A method for constructing an anode furnace

By designing and planning, and conducting multiple furnace operations, combined with the phased construction of various refractory materials, the problem of imperfect anode furnace construction process was solved, achieving stability of furnace temperature and equipment durability, and increasing production capacity.

CN118066873BActive Publication Date: 2026-11-17铜陵有色金属集团股份有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410023035.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-05
Publication Date
2026-11-17
Estimated Expiration
2044-01-05

AI Technical Summary

Technical Problem

The existing anode furnace lining process is imperfect, resulting in reduced overall stability and difficulty in ensuring stable internal temperature. The furnace lining is easily damaged by the mechanical scouring and erosion of high-temperature melt, affecting production capacity.

Method used

Through design planning and multiple furnace operations, combined with the phased construction of various refractory materials, the stability of the base is ensured. Asbestos boards and reinforcing boards are laid inside the furnace to enhance the stability of the refractory materials, control the thickness and gaps of brick joints and mortar, and optimize the construction of the furnace mouth and water channels.

Benefits of technology

It improves the stability of furnace temperature, reduces the erosion of slag and quartz flux, reduces mechanical collisions and wear, extends the service life of equipment, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses an anode furnace lining process method in the field of high-temperature smelting equipment technology. The method includes the following steps: Step 1: Design and planning: Draw a design drawing according to the required size of the anode furnace to confirm the final lining area; This anode furnace lining process method plans and pre-levels the lining environment to make the base more stable, and combines multiple furnace entry operations to lay the refractory material in batches. After the main refractory material of the furnace lining is successfully laid, the furnace temperature is stabilized, allowing the furnace lining to withstand the intense mechanical scouring of higher temperature melts during the blowing process, reducing the degree of slag and quartz flux erosion, stabilizing the furnace temperature periodically, reducing the disadvantages of mechanical collision and easy wear during furnace mouth cleaning and oxidation-reduction port maintenance, optimizing operating conditions, reducing the later maintenance cycle, and effectively improving production capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention discloses a method for constructing an anode furnace, specifically in the field of high-temperature smelting equipment technology. Background Technology

[0002] As a production equipment that requires auxiliary heating, the oxygen combustion technology of the anode furnace has obvious advantages in terms of environmental protection and economy compared with the traditional combustion air combustion.

[0003] 90% of the world's copper smelting capacity comes from pyrometallurgical processes. However, the pyrometallurgical copper refining process has always suffered from problems such as large amounts of smelting waste gas, high energy consumption, and low reaction efficiency. This is mainly because the combustion system uses traditional ambient temperature, high-volume combustion fuels (such as natural gas or heavy oil), resulting in significant heat loss due to the large amount of carbon oxides and nitrogen oxides in the flue gas. Furthermore, heavy oil has high viscosity, high impurities, poor atomization, incomplete combustion, and high fuel consumption. In addition, the rotary anode furnace itself has relatively weak reaction kinetics, leading to a long operating cycle.

[0004] The anode roasting furnace is one of the most important pieces of equipment in the anode roasting process, and also the most expensive. It is constructed from various types of refractory materials, with the most crucial component being the feed box structure formed by the fire channel walls and transverse walls. Anode carbon blocks are sequentially and vertically loaded into the feed box, and fuel is injected into the fire channel for combustion. The highest flue gas temperature in the fire channel is 1150℃~1200℃, with a heating curve of 150h~200h. The entire roasting system is divided into a preheating zone, a heating zone, and a cooling zone. During each roasting cycle, the refractory material undergoes temperature changes from low to high and back again, placing increasingly stringent demands on its performance.

[0005] A good furnace construction requires strict adherence to furnace construction regulations and requirements, and must conform to the design drawings; brick joints must be uniform, especially the joints in the fire channel walls, to ensure even overflow of volatile organic compounds from the charcoal blocks; expansion joints must be provided according to design requirements, their location and structure must be accurate, their width should not have negative tolerances, and the joints must be tightly filled with refractory fiber products and free of other debris; ensure the mortar is full, thereby enhancing the overall strength of the roasting furnace and reducing the overall air leakage coefficient; the aluminosilicate refractory fiber products and insulation fiber products must be tightly sealed, and the furnace wall inclination must be within a reasonable range.

