A heat treatment method for cast nickel-based heat-resistant alloys and its application
By using high-temperature solution treatment and aging treatment, the γ/Laves eutectic structure in nickel-based heat-resistant alloys is eliminated, and a disk-shaped precipitate phase is precipitated. This solves the problem of matching strength and plasticity of large-size nickel-based heat-resistant alloys at high temperatures, and meets the service requirements of ultra-supercritical power plants.
Patent Information
- Application Number
- CN202211395894.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-09
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-11-09
AI Technical Summary
Existing technologies struggle to effectively eliminate γ/Laves eutectic structures in large-size nickel-based heat-resistant alloy components, leading to reduced alloy plasticity and failing to meet the service requirements of ultra-supercritical power plants at 650-700℃.
High-temperature solution treatment and aging treatment were employed to eliminate the γ/Laves eutectic phase and precipitate Ni3Nb0.6Mo0.3Ti0.1 type disk-shaped precipitates with a size greater than 50 nm in the alloy, thereby optimizing the strength-ductility balance of the alloy.
It significantly improves the strength and plasticity of nickel-based heat-resistant alloys, meeting the service requirements of ultra-supercritical power plants at 650-700℃, and ensuring that the alloy has excellent performance at high temperatures.
Smart Images

Figure CN118048588B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of heat-resistant alloy hot working technology, and specifically relates to a heat treatment method and application of nickel-based casting alloys. Background Technology
[0002] The energy efficiency of thermal power generating units depends on two unit parameters: steam pressure and steam temperature. Improving these parameters can not only save a large amount of coal resources, but also significantly reduce the emissions of pollutants such as CO2, achieving energy conservation and emission reduction. This is an important way to realize the "dual carbon" strategy. Therefore, high-parameter, large-capacity ultra-supercritical power plants have become the next generation of units that countries around the world are focusing on developing.
[0003] Compared with the most advanced commercial 600℃-class ultra-supercritical power plants, the steam parameters of 650-700℃-class ultra-supercritical power plants are significantly increased, and the requirements for key high-temperature components are more stringent, such as the turbine cylinders, valve bodies, superheaters, reheaters, headers, and main steam pipelines in the boiler. The main requirements are: (1) thermal stability under ultra-long-term high-temperature service conditions; (2) extrapolated creep strength greater than 100MPa after 100,000 hours at 650-700℃; (3) steam oxidation corrosion layer thickness less than 1mm after 100,000 hours at 650-700℃; and (4) good processability. Under these service conditions, ferritic and austenitic heat-resistant steels can no longer meet the requirements for strength and corrosion resistance, and nickel-based heat-resistant alloys must be used.
[0004] Traditional nickel-based heat-resistant alloys are used in aero-engines, ground-based gas turbines, and other fields. Their castings are relatively small (typically a cast casing weighing 20-50 kg), allowing for vacuum smelting and casting. However, the hot-end components of ultra-supercritical power plants are much larger (typically a 12-ton cast turbine inner cylinder). Existing vacuum equipment cannot meet the requirements and is too costly, necessitating non-vacuum smelting and sand casting. Nickel-based heat-resistant alloys are characterized by multi-component and complex phase compositions. Non-vacuum smelting sand casting is often used when casting large-sized nickel-based heat-resistant alloy components. The nickel-based heat-resistant alloys prepared by this method differ from those produced by vacuum smelting and casting. The large size of the alloy results in a higher content of elements such as Si and Mn, leading to the easy formation of γ / Laves eutectic. The γ / Laves eutectic has a network structure, which significantly reduces the alloy's plasticity, failing to meet application requirements. At the same time, at high temperatures, intermetallic compounds, carbides, borides and other precipitation strengthening phases are easily precipitated. The morphology, type, size and distribution of the precipitated phases in the alloy need to be optimized through heat treatment process to achieve the best match between strength and plasticity and meet service requirements. Summary of the Invention
[0005] To address the problems existing in the prior art, the present invention aims to provide a heat treatment method and application for nickel-based casting alloys containing γ / Laves eutectic, which can effectively eliminate the γ / Laves eutectic structure and obtain a disk-shaped precipitated strengthening phase, while taking into account both strength and plasticity.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0007] A heat treatment method for cast nickel-based heat-resistant alloys includes the following steps:
[0008] (1) Take a cast nickel-based heat-resistant alloy as-cast component. The alloy composition by mass percentage is: C 0.01~0.1%, Cr 16~25%, Mo 8.02~10%, Nb 0.5~5.0%, Al 0.01~1.8%, Ti 0.01~1.0%, B 0.001~0.008%, Si 0.002~1.0%, Mn 0.001~1.0%, with the balance being Ni and unavoidable impurities. The as-cast component contains a γ / Laves eutectic phase.
