potential as a next-generation structural material, attracting widespread attention from researchers both domestically and internationally.
[0003] Extreme operating conditions such as marine and nuclear power environments require novel structural materials with excellent mechanical properties, corrosion resistance, and even neutron radiation resistance. These materials are fundamental to ensuring the safe, efficient, and long-life operation of equipment and components. Currently, the application of multi-component alloys in this field is relatively limited. Summary of the Invention
[0004] This application provides a multi-component alloy, its preparation method, and its application, which addresses the technical problem that multi-component alloys are relatively rarely used in marine and nuclear power environments.
[0005] The first aspect of this application provides a multi-component alloy with the chemical formula Cr. 1.3 Fe2Ni2(AlTi) x The components are composed according to the molar ratio of the subscripts in the chemical formula, where x is (0, 0.4).
[0006] Furthermore, x can be 0.1, 0.2, 0.3, or 0.4.
[0007] The second aspect of this application is a method for preparing a multi-component alloy, wherein five raw materials, namely Cr, Fe, Ni, Al and Ti, are mixed in a molar ratio of 1.3:2:2:x:x and then subjected to high-vacuum arc melting. After melting, the resulting metal solution is vacuum cast into a multi-component alloy ingot; wherein x is taken as (0, 0.4).
[0008] Furthermore, the purity of each of the aforementioned component raw materials is greater than or equal to 99.9%.
[0009] Furthermore, during the high-vacuum electric arc melting process, the raw materials are stacked according to their melting points from low to high, with the raw materials having the lowest melting points placed on the heated surface of the melting vessel.
[0010] Furthermore, before the high-vacuum arc melting, the vacuum is evacuated to 9×10⁻⁶. -4 Pa ~ 1×10-3 Pa, then purged with argon to -0.03MPa to -0.02MPa, and finally the Ti ingot was melted 3 to 5 times, each time for 60 to 80 seconds.
[0011] Furthermore, the high-vacuum arc melting is performed 5 to 6 times, with a melting current of 240A to 270A, and each melting arc lasts for 2 to 3 minutes.
[0012] Furthermore, during the high-vacuum arc melting process, after each of the component raw materials has melted into a liquid state, it is electromagnetically stirred 5 to 6 times, with an electromagnetic stirring current of 1.5A to 2.5A, and each stirring session lasting 1 to 2 minutes.
[0013] The third aspect of this application provides the application of the multi-component alloys obtained by the preparation method of the multi-component alloys of the first aspect and the second aspect in nuclear power environments and marine environments.
[0014] Beneficial effects
[0015] In the embodiments of this application, the chemical formula Cr was used. 1.3 Fe2N i2 (AlTi) x This multi-component alloy, in which Al, Ti, and Ni combine to form a BCC structure, transforms the alloy system from a single-phase FCC structure to a two-phase structure. The formation of the second phase makes dislocation movement more difficult, and the significant difference in atomic radii between Al and Ti and Fe, Ni, and Cr easily leads to larger lattice distortions. The combined effect of these two elements enhances the mechanical properties of the material. Simultaneously, Cr is enriched in the FCC phase, while Al and Ti are enriched in the BCC phase, enabling the formation of a dense passivation film on the alloy surface, thus improving the material's corrosion resistance.
[0016] Depending on the AlTi content, Cr 1.3 Fe2N i2 (AlTi) x The multi-component alloys exhibit tensile strengths ranging from 301 MPa to 910 MPa, elongation after fracture from 6% to 61%, self-corrosion potentials from -73.8 mV to -257.4 mV, and self-corrosion current densities of 6.83 × 10⁻⁶. -8 A / cm 2 ~7.64×10 -8 A / cm 2 In particular, when x = 0.2 and 0.3, the alloy exhibits better overall performance, with tensile strengths of 820 MPa and 864 MPa, elongation after fracture of 35% and 21%, respectively, and a self-corrosion current density of 6.70 × 10⁻⁶. - 8 A / cm 2With 6.83×10 -8 A / cm 2 The self-corrosion potentials are -192.6mV and -226.7mV, and the overall performance of the alloy is better than most as-cast multi-component alloys.