[0006] The current anode furnaces suffer from imperfect construction processes and lack environmental compatibility, which is equivalent to not having a solid foundation and reducing overall stability. Secondly, after the refractory materials are laid in a conventional manner, it is difficult to ensure stable internal temperature. The furnace lining is also unable to withstand the intense mechanical erosion of the high-temperature melt during the blowing process. When slag and quartz solvent erode the furnace, the furnace temperature stability decreases. Furthermore, the drawbacks of mechanical collision and wear during furnace mouth cleaning and oxidation-reduction port maintenance will inevitably lead to the deterioration of working conditions, and short maintenance cycles also reduce production capacity. Summary of the Invention

[0007] The purpose of this invention is to provide an anode furnace lining method to address the problems mentioned in the background art. These problems include imperfect lining processes, lack of environmental compatibility, and a lack of solid foundation, leading to reduced overall stability. Furthermore, conventional refractory lining methods make it difficult to maintain internal temperature stability, and the furnace lining cannot withstand the intense mechanical erosion of the high-temperature melt during the blowing process. Erosion by slag and quartz solvent further reduces furnace temperature stability. Additionally, mechanical collisions and wear during furnace mouth cleaning and oxidation-reduction port maintenance inevitably worsen working conditions, and short maintenance cycles reduce production capacity.

[0008] To achieve the above objectives, the present invention provides the following technical solution: a method for constructing an anode furnace, comprising the following steps:

[0009] Step 1: Design Planning: Draw design drawings according to the required size of the anode furnace to confirm the final masonry area;

[0010] Step Two: Material Confirmation: This includes material preparation, material inspection, and site leveling;

[0011] Material preparation: Select asbestos boards, clay bricks, wall bricks, furnace bricks, strip bricks, magnesia-chrome bricks, magnesia-chrome mortar, cardboard, threaded rods, copper-coated bricks, and reinforcing plates;

[0012] Material inspection: Check whether each material conforms to the thickness, length, and width drawn in the design drawings, and whether it meets the qualification standards;

[0013] Site leveling: Remove soil and debris from the masonry location, and use quicklime to draw the edge of the masonry area according to the drawings to determine the masonry area. Dig a pit 0.2m to 0.5m deep within the area, fill it with interlaced steel bars, and pour concrete to fill two-thirds of the pit. After 24H to 48H, backfill with soil, level and compact it, and then place and fix the furnace body.

[0014] Step 3: One-time furnace loading operation;

[0015] Specifically:

[0016] When personnel enter the furnace, they first lay asbestos boards, which are 3mm to 5mm thick, 1m to 1.5m long, and 1m to 1.5m wide. Six to nine boards are laid in one layer, and five to eight layers are laid in total.

[0017] Lay clay bricks with a thickness of 4cm to 6.5cm, a length of 15cm to 23cm, and a width of 8cm to 11.4cm. Lay 45 to 52 bricks per layer and build 65 to 72 layers. Use clay mortar for the bricklaying and control the brick joints to be 1.5mm to 1.7mm. Lay the first layer of bricks with a line in mind and use a spirit level to find the center first.

[0018] Next, lay the wall bricks, with a thickness of 7.5cm to 9cm, a length of 40cm to 45.46cm, and a width of 25cm to 37.2cm. Lay 45 to 60 bricks at each end. When laying the bricks, the workers should control the angle of the bricks and set up stiffening slabs. The angle of the bricks and the stiffening slabs should be kept on the same plane.

[0019] Then, the furnace body bricks are laid, with a thickness of 6cm to 8.03cm, a length of 35cm to 45cm, and a width of 10cm to 15cm. 3 to 5 layers are laid, with joints in the middle of each layer. The joint bricks are 8cm to 10cm thick and laid with magnesium mortar. Three bricks are laid with a small piece of cardboard, and every seven layers are laid with a large piece of cardboard. The mortar joints are kept within 1mm to 2mm. The bricks are laid with a guide line to ensure that the brick surface is flat and the bricks are in a straight line. There are 65 to 80 bricks per layer. The gaps at the joints of the end walls are controlled and the reinforcing plates are covered.

