Light emitting diode chip and preparation method thereof

By designing a multi-quantum well structure in the light-emitting diode chip, blue light emission at four different peak wavelengths is achieved, solving the problems of excessive blue light and lack of green light in the white light spectrum in the existing technology, improving the color rendering index and lighting health .

CN118039759BActive Publication Date: 2024-11-22HUNAN XIANGNENG SEMICONDUCTOR TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410364112.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2024-11-22
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

The blue light peak in the white spectrum of existing light emitting diode chips is relatively strong, and the lack of green light parts is difficult to improve the color rendering index.

Method used

Design a light emitting diode chip, whose gallium nitride epitaxial sheet includes a multi-quantum well structure, and by alternately growing multiple quantum well layers, emitting four different peak values ​​of 465-475nm, 455-465nm, 445-455nm and 435-445nm respectively The blue light at wavelengths is adjusted to adjust the thickness and doping concentration of the quantum barrier to form a continuous 400-500nm luminescence spectrum.

Benefits of technology

Four peak wavelengths of luminescence in the range of 400-500nm are achieved, which disperses the blue light energy distribution, reduces the blue light luminous intensity in the spectrum, improves the color rendering index and fidelity, and is suitable for lighting health.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118039759B_ABST
    Figure CN118039759B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of semiconductor technology, and provides a light-emitting diode chip and a preparation method thereof. The light-emitting diode chip of the present invention includes a gallium nitride epitaxial wafer; the gallium nitride epitaxial wafer includes a sapphire substrate, a buffer layer, a UGaN layer, an N-type doped NGaN layer, a light-emitting layer, a P-type doped PGaN layer and an ohmic contact layer from bottom to top; the light-emitting layer can emit blue light of four different peak wavelengths, which is continuous within 400-500nm, and the relative luminous intensity is greatly reduced compared with the single-peak blue light; and by controlling the change of the four peak spacings and the luminous intensity, under the driving current density of 10A / cm2~100A / cm2, the difference of the main wavelength change does not exceed 3nm, and the half-wave width is greater than 30nm. The spectrum design of the present invention reduces the influence of the driving current density change on the light-emitting diode spectrum waveform, so that the spectrum has good stability relative to the driving current change; the white light spectrum of the lamp bead made of this light-emitting diode chip is similar to sunlight, which is conducive to improving the color rendering index Ra, saturation Rg and fidelity Rf.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a light emitting diode chip and a preparation method thereof. Background Art

[0002] In the prior art, the traditional light-emitting diode chip adopts the method of "a set of MQW produces a single peak". The traditional method first uses a metal organic chemical vapor deposition reaction chamber to grow a buffer layer, a UGaN layer, and a nGaN layer on a sapphire and SiO2 composite substrate in sequence. The buffer layer is a buffer layer, which is subdivided into two layers: the first layer is an AlN layer, and the second layer is AlGaN. The UGaN layer is an undoped GaN layer, which is subdivided into two layers: the first layer is a 3D layer mainly grown in a 3D manner, and the second layer is a 2D layer mainly grown in a 2D manner. The nGaN layer is an n-type GaN layer doped with Si, and the doping concentration is generally between 1.0E+19 and 3.0E+19. Then grow the SW layer (shallow well layer), which is subdivided into two layers, the SWW well and the SWB barrier: the SWW layer is an InGaN layer, and the SWB layer is a GaN layer. These two layers grow alternately and cycle 3-6 times. The InGaN layer here has a lower component, and the entire shallow well layer has the function of adjusting the lattice and stress, and stores a certain amount of electrons. Similarly, the next step is to grow HTMQW6 (high temperature well layer), which is subdivided into two layers: HTQW well and HTQB barrier: HTQW layer is InGaN layer, HTQB layer is GaN layer, these two layers are grown alternately, and the cycle is 3-6 times. The In component here is higher than that of the shallow well layer, and lower than that of the light-emitting area behind. The lattice and stress are adjusted again to store a certain amount of electrons. Then grow the quantum well light-emitting area 7, which is subdivided into two layers: QW well and QB barrier: QW well is InGaN layer, QB barrier is GaN layer. This part of the traditional LED epitaxial structure is formed by the alternating growth of QW layer and QB layer, and the cycle is 9-12 times.