[0017] The raw materials of this invention are readily available, and the preparation method is simple and easy to implement, which greatly reduces the preparation cost of the alloy. At the same time, it combines excellent mechanical properties and corrosion resistance, and does not contain Co, so it has a good cost performance. The alloy system can be widely used in extreme environments such as nuclear power and ocean, which greatly expands the industrial application scenarios of multi-component alloys. Attached Figure Description
[0018] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments and descriptions of this application are used to explain this application and do not constitute an undue limitation of this application. In the drawings:
[0019] Figure 1 The X-ray diffraction pattern of the multi-component alloy in Example 1 of this invention;
[0020] Figure 2 This is a hardness diagram of the multi-component alloy in Example 1 of the present invention;
[0021] Figure 3 The mechanical properties diagram of the multi-component alloy in Example 1 of this invention is shown.
[0022] Figure 4 The polarization curve of the multi-component alloy in Example 1 of this invention in a 3.5 wt.% NaCl solution is shown. Detailed Implementation
[0023] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. This application will now be described in detail with reference to the accompanying drawings and embodiments.
[0024] Example 1
[0025] Example 1 of the present invention provides a method for preparing a multi-component alloy, comprising the following steps:
[0026] Step 1: Combine the component raw materials Cr, Fe, Ni, Al, and Ti according to the general formula Cr 1.3 The molar ratio of the subscripts of each component in Fe2Ni2(AlTi)x is weighed, where x is taken as (0, 0.4).
[0027] The raw materials Cr, Fe, Ni, Al and Ti are all high-purity raw materials that are industrial grade raw materials with a purity of 99.9% or higher. These raw materials are then pretreated to remove impurities. The Fe, Ni, Cr, Al and Ti metal particles are then ultrasonically cleaned with anhydrous ethanol to obtain clean metal particles, ensuring that the weighing amount is accurate and free of impurities.
[0028] Step 2: Place the weighed raw materials into a vacuum arc melting furnace and melt them under the protection of high-purity Ar gas with a purity of ≥99.9%. After melting, the resulting metal solution is vacuum cast and then cooled in the furnace to form a multi-component alloy ingot.
[0029] In the above embodiment, a crucible is placed in the vacuum arc melting furnace as a carrier to hold the raw materials of each component. In order to prevent the raw material components with low melting point from volatilizing when heated, the raw materials of each component are stacked in the order of melting point from low to high, namely Al, Ni, Fe, Ti and Cr, with Al, the raw material with the lowest melting point, placed on the bottom of the crucible, and the remaining raw materials are stacked one by one.
[0030] In the above embodiments, to avoid the presence of harmful gases in the vacuum arc melting furnace that could affect the alloy's properties, the vacuum level of the arc furnace is evacuated to 9 × 10⁻⁶ before melting using a molecular pump or vacuum pump. -4 ~1×10 -3 The vacuum level within the above range can prevent the alloy from oxidizing during the melting process. Afterwards, argon gas is purged to -0.05MPa to -0.04MPa, and the Ti ingot is melted 3 to 5 times before melting, each time for 60 to 80 seconds.
[0031] In the above embodiments, in order to prevent the occurrence of unfused or incompletely melted high-melting-point alloying elements, and thus ensure the uniform distribution of alloying elements and prevent the enrichment of elements from adversely affecting the performance of the alloy, the melting current is 240A to 270A, and the melting is repeated 5 to 6 times, with each melting arc lasting 2 to 3 minutes.
[0032] In the above embodiments, since different elements have different melting rates, as well as varying viscosities and fluidities after melting, electromagnetic stirring is activated after the alloy transitions from a solid to a liquid state during the melting process to promote fusion of the various alloy components. The electromagnetic stirring current must be within the safe allowable range of the vacuum arc melting furnace; in this embodiment, it is set to 1.5A to 2.5A, with 5 to 6 electromagnetic stirring cycles, each lasting 1 to 2 minutes. Under the action of the aforementioned electromagnetic stirring current, the liquid metal exhibits good fluidity, the alloying elements are fully fused, and the alloy properties reach their optimal state.