[0020] Step 4: Secondary furnace loading operation;

[0021] Specific location:

[0022] Workers enter the furnace to clean the mud from yesterday's surface of the bricks. The laborers carry the bricks into the furnace, and the senior workers begin to lay the bricks. They lay electrofused magnesia-chrome bricks with a thickness of 6cm to 8.03cm, a length of 35cm to 45cm, and a width of 10cm to 15cm, laying 25 to 35 layers.

[0023] Lay electrofused rebonded magnesia-chrome bricks, 6cm-8.03cm thick, 30cm-45cm long, and 12cm-15cm wide, in 22-30 layers. At the 30th-32nd brick of the furnace body on the east side, lay copper-exit bricks, 10cm-15cm thick, 45.2cm long, and 20.26-24.9cm wide. Process strip bricks about 10cm long on both sides of the copper-exit, and use J-8 bricks at the top and bottom, with a height of 7.5cm thick, 38cm long, and 18-20cm wide.

[0024] Lay electrofused magnesia-chrome bricks, 6cm-8.03cm thick, 30cm-45cm long, and 10cm-15cm wide, in 12-14 layers. Then, install threaded rods, 12-14 rods per row, 70cm-80cm long. First, lay asbestos boards, 3mm-5mm thick, 1m-1.5m long and 1m-1.5m wide, 6-9 boards per layer, for four layers. Then, lay clay bricks, 5cm-6.5cm thick, 13cm-23cm long, and 8cm-11.4cm wide, 40-52 bricks per layer, for 15-20 layers.

[0025] Step 5: Brick transportation and construction;

[0026] Specifically:

[0027] Organize personnel to transport bricks into the furnace. Before rotating the furnace, personnel inside the furnace must be evacuated. Construction can only begin after the furnace has been rotated to the correct angle and safety has been confirmed. Personnel enter the furnace to lay bricks, with a thickness of 6cm to 8.03cm, a length of 25cm to 38cm, and a width of 10cm to 15cm, in 8 to 10 layers.

[0028] Lay two layers of asbestos board, then lay 15 to 20 layers of bricks, with 30 to 40 bricks on each side, for a total of 25 to 30 layers;

[0029] Step Six: Converter Inspection;

[0030] Specifically:

[0031] Once the furnace is rotated to the rear opening, the scaffolders are contacted to secure the platform behind the furnace. Before entering the furnace, personnel must check the lead screw and confirm that the furnace is safe. Then, the furnace body bricks are laid. When the furnace opening is 35cm to 50cm below the opening, bricks are laid to match the furnace opening position. During the laying process, the gaps between the bricks and the water channels are tamped with large pieces of material to prevent molten copper from entering.

[0032] The furnace opening is constructed by using bricks to cover the water channels on both sides. The bricks are 6cm to 10cm thick, 25 to 38cm long, and 20cm to 30cm wide.

[0033] The furnace body on both sides is built, and the height of the brickwork is the middle position between the furnace opening and the water channel. Pressure plates are welded on, and a second set of threaded rods is installed. There are a total of 12 to 16 threaded rods to ensure that the threaded rods are on the same plane and to tighten the threaded rods.

[0034] Turn the furnace opening to the front furnace opening position and keep it level. Check the inside of the furnace and only proceed with construction after confirming safety. Clean the inside of the furnace. The welder cuts the pressure plate and lays asbestos board. Then lay clay bricks to restore the copper fitting height to the intersection position. The intersection is built with processed bricks. The furnace opening water channel is wrapped. The gaps are tamped with large material. The small gaps at the furnace opening intersection are filled with magnesium mud. The closing bricks are driven in with a sledgehammer.

[0035] Step 7: Finishing touches;

[0036] Specific location:

[0037] Personnel first enter the furnace to clean the furnace, then lay the end wall bricks, 7.5cm-8cm thick, 30cm-45cm long, and 15cm-16cm wide. The first layer is leveled, and the bricks are tamped tightly with large pieces of material between them and the furnace body steel shell. Each layer is tamped and then laid, and the flue bricks are wrapped.

[0038] When building the end wall, a platform should be built. Pay attention to the gaps around the bricks of the end wall and ensure that the magnesia mortar is full. The finishing bricks should be measured in advance.