[0003] However, using a single-peak blue LED chip to excite the phosphor to emit white light has a very sharp blue peak in the white light spectrum, and the cyan part is missing, so there are still the following major disadvantages:

[0004] ① The relative light intensity of the blue light peak in the white light spectrum is too strong, causing blue light damage and is not conducive to eye health;

[0005] ② The white light spectrum lacks the cyan part, which is very different from the solar spectrum;

[0006] ③The CRI is between 70-80 and it is difficult to reach above 95.

[0007] Therefore, it is necessary to provide a new light emitting diode chip and a preparation method thereof to solve the above problems existing in the prior art. Summary of the invention

[0008] The first object of the present invention is to provide a light emitting diode chip, and the specific technical solution is as follows:

[0009] A light-emitting diode chip, comprising a gallium nitride epitaxial wafer;

[0010] The GaN epitaxial wafer includes, from bottom to top, a sapphire substrate, a buffer layer, a UGaN layer, an N-type doped NGaN layer, a light-emitting layer, a P-type doped PGaN layer and an ohmic contact layer;

[0011] The light-emitting layer is used for emitting blue light with four different peak wavelengths.

[0012] Preferably, the light-emitting layer is a multi-quantum well structure, which includes a first quantum well layer, a second quantum well layer, a third quantum well layer and a fourth quantum well layer divided according to the light-emitting wavelength, and the first quantum well layer is arranged close to the P-type doped PGaN layer;

[0013] The fourth quantum well layer includes a plurality of fourth well barrier units, each of which includes a quantum well QW4 and a quantum barrier QB4, and its light emission peak wavelength is 465-475 nm, which is called the fourth peak wavelength;

[0014] The third quantum well layer includes a plurality of third well barrier units arranged on the fourth quantum well layer, each of which includes a quantum well QW3 and a quantum barrier QB3, and its light emission peak wavelength is 455-465nm, which is called the third peak wavelength;

[0015] The second quantum well layer includes a plurality of second well barrier units arranged on the third quantum well layer, each of the second well barrier units includes a quantum well QW2 and a quantum barrier QB2, and its emission peak wavelength is 445-455nm, which is called the second peak wavelength;

[0016] The first quantum well layer includes a plurality of first well barrier units arranged on the second quantum well layer, each of the first well barrier units includes a quantum well QW1 and a quantum barrier QB1, and its emission peak wavelength is 435-445nm, which is called the first peak wavelength;

[0017] The first peak wavelength luminescence intensity is between 0.8 and 1.2 times the second peak wavelength luminescence intensity; the third peak wavelength luminescence intensity is between 0.4 and 0.8 times the second peak wavelength luminescence intensity; the fourth peak wavelength luminescence intensity is between 0.3 and 0.8 times the second peak wavelength luminescence intensity.

[0018] Preferably, the fourth quantum well layer includes d groups of fourth well barrier units grown cyclically and alternately; the third quantum well layer includes c groups of third well barrier units grown cyclically and alternately; the second quantum well layer includes b groups of second well barrier units grown cyclically and alternately; the first quantum well layer includes a group of first well barrier units grown cyclically and alternately;

[0019] The number of cycles satisfies the following relationship: a ≥ m / 2, 1 ≤ b ≤ m / 3, 1 ≤ c ≤ m / 4, 1 ≤ d ≤ m / 4;

[0020] Where m is the total number of cycles of the four groups of quantum wells.

[0021] Preferably, the thickness of quantum barrier QB4 is d4, the thickness of quantum barrier QB3 is d3, the thickness of quantum barrier QB2 is d2, the thickness of quantum barrier QB1 is d1, and d4≥d3≥d2>d1.

[0022] Preferably, the concentration of Si doped with quantum barrier QB4 is C4, the concentration of Si doped with quantum barrier QB3 is C3, the concentration of Si doped with quantum barrier QB2 is C2, the concentration of Si doped with quantum barrier QB1 is C1, C4≤C3≤C2≤C1 and C1 / C4≤3.