[0033] The multi-component alloy obtained through the above steps has the chemical formula Cr. 1.3 Fe2Ni2(AlTi)x The components are composed according to the molar ratio of the subscripts in the chemical formula, where x is (0, 0.4).
[0034] In the above embodiments, x taking the values of 0.1, 0.2, 0.3, or 0.4 corresponds to obtaining Cr. 1.3 Fe2Ni2(AlTi) 0.1 Cr 1.3 Fe2Ni2(AlTi) 0.2 Cr 1.3 Fe2Ni2(AlTi) 0.3 and Cr 1.3 Fe2Ni2(AlTi) 0.4 .
[0035] The micro-Vickers hardness, mechanical properties, and electrochemical properties of the multi-component alloy prepared in Example 1 were tested. The specific testing methods are as follows:
[0036] The prepared multi-component alloy samples were coarsely ground with sandpaper of different grades, finely ground to 2000 grit, and then polished with W2.5 diamond polishing paste on a polishing machine until the surface was free of scratches. After rinsing with alcohol, the samples were dried.
[0037] XRD tests were performed using an Empyrean multi-functional powder X-ray diffractometer. The test results are as follows: Figure 1 As shown in the figure, with the increase of Al and Ti content, the multi-component alloy transforms from a single FCC phase to an FCC+BCC dual-phase structure.
[0038] The hardness of multi-component alloy materials was tested using an HV-1000BZ automatic turret microhardness tester. The test results are as follows: Figure 2 As shown in the figure, the hardness increases with increasing Al and Ti content.
[0039] The mechanical properties of multi-component alloy materials were tested using an E44.304-B type electronic universal testing machine. The test results are as follows: Figure 3 As shown in the figure, the strength of the alloy increases with increasing Al and Ti content.
[0040] Electrochemical corrosion performance tests were conducted on multi-component alloy samples using the CorrTest electrochemical testing system. The test results are as follows: Figure 4 As shown, the corrosion potential is basically between 0 and -0.3V.
[0041] Comparative Example
[0042] Table 1 presents the multi-component alloys Cr obtained when x is 0.2 and 0.3 in the multi-component alloys of the embodiments of the present invention. 1.3Fe2Ni2(AlTi) 0.2 Cr 1.3 Fe2Ni2(AlTi) 0.3 Performance comparison with some as-cast multi-component alloys. As shown in Table 1, the overall performance of the alloy obtained in this embodiment is superior to most as-cast multi-component alloys.
[0043] Table 1
[0044] Alloy Sample Tensile strength (MPa) Elongation after fracture (%) <![CDATA[Cr 1.3 Fe2Ni2(AlTi) 0.2 ]]> 820 35 <![CDATA[Cr 1.3 Fe2Ni2(AlTi) 0.3 ]]> 864 21 CoCrFeNi 413 48 <![CDATA[Al 0.3 CoCrFeNi]]> 528 37 <![CDATA[FeMnNiCuCoSn 0.03 ]]> 477 17 CoCrFeMnNi 491 71
[0045] Table 2 presents the results of multi-component alloys Cr obtained when x is 0.2 and 0.3 in this embodiment. 1.3 Fe2Ni2(AlTi) 0.2 Cr 1.3 Fe2Ni2(AlTi) 0.3 Electrochemical parameters of the alloy in 3.5 wt.% NaCl solution were compared with those of 304SS and other multi-component alloys. Table 2 shows that the self-corrosion current density of the alloy in this embodiment is lower than that of other multi-component alloys and 304SS. This means that the corrosion rate of the alloy sample is slower and the self-corrosion potential is relatively larger during corrosion, indicating a relatively weaker tendency to corrode. The combination of these two factors suggests that the Cr alloy in this embodiment exhibits... 1.3 Fe2Ni2(AlTi) 0.2 and Cr 1.3 Fe2Ni2(AlTi) 0.3 The electrochemical performance of the alloy is superior to that of other common multi-component alloys and 304ss.