[0039] Preferably, the anode furnace includes a cylinder, end caps, oxidation-reduction port, copper port, furnace opening, dilute oxygen burner port, flue gas port, flue gas pipe, and furnace opening cover, and the cylinder has a diameter of 65mm to 80mm.

[0040] Preferably, the end caps on both sides of the furnace body are 325mm to 425mm in size and are bonded with magnesia-chrome bricks at intervals.

[0041] Preferably, the oxidation-reduction port includes an eyelet brick, the eyelet brick is 350mm to 450mm in size, and 1 to 3 eyelet bricks are provided, of which 1 to 2 are perforated.

[0042] Preferably, the copper-fitted bricks are 350mm to 450mm in size, and 1 to 3 copper-fitted bricks are provided, all of which are perforated.

[0043] Preferably, the rarefied oxygen burner nozzle area is made of magnesium-chromium castable.

[0044] Preferably, a 5mm to 10mm aluminum silicate fiberboard is installed on the smoke exhaust port and the smoke exhaust pipe.

[0045] Compared with the prior art, the beneficial effects of the present invention are as follows: This anode furnace lining process method plans and pre-levels the lining environment to make the base more stable. Combined with multiple furnace entry operations, the refractory material is laid in batches. After the main refractory material of the furnace lining is successfully laid, the furnace temperature is stabilized. This allows the furnace lining to withstand the intense mechanical erosion of the high-temperature melt during the blowing process, reducing the degree of slag and quartz flux erosion. It also makes the furnace temperature periodically stable, reducing the disadvantages of mechanical collision and easy wear during furnace mouth cleaning and oxidation-reduction port maintenance. This optimizes the working conditions, reduces the cycle of later maintenance, and effectively improves production capacity. Detailed Implementation

[0046] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," and "counterclockwise," etc., indicate the orientation or positional relationship based on the context, and are only for the convenience of describing this invention and simplifying the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention.

[0047] In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified.

[0048] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installed," "equipped with," "sleeved / connected," "connected," etc., should be interpreted broadly. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be a connection within two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0049] This invention provides a technical solution that plans and pre-levels the refractory environment to make the base more stable. Combined with multiple furnace-entry operations, the refractory material is laid in batches. This ensures stable furnace temperature after the main refractory material of the furnace lining is successfully laid, allowing the lining to withstand the intense mechanical erosion of the high-temperature melt during blowing. This reduces the degree of slag and quartz flux erosion, stabilizes the furnace temperature periodically, and reduces the drawbacks of mechanical collisions and easy wear during furnace mouth cleaning and oxidation-reduction port maintenance. This optimizes operating conditions, shortens the later maintenance cycle, and effectively improves production capacity. Specifically, it is a method for lining an anode furnace, and the steps of this method are as follows:

[0050] Step 1: Design Planning: Draw design drawings according to the required size of the anode furnace to confirm the final masonry area;

[0051] Step Two: Material Confirmation: This includes material preparation, material inspection, and site leveling;

[0052] Material preparation: Select asbestos boards, clay bricks, wall bricks, furnace bricks, strip bricks, magnesia-chrome bricks, magnesia-chrome mortar, cardboard, threaded rods, copper-coated bricks, and reinforcing plates;

[0053] Material inspection: Check whether each material conforms to the thickness, length, and width drawn in the design drawings, and whether it meets the qualification standards;

[0054] Site leveling: Remove soil and debris from the masonry location, and use quicklime to draw the edge of the masonry area according to the drawings to determine the masonry area. Dig a 0.2m pit within the area, fill it with interlaced steel bars, and pour concrete to fill two-thirds of the pit. After 24 hours, backfill with soil, level and compact it, and then place and fix the furnace body.

[0055] Step 3: One-time furnace loading operation;

[0056] Specifically:

[0057] Personnel enter the furnace and first lay asbestos boards, 3mm thick, 1m long and 1m wide, with 6 boards laid per layer, for a total of 5 layers;

[0058] Lay out clay bricks, 4cm thick, 15cm long, and 8cm wide, 45 bricks per layer, for a total of 65 layers. Use clay mortar for the bricklaying, and control the brick joints to be 1.5mm. Lay the first layer of bricks along a line, and use a spirit level to find the center first.