[0023] Preferably, the range of C1 is 4.8 to 5.2E+17 atoms / cm 3 ; C2 range is 3.3~3.7E+17atoms / cm 3 ; C3 range is 2.0~2.6E+17atoms / cm 3 ; C4 range is 1.8~2.4E+17atoms / cm 3 ; The range of d1 is 7.5~8.5nm, the range of d2 is 8.5~10nm, the range of d3 is 9~10.5nm, and the range of d4 is 9.5~11nm.

[0024] Preferably, an LTP layer and an EBL layer grown in sequence are included between the light emitting layer and the P-type doped PGaN layer, the LTP layer is a low temperature grown Mg-doped P-type GaN layer; and the EBL layer is an electron blocking layer.

[0025] The present invention also provides a method for manufacturing the light emitting diode chip as described above, comprising the following steps:

[0026] Step 1: Using a metal organic chemical vapor deposition reaction chamber, a buffer layer, a UGaN layer and an N-type doped NGaN layer are sequentially grown on a sapphire and SiO2 composite substrate;

[0027] Step 2: Alternately grow SWW wells and SWB barriers on the N-type doped NGaN layer obtained in step 1, and cycle for 3-6 times to obtain a shallow well layer SW;

[0028] Step 3: Alternately grow HTQW wells and HTQB barriers on the shallow well layer SW, and cycle for 3-6 times to obtain a high-temperature well layer HTMQW;

[0029] Step 4: On the high-temperature well layer HTMQW, first grow a quantum well QW4, and then cover it with a quantum barrier QB4, the two grow alternately, the number of cycles is d, and the fourth quantum well layer is obtained, and its peak emission wavelength is 465-475nm, then grow a quantum well QW3 on the fourth quantum well layer, and then cover it with a quantum barrier QB3, the two grow alternately, the number of cycles is c, and the third quantum well layer is obtained, and its peak emission wavelength is 455-465nm; then grow a quantum well QW2 on the third quantum well layer, and cover it with a quantum barrier QB2, the two grow alternately, the number of cycles is b, and the second quantum well layer is obtained, and its peak emission wavelength is 445-455nm; finally, grow a quantum well QW1 on the second quantum well layer, and cover it with a quantum barrier QB1, the two grow alternately, the number of cycles is a, and the first quantum well layer is obtained, and its peak emission wavelength is 435-445nm;

[0030] The number of cycles also satisfies the following relationship: a≥m / 2, 1≤b≤m / 3, 1≤c≤m / 4, 1≤d≤m / 4, and a light-emitting layer having a total number of cycles of m is obtained;

[0031] Step 5: growing an LTP layer on the light-emitting layer, which is a low-temperature grown Mg-doped P-type GaN layer with a high doping concentration;

[0032] Step 6: Grow an EBL layer on the LTP layer. This layer is an electron blocking layer and is composed of AlGaN. The Al component is from high to low along the growth direction.

[0033] Step 7: growing a PGaN layer on the EBL layer, which is a Mg-doped GaN layer with a doping concentration between 1.0E+19 and 3.0E+20, for providing holes;

[0034] Step 8: Finally, grow the P++ layer, which is a GaN layer heavily doped with Mg, with a doping concentration between 4.0E+20 and 9.0E+20. This layer is an ohmic contact layer. At this point, the GaN epitaxial wafer is completed.

[0035] Step nine: Use the gallium nitride epitaxial wafer obtained in step eight to make a light-emitting diode chip.

[0036] Preferably, the emission peak wavelength range of each quantum well layer in step 4 is adjusted by changing the thickness of the quantum well and / or adjusting the temperature.

[0037] Preferably, in the step 4:

[0038] The thickness of quantum barrier QB4 is d4, the thickness of quantum barrier QB3 is d3, the thickness of quantum barrier QB2 is d2, the thickness of quantum barrier QB1 is d1, and d4≥d3≥d2>d1 is controlled;

[0039] The concentration of Si doped with quantum barrier QB4 is C4, the concentration of Si doped with quantum barrier QB3 is C3, the concentration of Si doped with quantum barrier QB2 is C2, and the concentration of Si doped with quantum barrier QB1 is C1. C4≤C3≤C2≤C1 and C1 / C4≤3 are controlled.