[0009] (2) The casting is subjected to high-temperature solution treatment: the solution treatment temperature is 1100℃~1220℃, the solution treatment time is at least 0.5h, and the casting is air-cooled or water-quenched to room temperature to obtain a solution-treated casting.
[0010] In the heat treatment method for the cast nickel-based heat-resistant alloy, in step (1), the γ / Laves eutectic phase is distributed in the interdendritic space with an area fraction of 0.5-2.5%.
[0011] In the heat treatment method for cast nickel-based heat-resistant alloys, in step (2), preferably, the solution temperature range is 1150℃~1210℃, the solution time is at least 1h, and the casting is air-cooled or water-quenched to room temperature to obtain a solution-treated casting.
[0012] In the heat treatment method for the cast nickel-based heat-resistant alloy, in step (2), the composition is homogenized and the γ / Laves eutectic is eliminated by high-temperature solution treatment.
[0013] The heat treatment method for cast nickel-based heat-resistant alloys involves subjecting the solution-treated casting to high-temperature aging treatment: the aging temperature is 625℃~725℃, the aging time is at least 24 hours, and the casting is then air-cooled or water-quenched to room temperature to obtain the aged casting.
[0014] The aforementioned heat treatment method for cast nickel-based heat-resistant alloys involves high-temperature aging treatment to induce the precipitation of Ni3Nb particles with a size greater than 50 nm in the alloy γ matrix. 0.6 Mo 0.3 Ti 0.1 Disc-shaped precipitate phase.
[0015] The room temperature elongation and reduction of area of the obtained solution-treated castings shall not be less than 45%, and the room temperature yield strength of the aged castings shall not be less than 400 MPa.
[0016] An application of a heat treatment method for cast nickel-based heat-resistant alloys, which is used in the manufacture of heat-resistant alloys in the fields of thermal power plants, petrochemicals, or nuclear energy.
[0017] The heat treatment method is used in the manufacture of key components in ultra-supercritical power plants at 650–750℃.
[0018] The key components are cast parts that come into contact with high-temperature and high-pressure steam, such as turbine inner cylinders, valve bodies, or nozzles.
[0019] The casting blanks of the casting components weigh more than 5 tons and are produced by non-vacuum smelting and sand casting.
[0020] The beneficial effects of this invention are:
[0021] Typically, the area fraction of the γ / Laves eutectic phase in such castings is 0.5%–2.5%. In a typical composition of 0.5% Si–0.5% Mn, the area fraction is 1.7±0.3%. Based on the characteristics of precipitates in cast nickel-based heat-resistant alloys, appropriate solution treatment can achieve compositional homogenization and eliminate the γ / Laves eutectic phase while avoiding initial melting of the γ / Laves eutectic phase. After remelting the γ / Laves eutectic phase at high temperature and air-cooling or water-quenching to room temperature, the network structure in the alloy disappears, and the alloy's plasticity is improved. By performing appropriate aging treatment on the solution-treated castings, optimized precipitates can be obtained. Since the disk-shaped precipitates hinder the movement of dislocations, the yield strength of the alloy is significantly improved, giving the alloy both excellent strength and plasticity. Attached Figure Description
[0022] Figure 1 The microstructure of the cast nickel-based heat-resistant alloy component is shown in (a), where (a) is the microstructure and (b) is a magnified view of the microstructure in (a).
[0023] Figure 2 The solid solution microstructure of the cast nickel-based heat-resistant alloy parts used are as follows: (a) 1200℃ / 1h / water quenching; (b) 1250℃ / 1h / water quenching.
[0024] Figure 3 The precipitation kinetics curve (a) and morphological characteristics (b) of the disc-shaped precipitates during the aging process of the cast nickel-based heat-resistant alloy at 700℃ are shown. Detailed Implementation
[0025] The present invention will now be further described in conjunction with specific embodiments.