[0059] Next, lay the wall bricks, 7.5cm thick, 40cm long, and 25cm wide, with 45 bricks at each end. When laying the bricks, the workers should control the angle of the bricks and set up stiffening ribs. The angle of the bricks and the stiffening ribs should be kept on the same plane.

[0060] Then, the furnace body bricks are laid, 6cm thick, 35cm long, and 10cm wide, in 3 layers, with each layer having a joint in the middle. The joint bricks are 8cm thick and laid with magnesium mortar. Three bricks are laid with a small piece of cardboard, and every seven layers are laid with a large piece of cardboard. The mortar joints are kept within 1mm. The bricks are laid with a guide line to ensure that the brick plane is flat and the bricks are in a straight line. There are 65 bricks per layer. The gaps at the joints of the end walls are controlled and the reinforcing plates are covered.

[0061] Step 4: Secondary furnace loading operation;

[0062] Specific location:

[0063] Workers enter the furnace to clean the mud from yesterday's brick surface. The laborers transport the bricks into the furnace, and the senior workers begin to lay the bricks. They lay electrofused and bonded magnesia-chrome bricks, 6cm thick, 35cm long, and 10cm wide, and 25 layers thick, 30cm long, and 10cm wide.

[0064] Lay out 6cm thick, 30cm long and 12cm wide electrofused magnesia-chrome bricks, 22 layers in total. At the 30th brick of the furnace body on the east side, lay out copper-exit bricks, 10cm thick, 45.2cm long and 20.26cm wide. Process strip bricks about 10cm long on both sides of the copper-exit. Use J-8 bricks at the top and bottom, with a height of 7.5cm thick, 38cm long and 18cm wide.

[0065] Lay electrofused magnesia-chrome bricks, 6cm thick, 30cm long, and 10cm wide, in 12 layers. Workers then begin installing threaded rods, 12 in a row, 70cm long each. First, lay asbestos boards, 3mm thick, 1m long and 1m wide, 6 boards per layer, for 4 layers. Then, lay clay bricks, 5cm thick, 13cm long and 8cm wide, 40 bricks per layer, for 15 layers.

[0066] Step 5: Brick transportation and construction;

[0067] Specifically:

[0068] Organize personnel to transport bricks into the furnace. Before rotating the furnace, personnel inside the furnace must evacuate. Construction can only begin after the furnace has been rotated to the correct angle and safety has been confirmed. Personnel enter the furnace to lay bricks, which are 6cm thick, 25cm long, and 10cm wide, and are laid in 8 layers.

[0069] Lay two layers of asbestos board, then lay 15 layers of bricks, 30 bricks on each side, for a total of 25 layers;

[0070] Step Six: Converter Inspection;

[0071] Specifically:

[0072] Once the furnace is rotated to the rear opening, the scaffolders are contacted to secure the platform behind the furnace. Before entering the furnace, personnel must check the lead screw and confirm that the furnace is safe. Then, the furnace body bricks are laid. When the furnace opening is 35cm below the opening, bricks are laid to match the furnace opening position. During the laying process, the gaps between the bricks and the water channels are tamped with large pieces of material to prevent molten copper from entering.

[0073] The furnace opening is constructed by using bricks to cover the water channels on both sides of the furnace opening. The bricks are 6cm thick, 25cm long, and 20cm wide.

[0074] The furnace body on both sides is built with bricks at the middle position between the furnace opening and the water channel. Pressure plates are welded on, and a second set of 12 threaded rods are installed to ensure that the threaded rods are on the same plane and to tighten the threaded rods.

[0075] Turn the furnace opening to the front furnace opening position and keep it level. Check the inside of the furnace and only proceed with construction after confirming safety. Clean the inside of the furnace. The welder cuts the pressure plate and lays asbestos board. Then lay clay bricks to restore the copper fitting height to the intersection position. The intersection is built with processed bricks. The furnace opening water channel is wrapped. The gaps are tamped with large material. The small gaps at the furnace opening intersection are filled with magnesium mud. The closing bricks are driven in with a sledgehammer.