[0040] The application of the technical solution of the present invention has the following beneficial effects:

[0041] The light-emitting diode chip of the present invention has four obvious inflection points on the continuous luminous spectrum of 400-500nm under the driving current density of 10A / cm2 to 100A / cm2, corresponding to four peak wavelengths, the luminous intensity of the first peak wavelength is between 0.8 and 1.2 times of the luminous intensity of the second peak wavelength; the luminous intensity of the third peak wavelength is between 0.4 and 0.8 times of the luminous intensity of the second peak wavelength; the luminous intensity of the fourth peak wavelength is between 0.3 and 0.8 times of the luminous intensity of the second peak wavelength; with the change of current, the half width HW is greater than 30nm, and the difference of the main wavelength change does not exceed 3nm. The present invention divides the blue light part of the LED chip into 4 peaks, the energy distribution of the blue light part is dispersed, the luminous intensity of the blue light on the spectrum is greatly reduced, and it is continuous within 400-500nm, without lacking a certain section of light, and after exciting the phosphor, the entire white light spectrum is similar to sunlight, which is beneficial to improving the color rendering index Ra, saturation Rg and fidelity Rf, and is beneficial to lighting health.

[0042] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0044] Figure 1 is an electroluminescence spectrum diagram of the light-emitting diode chip of Example 1 of the present invention, wherein: Figure 1 (a) is the spectrum of y1=1.2y2; Figure 1 (b) is the spectrum diagram when y1=0.8y2;

[0045] Figure 2 It is a schematic diagram of the structure of a traditional light-emitting diode chip;

[0046] Figure 3 is a schematic diagram of a light emitting area of ​​a light emitting diode chip in Embodiment 1 of the present invention;

[0047] Figure 4 is a schematic diagram of a light emitting area of ​​a light emitting diode chip of Example 2;

[0048] Figure 5 is a schematic diagram of the light emitting area of ​​the light emitting diode chip of Example 3;

[0049] Figure 6 Schematic diagram of the light emitting area of ​​the light emitting diode chip of Example 4. DETAILED DESCRIPTION

[0050] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, but the present invention can be implemented in many different ways as defined and covered by the claims.

[0051] Embodiment 1:

[0052] This embodiment discloses a light-emitting diode chip, the light-emitting layer of the gallium nitride epitaxial wafer of which can emit blue light with four different peak wavelengths, and is manufactured by the following preparation method:

[0053] Step 1: Use a metal organic chemical vapor deposition reaction chamber to sequentially grow a buffer layer, a UGaN layer and an N-type doped NGaN layer on a sapphire and SiO2 composite substrate; the buffer layer of this embodiment includes an AlN layer and an AlGaN layer; the UGaN layer is an undoped GaN layer, including a 3D layer mainly grown in a 3D manner and a 2D layer mainly grown in a 2D manner; the NGaN layer is an N-type GaN layer doped with Si, and the doping concentration is generally between 1.0E+19 and 3.0E+19.

[0054] Step 2: Alternately grow SWW wells and SWB barriers on the N-type doped NGaN layer obtained in step 1, and cycle for 3-6 times to obtain a shallow well layer SW; in this embodiment, the SWW layer is an InGaN layer, and the SWB layer is a GaN layer; the InGaN layer here has a lower component, and the entire shallow well layer has the function of adjusting the lattice stress and stores a certain amount of electrons.

[0055] Step 3: Alternately grow HTQW wells and HTQB barriers on the shallow well layer SW, and cycle 3-6 times to obtain a high-temperature well layer HTMQW; in this embodiment, the HTQW layer is an InGaN layer, and the HTQB layer is a GaN layer. These two layers are grown alternately, and the In component here is higher than that of the shallow well layer and lower than that of the subsequent light-emitting area. The lattice and stress are adjusted again to store a certain amount of electrons.