[0026] Example 1
[0027] A heat treatment method for cast nickel-based heat-resistant alloys includes the following steps:
[0028] 1) Take a cast nickel-based heat-resistant alloy with the following composition: C 0.051%, Cr 21.6%, Mo 9.39%, Nb 3.68%, Al 0.24%, Ti 0.2%, B 0.004%, Si 0.5%, Mn 0.49%, with the balance being Ni and unavoidable impurities;
[0029] 2) Perform high-temperature solution treatment on the casting: The solution treatment temperature is 1200℃, the solution treatment time is 1h, and the casting is water quenched (WQ) to room temperature to obtain a solution-treated casting.
[0030] The room temperature yield strength of the solution-treated casting is 304 MPa, and the elongation and reduction of area are 55% and 56%, respectively (Table 1).
[0031] Example 2
[0032] A heat treatment method for cast nickel-based heat-resistant alloys includes the following steps:
[0033] 1) Take a cast nickel-based heat-resistant alloy with the following composition: C 0.051%, Cr 21.6%, Mo 9.39%, Nb 3.68%, Al 0.24%, Ti 0.2%, B 0.004%, Si 0.5%, Mn 0.49%, with the balance being Ni and unavoidable impurities;
[0034] 2) Perform high-temperature solution treatment on the casting: The solution treatment temperature is 1150℃, the solution treatment time is 1h, and the casting is quenched in water to room temperature to obtain a solution-treated casting.
[0035] The room temperature yield strength of the solution-treated casting is 307 MPa, and the elongation and reduction of area are 53% and 49%, respectively (Table 1).
[0036] Example 3
[0037] A heat treatment method for cast nickel-based heat-resistant alloys includes the following steps:
[0038] 1) Take a cast nickel-based heat-resistant alloy with the following composition: C 0.051%, Cr 21.6%, Mo 9.39%, Nb 3.68%, Al 0.24%, Ti 0.2%, B 0.004%, Si 0.5%, Mn 0.49%, with the balance being Ni and unavoidable impurities;
[0039] 2) Perform high-temperature solution treatment on the casting: The solution treatment temperature is 1100℃, the solution treatment time is 0.5h, and the casting is air-cooled to room temperature to obtain a solution-treated casting.
[0040] The room temperature yield strength of the solution-treated casting is 325 MPa, and the elongation and reduction of area are 49% and 47%, respectively (Table 1).
[0041] Example 4
[0042] In this embodiment, the solution-treated casting from Example 1 was subjected to high-temperature aging treatment. The aging treatment regime was as follows: aging temperature 700℃, aging time 24h, air cooling (AC) to room temperature, to obtain an aged casting. The room temperature yield strength of the aged casting was 422MPa, and the elongation was 39% (Table 2).
[0043] Example 5
[0044] In this embodiment, the solution-treated casting from Example 1 was subjected to high-temperature aging treatment. The aging treatment regime was as follows: aging temperature 700℃, aging time 36h, water quenching to room temperature, to obtain an aged casting. The room temperature yield strength of the aged casting was 468MPa, and the elongation was 43% (Table 2).
[0045] Comparative Example 1
[0046] A heat treatment method for cast nickel-based heat-resistant alloys includes the following steps:
[0047] 1) Take a cast nickel-based heat-resistant alloy with the following composition: C 0.051%, Cr 21.6%, Mo 9.39%, Nb 3.68%, Al 0.24%, Ti 0.2%, B 0.004%, Si 0.5%, Mn 0.49%, with the balance being Ni and unavoidable impurities;
[0048] 2) Perform high-temperature solution treatment on the casting: The solution treatment temperature is 1250℃, the solution treatment time is 1h, and the casting is quenched in water to room temperature to obtain a solution-treated casting.
[0049] The room temperature yield strength of the solution-treated casting is 245 MPa, and the elongation and reduction of area are 15% and 17%, respectively. The solution temperature is significantly higher than the upper limit temperature of solution treatment, which leads to a significant reduction in plasticity (Table 1).
[0050] Comparative Example 2
[0051] A heat treatment method for cast nickel-based heat-resistant alloys includes the following steps:
[0052] 1) Take a cast nickel-based heat-resistant alloy with the following composition: C 0.051%, Cr 21.6%, Mo 9.39%, Nb 3.68%, Al 0.24%, Ti 0.2%, B 0.004%, Si 0.5%, Mn 0.49%, with the balance being Ni and unavoidable impurities;
[0053] 2) Perform high-temperature solution treatment on the casting: The solution treatment temperature is 1225℃, the solution treatment time is 1h, and the casting is quenched in water to room temperature to obtain a solution-treated casting.