[0076] Step 7: Finishing touches;

[0077] Specific location:

[0078] Personnel first entered the furnace to clean the furnace, then laid the end wall bricks, 7.5cm thick, 30cm long and 15cm wide, for the first layer to level the surface. The bricks were then tamped tightly with large pieces of material between them and the furnace steel shell. Each layer was tamped before the flue bricks were wrapped.

[0079] When building the end wall, a platform should be built. Pay attention to the gaps around the bricks of the end wall and ensure that the magnesia mortar is full. The finishing bricks should be measured in advance.

[0080] The anode furnace includes a cylinder, end caps, oxidation-reduction inlet, copper inlet, furnace opening, dilute oxygen burner inlet, flue gas outlet, flue gas pipe, and furnace opening cover. The cylinder is 65mm in diameter, the end caps on both sides of the furnace are 325mm in diameter, and are combined with magnesia-chrome bricks in an intermittent manner. The oxidation-reduction inlet includes an eyelet brick, which is 350mm in diameter and is provided in one piece, one of which is perforated. The copper inlet brick is 350mm in diameter and is provided in one piece, both of which are perforated. The dilute oxygen burner inlet area is made of magnesia-chrome castable material. The flue gas outlet and flue gas pipe are covered with 5mm aluminum silicate fiberboard.

[0081] Example 1

[0082] A method for constructing an anode furnace, comprising the following steps:

[0083] Step 1: Design Planning: Draw design drawings according to the required size of the anode furnace to confirm the final masonry area;

[0084] Step Two: Material Confirmation: This includes material preparation, material inspection, and site leveling;

[0085] Material preparation: Select asbestos boards, clay bricks, wall bricks, furnace bricks, strip bricks, magnesia-chrome bricks, magnesia-chrome mortar, cardboard, threaded rods, copper-coated bricks, and reinforcing plates;

[0086] Material inspection: Check whether each material conforms to the thickness, length, and width drawn in the design drawings, and whether it meets the qualification standards;

[0087] Site leveling: Remove soil and debris from the masonry location, and use quicklime to draw the edge of the masonry area according to the drawings to determine the masonry area. Dig a 0.5m pit within the area, fill it with interlaced steel bars, and pour concrete to fill two-thirds of the pit. After 48 hours, backfill with soil, level and compact it, and place and fix the furnace body.

[0088] Step 3: One-time furnace loading operation;

[0089] Specifically:

[0090] Personnel enter the furnace and first lay asbestos boards, 5mm thick, 1.5m long and 1.5m wide, with 9 boards laid per layer, for a total of 8 layers;

[0091] Lay out clay bricks, 6.5cm thick, 23cm long, and 11.4cm wide, 52 bricks per layer, for a total of 72 layers. Use clay mortar for the bricklaying, and control the brick joints to be 1.7mm. Lay the first layer of bricks along a line, and use a level to find the center first.

[0092] Next, lay the wall bricks, 9cm thick, 45.46cm long, and 37.2cm wide, with 60 bricks at each end. When laying the bricks, the workers should control the angle of the bricks and set up stiffening ribs. The angle of the bricks and the stiffening ribs should be kept on the same plane.

[0093] Then, the furnace body bricks are laid, 8.03cm thick, 45cm long, and 15cm wide, in 5 layers. Each layer has a joint in the middle, with 10cm joint bricks. Magnesium mortar is used for the joints. Three bricks are joined with a small piece of cardboard, and every seven layers are joined with a large piece of cardboard. The mortar joints are kept within 2mm. The bricks are laid with a guide line to ensure that the brick surface is flat and the bricks are in a straight line. There are 80 bricks per layer. The gaps at the joints of the end walls are controlled, and the reinforcing plates are covered.

[0094] Step 4: Secondary furnace loading operation;

[0095] Specific location:

[0096] Workers enter the furnace to clean the mud from yesterday's brick surface. The laborers carry the bricks into the furnace, and the senior workers begin to lay the bricks. They lay electrofused and bonded magnesia-chrome bricks, 8.03cm thick, 45cm long, and 15cm wide, in 35 layers.