[0056] Step 4: On the high-temperature well layer HTMQW, first grow a quantum well QW4, and then cover it with a quantum barrier QB4, the two grow alternately, the number of cycles is d, and the fourth quantum well layer is obtained, and its peak emission wavelength is 465-475nm; then grow a quantum well QW3 on the fourth quantum well layer, and then cover it with a quantum barrier QB3, the two grow alternately, the number of cycles is c, and the third quantum well layer is obtained, and its peak emission wavelength is 455-465nm; then grow a quantum well QW2 on the third quantum well layer, and cover it with a quantum barrier QB2, the two grow alternately, the number of cycles is b, and the second quantum well layer is obtained, and its peak emission wavelength is 445-455nm; finally, on the second A quantum well QW1 is grown on the quantum well layer, and a quantum barrier QB1 is covered thereon. The two grow alternately, and the number of cycles is a, to obtain a first quantum well layer, whose peak emission wavelength is 435-445 nm. In this embodiment, the corresponding wavelength range is adjusted by changing the thickness of the quantum well and / or adjusting the temperature; and the thickness of the quantum barrier QB4 is controlled to be ≥ the thickness of the quantum barrier QB3 ≥ the thickness of the quantum barrier QB2> the thickness of the quantum barrier QB1, and the concentration of doped Si in the quantum barrier QB4 is controlled to be ≤ the concentration of doped Si in the quantum barrier QB3 ≤ the concentration of doped Si in the quantum barrier QB2 ≤ the concentration of doped Si in the quantum barrier QB1, and the ratio of the maximum value to the minimum value of the concentration of doped Si is controlled to be within 3;

[0057] The number of cycles also satisfies the following relationship: a ≥ m / 2, 1 ≤ b ≤ m / 3, 1 ≤ c ≤ m / 4, 1 ≤ d ≤ m / 4, and a light-emitting layer with a total number of cycles of m is obtained, see Figure 3 .

[0058] Step 5: Grow an LTP layer on the light-emitting layer. This layer is a low-temperature grown Mg-doped P-type GaN layer with a high doping concentration. In this embodiment, between 8.0E+19 and 3.0E+20, the LTP layer is closest to the light-emitting area, which is conducive to providing holes and gathering holes nearby. In addition, the LTP layer is conducive to filling the V-shaped pits in the light-emitting area, and the surface of the grown layer is relatively rough, which is conducive to improving the light extraction efficiency.

[0059] Step 6: Grow an EBL layer on the LTP layer. This layer is an electron blocking layer and is composed of AlGaN. The Al component is from high to low along the growth direction; it is conducive to hole climbing and hole transmission is more efficient.

[0060] Step 7: Grow a PGaN layer on the EBL layer. This layer is a Mg-doped GaN layer with a doping concentration between 1.0E+19 and 3.0E+20, which is used to provide holes.

[0061] Step 8: Finally, grow the P++ layer, which is a GaN layer heavily doped with Mg, with a doping concentration between 4.0E+20 and 9.0E+20. This layer is an ohmic contact layer. At this point, the GaN epitaxial wafer is completed.

[0062] Step nine: Use the gallium nitride epitaxial wafer obtained in step eight to make a light-emitting diode chip.

[0063] The emission spectrum of the above LED chips has multiple peak inflection points, see Figure 1 ,in Figure 1 (a) is the spectrum of y1=1.2y2; Figure 1 (b) is a spectrum diagram of y1=0.8y2. In the electroluminescence spectrum diagram of the light-emitting diode chip of this embodiment, the horizontal axis represents the wavelength, and the vertical axis represents the relative light intensity. The first inflection point is recorded as (x1, y1), corresponding to the peak wavelength x1 of the first quantum well layer, and the relative light intensity y1 corresponding to the peak wavelength of the first quantum well layer; the second inflection point is recorded as (x2, y2), corresponding to the peak wavelength x2 of the second quantum well layer, and the relative light intensity y2 corresponding to the peak wavelength of the second quantum well layer; the third inflection point is recorded as (x3, y3), corresponding to the peak wavelength x3 of the third quantum well layer, and the relative light intensity y3 corresponding to the peak wavelength of the third quantum well layer; the fourth inflection point is recorded as (x4, y4), corresponding to the peak wavelength x4 of the fourth quantum well layer, and the relative light intensity y4 corresponding to the peak wavelength of the fourth quantum well layer; the above four groups of relative light intensities satisfy the following relationship: if y2=1.0, then 0.8≤y1≤1.2, 0.4≤y3≤0.8, 0.3≤y4≤0.8.