[0046] Table 2
[0047]
[0048] Therefore, this embodiment uses a FeNiCr multi-component alloy as the matrix and combines traditional alloy design methods. By adjusting the composition and adding Al and Ti elements with significantly different atomic radii from the matrix elements, and further controlling the vacuum degree, protective atmosphere, and melting current during the melting process, a multi-component alloy with excellent mechanical properties and good corrosion resistance is prepared. This provides a complete technical route for the composition design and preparation of multi-component alloys with excellent performance. The raw materials in the above embodiment are readily available, and the preparation method is simple and easy to implement, greatly reducing the alloy preparation cost. At the same time, the excellent mechanical properties and corrosion resistance are combined, and the absence of Co element provides good cost performance. The alloy system can be widely used in extreme environments such as nuclear power and marine environments, such as key metal components of equipment in nuclear power, oil and gas extraction, and seawater desalination, greatly expanding the industrial application scenarios of multi-component alloys.
[0049] The above are merely embodiments of this application and are not intended to limit the scope of this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of the claims of this application.
Claims
1. A multi-component alloy, characterized in that, Its chemical formula is Cr 1.3 Fe2Ni2(AlTi) x The components are composed according to the molar ratios indicated by the subscripts in the chemical formula, where x is taken as... The alloy system is a two-phase structure, in which Al, Ti and Ni elements combine to form a BCC structure, with Cr enriched in the FCC phase and Al and Ti enriched in the BCC phase. In this process, the raw materials are mixed in a molar ratio and subjected to high-vacuum arc melting. After melting, the resulting metal solution is vacuum cast into a multi-component alloy ingot. The high-vacuum arc melting is performed 5 to 6 times, with a melting current of 240A to 270A, and each melting arc lasts for 2 to 3 minutes. During the high-vacuum arc melting, after each raw material has melted into a liquid state, it is electromagnetically stirred 5 to 6 times, with an electromagnetic stirring current of 1.5A to 2.5A, and each stirring lasts for 1 to 2 minutes.
2. The multi-component alloy according to claim 1, characterized in that, The value of x is 0.2 or 0.
3.
3. A method for preparing a multi-component alloy, characterized in that, Five raw materials, namely Cr, Fe, Ni, Al, and Ti, were mixed in a molar ratio of 1.3:2:2:x:x and then subjected to high-vacuum arc melting. The purity of each raw material was greater than or equal to 99.9%. After melting, the resulting metal solution was vacuum cast into a multi-component alloy ingot. Wherein, x represents... Al, Ti, and Ni elements combine to form a BCC structure, and the alloy system is a two-phase structure, with Cr enriched in the FCC phase and Al and Ti enriched in the BCC phase. Before the high-vacuum arc melting, the vacuum level is evacuated to 9×10⁻⁶. -4 Pa ~ 1×10 -3 Pa, then purged with argon gas to -0.03MPa to -0.02MPa, and finally the Ti ingot was melted 3 to 5 times, each time for 60 to 80 seconds; The high-vacuum electric arc melting is performed 5 to 6 times, with a melting current of 240A to 270A, and each melting arc lasts for 2 to 3 minutes. During the high-vacuum electric arc melting process, after each component raw material has melted into a liquid state, it is electromagnetically stirred 5 to 6 times. The electromagnetic stirring current is 1.5A to 2.5A, and the duration of each stirring is 1 to 2 minutes.
4. The method according to claim 3, characterized in that, During the high-vacuum electric arc melting process, the raw materials are stacked according to their melting points from low to high, with the raw materials having the lowest melting points placed on the heated surface of the melting vessel.
5. Applications of the multi-component alloys prepared by the methods of claims 1-2 and 3-4 in nuclear power plant environments and marine environments.
Citation Information
Patent Citations
High-entropy alloy resistant to marine microbiological corrosion and preparing method and application thereof
CN110760733A
Low thermal neutron absorption section type medium-entropy alloy with nanometer precipitated phase and preparation method thereof
CN113308635A