[0097] Lay out 6cm thick, 45cm long and 15cm wide electrofused magnesia-chrome bricks, 30 layers in total. At the 32nd brick of the furnace body on the east side, lay out copper-exit bricks, 15cm thick, 45.2cm long and 24.9cm wide. Process strip bricks about 10cm long on both sides of the copper-exit. Use J-8 bricks at the top and bottom, with a height of 7.5cm thick, 38cm long and 20cm wide.

[0098] The process begins with laying electrofused magnesia-chrome bricks, 8.03cm thick, 45cm long, and 15cm wide, in 14 layers. Workers then begin installing threaded rods, 14 in a row, 80cm long each. Asbestos boards, 5mm thick, 1.5m long and 1.5m wide, are laid, with 9 boards per layer, for four layers. Clay bricks, 6.5cm thick, 23cm long and 11.4cm wide, are laid, with 52 bricks per layer, for 20 layers.

[0099] Step 5: Brick transportation and construction;

[0100] Specifically:

[0101] Organize personnel to transport bricks into the furnace. Before rotating the furnace, personnel inside the furnace must evacuate. Construction can only begin after the furnace has been rotated to the correct angle and safety has been confirmed. Personnel enter the furnace to lay bricks, which are 7cm thick, 38cm long, and 15cm wide, and are laid in 10 layers.

[0102] Lay two layers of asbestos board, then lay 20 layers of bricks, 40 bricks on each side, for a total of 30 layers;

[0103] Step Six: Converter Inspection;

[0104] Specifically:

[0105] Once the furnace is rotated to the rear opening, the scaffolders are contacted to secure the platform behind the furnace. Before entering the furnace, personnel must check the lead screw and confirm that the furnace is safe. Then, the furnace body bricks are laid. When the furnace opening is 50cm below the opening, bricks are laid to match the furnace opening position. During the laying process, the gaps between the bricks and the water channels are tamped with large pieces of material to prevent molten copper from entering.

[0106] The furnace opening is constructed by using bricks to cover the water channels on both sides of the furnace opening. The bricks are 10cm thick, 35cm long, and 30cm wide.

[0107] The furnace body on both sides is built with bricks at the middle position between the furnace opening and the water channel. Pressure plates are welded on, and a second set of 16 threaded rods are installed to ensure that the threaded rods are on the same plane and to tighten the threaded rods.

[0108] Turn the furnace opening to the front furnace opening position and keep it level. Check the inside of the furnace and only proceed with construction after confirming safety. Clean the inside of the furnace. The welder cuts the pressure plate and lays asbestos board. Then lay clay bricks to restore the copper fitting height to the intersection position. The intersection is built with processed bricks. The furnace opening water channel is wrapped. The gaps are tamped with large material. The small gaps at the furnace opening intersection are filled with magnesium mud. The closing bricks are driven in with a sledgehammer.

[0109] Step 7: Finishing touches;

[0110] Specific location:

[0111] Personnel first entered the furnace to clean the furnace, then laid the end wall bricks, 8cm thick, 45cm long, and 16cm wide, as the first layer for leveling. The bricks were then tamped tightly with large pieces of material between them and the furnace steel shell. Each layer was tamped before the flue bricks were wrapped.

[0112] When building the end wall, a platform should be built. Pay attention to the gaps around the bricks of the end wall and ensure that the magnesia mortar is full. The finishing bricks should be measured in advance.

[0113] Example 2

[0114] A method for constructing an anode furnace, comprising the following steps:

[0115] Step 1: Design Planning: Draw design drawings according to the required size of the anode furnace to confirm the final masonry area;

[0116] Step Two: Material Confirmation: This includes material preparation, material inspection, and site leveling;

[0117] Material preparation: Select asbestos boards, clay bricks, wall bricks, furnace bricks, strip bricks, magnesia-chrome bricks, magnesia-chrome mortar, cardboard, threaded rods, copper-coated bricks, and reinforcing plates;

[0118] Material inspection: Check whether each material conforms to the thickness, length, and width drawn in the design drawings, and whether it meets the qualification standards;

[0119] Site leveling: Remove soil and debris from the masonry location, and use quicklime to draw the edge of the masonry area according to the drawings to determine the masonry area. Dig a 0.3m pit within the area, fill it with interlaced steel bars, and pour concrete to fill two-thirds of the pit. After 36 hours, backfill with soil, level and compact it, and then place and fix the furnace body.