[0064] The light-emitting diode chip of this embodiment has four obvious inflection points on the continuous luminous spectrum of 400-500nm under the driving current density of 10A / cm2 to 100A / cm2, corresponding to four peak wavelengths, the luminous intensity of the first peak wavelength is between 0.8 and 1.2 times of the luminous intensity of the second peak wavelength; the luminous intensity of the third peak wavelength is between 0.4 and 0.8 times of the luminous intensity of the second peak wavelength; the luminous intensity of the fourth peak wavelength is between 0.3 and 0.8 times of the luminous intensity of the second peak wavelength. And with the change of current, the half width HW is greater than 30nm, and the difference of the main wavelength change does not exceed 3nm. The present invention divides the blue light part of the LED chip into 4 peaks, the energy distribution of the blue light part is dispersed, the luminous intensity of the blue light on the spectrum is greatly reduced, and it is continuous within 400-500nm, without missing a certain section of light. After exciting the phosphor, the entire white light spectrum is similar to sunlight, which is beneficial to improve the color rendering index Ra, saturation Rg and fidelity Rf, and is beneficial to lighting health.

[0065] Embodiment 2:

[0066] Based on Example 1, this embodiment adjusts the wavelength range corresponding to the light-emitting region by changing the thickness of the quantum well and / or adjusting the temperature, such as Figure 4 As shown, different light emitting diode chips are obtained.

[0067] In this embodiment, the growth temperature of QW4 and QW1 is the same, but the thickness of QW is different. The thickness setting value of QW4 is 3.6nm±5%, the thickness setting value of QW3 is 3.4nm±5%, the thickness setting value of QW2 is 3nm±5%, and the thickness setting value of QW1 is 2.6nm±5%. The thickness setting values ​​of QB4 and QB3 are 10nm±10%, the thickness setting value of QB2 is 9nm±10%, and the thickness setting value of QB1 is 8nm±10%. The number of cycles d=1, c=1, b=2, a=8, the WLP design value of QW4 is 470±5nm, the WLP design value of QW3 is 463±5nm, the WLP design value of QW2 is 450±5nm, and the WLP design value of QW1 is 437±5nm. In order to enhance the relative intensity of the fourth light beam, the cycle number d can be increased; in order to enhance the intensity of the third and second light beams, the cycle numbers c and b can be increased; similarly, in order to enhance / reduce the relative intensity of the first light beam, the cycle number a can be increased / decreased.

[0068] Embodiment 3:

[0069] Based on Example 1, this embodiment adjusts the wavelength range corresponding to the light-emitting region by changing the thickness of the quantum well and / or adjusting the temperature, such as Figure 5 As shown, different light emitting diode chips are obtained.

[0070] The thickness of QW4 is the same as that of QW1, but the growth temperature is different. The thickness of QW is uniformly 3nm. If the growth temperature of QW2 is recorded as T, and the range of T is between 750-780 degrees, then the temperature setting value of QW4 is T-9℃, the temperature setting value of QW3 is T-6℃, and the temperature setting value of QW1 is T+8℃. The thickness setting value of QB4 is 11nm±10%, the thickness setting value of QB3 is 10nm±10%, the thickness setting value of QB2 is 9nm±10%, and the thickness setting value of QB1 is 8nm±10%. The number of cycles d=1, c=1, b=3, a=7, the WLP design value of QW4 is 468±5nm, the WLP design value of QW3 is 462±5nm, the WLP design value of QW2 is 450±5nm, and the WLP design value of QW1 is 438±5nm. In order to enhance the relative intensity of the fourth light beam, the cycle number d can be increased; in order to enhance the intensity of the third and second light beams, the cycle numbers c and b can be increased; similarly, in order to enhance / reduce the relative intensity of the first light beam, the cycle number a can be increased / decreased.

[0071] Embodiment 4:

[0072] Based on Example 1, this embodiment adjusts the wavelength range corresponding to the light-emitting region by changing the thickness of the quantum well and / or adjusting the temperature, such as Figure 6 As shown, different light emitting diode chips are obtained.