[0054] The room temperature yield strength of the solution-treated casting is 290 MPa, and the elongation and reduction of area are 57% and 42%, respectively. The reduction of area is lower because the solution temperature is higher than the upper limit temperature of the solution treatment (Table 1).
[0055] Comparative Example 3
[0056] A heat treatment method for cast nickel-based heat-resistant alloys includes the following steps:
[0057] 1) Take a cast nickel-based heat-resistant alloy with the following composition: C 0.051%, Cr 21.6%, Mo 9.39%, Nb 3.68%, Al 0.24%, Ti 0.2%, B 0.004%, Si 0.5%, Mn 0.49%, with the balance being Ni and unavoidable impurities;
[0058] 2) Perform high-temperature solution treatment on the casting: The solution treatment temperature is 1050℃, the solution treatment time is 1h, and the casting is quenched in water to room temperature to obtain a solution-treated casting.
[0059] The room temperature yield strength of the solution-treated casting is 326 MPa, and the elongation and reduction of area are 41% and 41%, respectively. The solution temperature is lower than the lower limit of the solution treatment temperature, resulting in low elongation and reduction of area (Table 1).
[0060] Comparative Example 4
[0061] A heat treatment method for cast nickel-based heat-resistant alloys includes the following steps:
[0062] 1) Take a cast nickel-based heat-resistant alloy with the following composition: C 0.051%, Cr 21.6%, Mo 9.39%, Nb 3.68%, Al 0.24%, Ti 0.2%, B 0.004%, Si 0.5%, Mn 0.49%, with the balance being Ni and unavoidable impurities;
[0063] 2) Perform high-temperature solution treatment on the casting: The solution treatment temperature is 1050℃, the solution treatment time is 0.25h, and the casting is quenched in water to room temperature to obtain a solution-treated casting.
[0064] The room temperature yield strength of the solution-treated casting was 317 MPa, with elongation and reduction of area of 32% and 30%, respectively. The solution treatment temperature and time were both below the lower limit, resulting in a significant decrease in both elongation and reduction of area (Table 1).
[0065] Comparative Example 5
[0066] In this comparative example, the solution-treated casting from Example 1 was subjected to high-temperature aging treatment. The aging treatment regime was as follows: aging temperature 600℃, aging time 36h, air cooling to room temperature, to obtain an aged casting. The room temperature yield strength of the aged casting was 301MPa, and the elongation was 54%. The yield strength was lower because the aging temperature was below the lower limit (Table 2).
[0067] Comparative Example 6
[0068] In this comparative example, the solution-treated casting from Example 1 was subjected to high-temperature aging treatment. The aging treatment regime was as follows: aging temperature 700℃, aging time 12h, air cooling to room temperature, to obtain an aged casting. The room temperature yield strength of the aged casting was 355MPa, and the elongation was 53%. The aging time was lower than the lower limit, resulting in a lower yield strength (Table 2).
[0069] Comparative Example 7
[0070] In this comparative example, the solution-treated casting from Example 1 was subjected to high-temperature aging treatment. The aging treatment regime was as follows: aging temperature 750℃, aging time 8h, air cooling to room temperature, to obtain an aged casting. The room temperature yield strength of the aged casting was 304MPa, and the elongation was 51%. The aging temperature was higher than the upper limit of the aging temperature, resulting in a lower yield strength (Table 2).
[0071] Table 1 Effect of solution treatment on room temperature tensile properties of cast nickel-based heat-resistant alloys
[0072] Example Solution treatment conditions Yield strength / MPa Elongation / % Reduction of area / % Example 1 1200℃ / 1h / WQ 304 55 56 Example 2 1150℃ / 1h / WQ 307 53 49 Example 3 1100℃ / 0.5h / AC 325 49 47 Comparative Example 1 1250℃ / 1h / WQ 245 15 17 Comparative Example 2 1225℃ / 1h / WQ 290 57 42 Comparative Example 3 1050℃ / 1h / WQ 326 41 41 Comparative Example 4 1050℃ / 0.25h / WQ 317 32 30
[0073] Table 2 Effect of aging treatment on room temperature tensile properties of cast nickel-based heat-resistant alloys (solution treatment regime: 1200℃ / 1h / WQ)
[0074]
[0075]
[0076] like Figure 1 As shown, the cast nickel-based heat-resistant alloy components exhibit significant dendritic segregation under as-cast conditions (the presence of dendritic structures indicates the existence of dendritic segregation), and a large amount of γ / Laves eutectic exists between the dendrites, with an area fraction of 1.7 ± 0.3%. Numerous dislocations tend to accumulate at the γ / Laves eutectic boundaries, reducing the coordination during alloy deformation, leading to uneven deformation, stress concentration, and the γ / Laves eutectic becoming a crack initiation source, thus reducing the alloy's plasticity. Figure 2It can be seen that Example 1 effectively eliminated the γ / Laves eutectic and dendritic structures by solution treatment at 1200℃ for 1 hour, and the plasticity of the alloy was significantly improved. However, Comparative Example 1 used solution treatment at 1250℃. The excessively high solution treatment temperature caused the initial melting of the γ / Laves eutectic and grain boundaries, resulting in a significant reduction in strength and plasticity. The excessively low solution temperature and short solution time of Comparative Examples 3 and 4 could not effectively eliminate the γ / Laves eutectic, resulting in poor plasticity.