[0073] The above QW thickness and growth temperature are used in combination. The thickness of QW4 is designed to be 3.6nm±5%, the thickness of QW3 is designed to be 3.4nm±5%, and the thickness of QW2 and QW1 is designed to be 3.0nm±5%; at the same time, the design temperature of QW4 / QW3 / QW2 is T, and the temperature setting value of QW1 is T+8℃; the number of cycles d=1, c=2, b=2, a=7, the WLP design value of QW4 is 470±5nm, the WLP design value of QW3 is 463±5nm, the WLP design value of QW2 is 450±5nm, and the WLP design value of QW1 is 438±5nm. In order to enhance the relative intensity of the fourth beam of light, the number of cycles d can be increased; in order to enhance the intensity of the third and second beams of light, the number of cycles c and b can be increased; similarly, in order to enhance / reduce the relative intensity of the first beam of light, the number of cycles a can be increased / decreased.

[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A light emitting diode chip, characterized in that: Including GaN epitaxial wafers; The GaN epitaxial wafer includes, from bottom to top, a sapphire substrate, a buffer layer, a UGaN layer, an N-type doped NGaN layer, a light-emitting layer, a P-type doped PGaN layer and an ohmic contact layer; The light-emitting layer is used to emit blue light with four different peak wavelengths; The light-emitting layer is a multi-quantum well structure, which includes a first quantum well layer, a second quantum well layer, a third quantum well layer and a fourth quantum well layer divided according to the light-emitting wavelength, and the first quantum well layer is arranged close to the P-type doped PGaN layer; The fourth quantum well layer includes a plurality of fourth well barrier units, each of which includes a quantum well QW4 and a quantum barrier QB4, and its light emission peak wavelength is 465-475 nm, which is called the fourth peak wavelength; The third quantum well layer includes a plurality of third well barrier units arranged on the fourth quantum well layer, each of the third well barrier units includes a quantum well QW3 and a quantum barrier QB3, and its emission peak wavelength is 455-465nm, which is called the third peak wavelength; The second quantum well layer includes a plurality of second well barrier units arranged on the third quantum well layer, each of the second well barrier units includes a quantum well QW2 and a quantum barrier QB2, and its emission peak wavelength is 445-455nm, which is called the second peak wavelength; The first quantum well layer includes a plurality of first well barrier units arranged on the second quantum well layer, each of the first well barrier units includes a quantum well QW1 and a quantum barrier QB1, and its emission peak wavelength is 435-445nm, which is called the first peak wavelength; The first peak wavelength luminous intensity is between 0.8 and 1.2 times the second peak wavelength luminous intensity; the third peak wavelength luminous intensity is between 0.4 and 0.8 times the second peak wavelength luminous intensity; the fourth peak wavelength luminous intensity is between 0.3 and 0.8 times the second peak wavelength luminous intensity; The fourth quantum well layer includes d groups of fourth well barrier units grown cyclically and alternately; the third quantum well layer includes c groups of third well barrier units grown cyclically and alternately; the second quantum well layer includes b groups of second well barrier units grown cyclically and alternately; the first quantum well layer includes a group of second well barrier units grown cyclically and alternately; The number of cycles satisfies the following relationship: a ≥ m / 2, 1 ≤ b ≤ m / 3, 1 ≤ c ≤ m / 4, 1 ≤ d ≤ m / 4; Where m is the total number of cycles of the four groups of quantum wells; The thickness of quantum barrier QB4 is d4, the thickness of quantum barrier QB3 is d3, the thickness of quantum barrier QB2 is d2, the thickness of quantum barrier QB1 is d1, d4≥d3≥d2>d1; The concentration of Si doped with quantum barrier QB4 is C4, the concentration of Si doped with quantum barrier QB3 is C3, the concentration of Si doped with quantum barrier QB2 is C2, the concentration of Si doped with quantum barrier QB1 is C1, C4≤C3≤C2≤C1 and C1 / C4≤3; The range of C1 is 4.8~5.2E+17atoms / cm3; the range of C2 is 3.3~3.7E+17atoms / cm3; the range of C3 is 2.0~2.6E+17atoms / cm3; the range of C4 is 1.8~2.4E+17atoms / cm3; The range of d1 is 7.5 to 8.5 nm, the range of d2 is 8.5 to 10 nm, the range of d3 is 9 to 10.5 nm, and the range of d4 is 9.5 to 11 nm.

2. The light emitting diode chip according to claim 1, characterized in that: An LTP layer and an EBL layer are sequentially grown between the light emitting layer and the P-type doped PGaN layer. The LTP layer is a P-type GaN layer doped with Mg grown at a low temperature. The EBL layer is an electron blocking layer.

3. A method for manufacturing a light emitting diode chip as claimed in any one of claims 1 to 2, characterized in that: The following steps are involved: Step 1: Using a metal organic chemical vapor deposition reaction chamber, a buffer layer, a UGaN layer and an N-type doped NGaN layer are sequentially grown on a sapphire and SiO2 composite substrate; Step 2: Alternately grow SWW wells and SWB barriers on the N-type doped NGaN layer obtained in step 1, and cycle for 3-6 times to obtain a shallow well layer SW; Step 3: Alternately grow HTQW wells and HTQB barriers on the shallow well layer SW, and cycle for 3-6 times to obtain a high-temperature well layer HTMQW; Step 4: On the high-temperature well layer HTMQW, first grow a quantum well QW4, and then cover it with a quantum barrier QB4, the two grow alternately, the number of cycles is d, and the fourth quantum well layer is obtained, and its peak emission wavelength is 465-475nm; then grow a quantum well QW3 on the fourth quantum well layer, and then cover it with a quantum barrier QB3, the two grow alternately, the number of cycles is c, and the third quantum well layer is obtained, and its peak emission wavelength is 455-465nm; then grow a quantum well QW2 on the third quantum well layer, and cover it with a quantum barrier QB2, the two grow alternately, the number of cycles is b, and the second quantum well layer is obtained, and its peak emission wavelength is 445-455nm; finally, grow a quantum well QW1 on the second quantum well layer, and cover it with a quantum barrier QB1, the two grow alternately, the number of cycles is a, and the first quantum well layer is obtained, and its peak emission wavelength is 435-445nm; The number of cycles also satisfies the following relationship: a≥m / 2, 1≤b≤m / 3, 1≤c≤m / 4, 1≤d≤m / 4, and a light-emitting layer having a total number of cycles of m is obtained; Step 5: growing an LTP layer on the light-emitting layer, which is a low-temperature grown Mg-doped P-type GaN layer; Step 6: Grow an EBL layer on the LTP layer. This layer is an electron blocking layer and is composed of AlGaN. The Al component is from high to low along the growth direction. Step 7: growing a PGaN layer on the EBL layer, which is a Mg-doped GaN layer with a doping concentration between 1.0E+19 and 3.0E+20, for providing holes; Step 8: Finally, grow the P++ layer, which is a GaN layer heavily doped with Mg, with a doping concentration between 4.0E+20 and 9.0E+20. This layer is an ohmic contact layer. At this point, the GaN epitaxial wafer is completed. Step nine: Use the gallium nitride epitaxial wafer obtained in step eight to make a light-emitting diode chip.

4. The method for preparing a light emitting diode chip according to claim 3, characterized in that: The luminescence peak wavelength range of each quantum well layer in step 4 is adjusted by changing the thickness of the quantum well and / or adjusting the temperature.

5. The method for preparing a light emitting diode chip according to claim 4, characterized in that: In the step 4: The thickness of quantum barrier QB4 is d4, the thickness of quantum barrier QB3 is d3, the thickness of quantum barrier QB2 is d2, and the thickness of quantum barrier QB1 is d1, and d4≥d3≥d2>d1 is controlled; The concentration of Si doped with quantum barrier QB4 is C4, the concentration of Si doped with quantum barrier QB3 is C3, the concentration of Si doped with quantum barrier QB2 is C2, and the concentration of Si doped with quantum barrier QB1 is C1. C4≤C3≤C2≤C1 and C1 / C4≤3 are controlled.