[0077] like Figure 3 As shown, solution-treated cast nickel-based heat-resistant alloy parts can precipitate disc-shaped strengthening phases after high-temperature aging, and their size increases with time. Figure 3 a, where d0 and d are the lengths of the long side of the disk-shaped precipitate at aging time t (unaged and aged time t, respectively). The disk-shaped precipitate can effectively hinder dislocation movement and improve the alloy strength. Furthermore, its strengthening effect increases with size. Examples 4 and 5 show a significant increase in room temperature yield strength compared to the solution state (Example 1) by aging at 700℃ to induce the formation of disk-shaped precipitates. However, in Comparative Example 5, the aging temperature is below the required lower limit, and in Comparative Example 6, the aging time is also below the required lower limit. The disk-shaped precipitate size is small, resulting in insufficient strengthening effect and thus lower strength than required. In Comparative Example 7, the aging temperature is above the upper limit, making it easier to precipitate harmful needle-like δ-phase, thus resulting in lower strengthening.
[0078] The results of the examples and comparative examples show that, based on the differences in phase precipitation and dissolution behavior in alloys, the present invention selects appropriate solid solution and aging treatment parameters, effectively eliminates γ / Laves eutectic and homogenizes the composition during high-temperature solid solution treatment, and precipitates disc-shaped precipitates with significant strengthening effect during high-temperature aging. This can significantly improve the strength of cast parts while ensuring plasticity and guarantee their safe use.
[0079] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A heat treatment method for cast nickel-based heat-resistant alloys, characterized in that, Includes the following steps: (1) Take a cast nickel-based heat-resistant alloy as-cast component. The alloy composition by mass percentage is: C 0.01~0.1%, Cr 16~25%, Mo 8.02~10%, Nb 0.5~5.0%, Al 0.01~1.8%, Ti 0.01~1.0%, B 0.001~0.008%, Si 0.5~1.0%, Mn 0.001~1.0%, with the balance being Ni and unavoidable impurities. The as-cast component contains a γ / Laves eutectic phase; the γ / Laves eutectic phase is distributed between dendrites, with an area fraction of 0.5~2.5%. (2) The casting is subjected to high-temperature solution treatment: the solution treatment temperature is 1100℃~1200℃, the solution treatment time is at least 1h, and the casting is air-cooled or water-quenched to room temperature to obtain a solution-treated casting; the solution treatment homogenizes the alloy composition and eliminates the γ / Laves eutectic phase; (3) The solution-treated casting is subjected to high-temperature aging treatment: the aging temperature is 625℃~725℃, the aging time is at least 24h, and the casting is air-cooled or water-quenched to room temperature to obtain the aged casting; the γ matrix in the aged casting contains a disk-shaped precipitate phase with a size of not less than 50nm; The room temperature elongation and reduction of area of the obtained solution-treated castings shall not be less than 45%, and the room temperature yield strength of the aged castings shall not be less than 400 MPa. The heat treatment method is used to manufacture key components in ultra-supercritical power plants at 650~750℃; the key components are cast components that come into contact with high-temperature and high-pressure steam; the casting blanks of the cast components weigh more than 5 tons and are produced by non-vacuum smelting and sand casting.
2. The heat treatment method for cast nickel-based heat-resistant alloys according to claim 1, characterized in that, This heat treatment method is applied to the manufacture of heat-resistant alloys in the fields of thermal power plants, petrochemicals, or nuclear energy.
Citation Information
Patent Citations
Ni base alloy and its manufacture
JP1987167839A