[0120] Step 3: One-time furnace loading operation;

[0121] Specifically:

[0122] Personnel enter the furnace and first lay asbestos boards, 4mm thick, 1.2m long and 1.2m wide, with 7 boards laid per layer, for a total of 6 layers;

[0123] Lay out clay bricks, 5cm thick, 20cm long, and 9cm wide, 50 bricks per layer, for a total of 60 layers. Use clay mortar for the bricklaying, and control the brick joints to be 1.2mm. Lay the first layer of bricks along a line, and use a spirit level to find the center first.

[0124] Next, lay the wall bricks, 8cm thick, 42cm long, and 28cm wide, with 50 bricks at each end. When laying the bricks, the workers should control the angle of the bricks and set up stiffening slabs. The angle of the bricks and the stiffening slabs should be kept on the same plane.

[0125] Then, the furnace body bricks are laid, 7cm thick, 40cm long, and 12cm wide, in 4 layers. Each layer has an 8cm joint in the middle, and the bricks at the joint are laid with magnesium mortar. Three bricks are laid with a small piece of cardboard, and every seven layers are laid with a large piece of cardboard. The mortar joints are kept within 1.5mm. The bricks are laid with a guide line to ensure that the brick surface is flat and the bricks are in a straight line. There are 70 bricks per layer. The gaps at the joints of the end walls are controlled and the reinforcing plates are covered.

[0126] Step 4: Secondary furnace loading operation;

[0127] Specific location:

[0128] Workers enter the furnace to clean the mud from yesterday's brick surface. The laborers transport the bricks into the furnace, and the senior workers begin to lay the bricks. They lay electrofused and bonded magnesia-chrome bricks, 7cm thick, 40cm long, and 12cm wide, or 7cm thick, 35cm long, and 12cm wide, laying 30 layers.

[0129] Lay electrofused reconstituted magnesia-chrome bricks, 7cm thick, 35cm long, and 12cm wide, in 25 layers. At the 28th brick of the furnace body on the east side, lay out copper-exit bricks, 12cm thick, 45.2cm long, and 22cm wide. Process strip bricks about 10cm long on both sides of the copper-exit. Use J-8 bricks at the top and bottom, with a height of 7.5cm thick, 38cm long, and 18cm wide.

[0130] The workers then began laying electrofused magnesia-chrome bricks, 7cm thick, 35cm long, and 12cm wide, in 13 layers. Next, they installed 12 threaded rods per row, each 75cm long. They then laid asbestos boards, 4mm thick, 1.2m long and 1.2m wide, with 7 boards per layer, for a total of four layers. Finally, they laid clay bricks, 6cm thick, 20cm long, and 10cm wide, with 45 bricks per layer, for a total of 18 layers.

[0131] Step 5: Brick transportation and construction;

[0132] Specifically:

[0133] Organize personnel to transport bricks into the furnace. Before rotating the furnace, personnel inside the furnace must evacuate. Construction can only begin after the furnace has been rotated to the correct angle and safety has been confirmed. Personnel enter the furnace to lay bricks, which are 7cm thick, 27cm long, and 12cm wide, and are laid in 9 layers.

[0134] Lay two layers of asbestos board, then lay 18 layers of bricks, with 35 bricks on each side, for a total of 27 layers.

[0135] Step Six: Converter Inspection;

[0136] Specifically:

[0137] Once the furnace is rotated to the rear opening, the scaffolders are contacted to secure the platform behind the furnace. Before entering the furnace, personnel must check the lead screw and confirm that the furnace is safe. Then, the furnace body bricks are laid. When the furnace opening is 45cm below the opening, bricks are laid to match the furnace opening position. During the laying process, the gaps between the bricks and the water channels are tamped with large pieces of material to prevent molten copper from entering.

[0138] The furnace opening is constructed by using bricks to cover the water channels on both sides of the furnace opening. The bricks are 7cm thick, 30cm long, and 25cm wide.

[0139] The furnace body on both sides is built with bricks laid at the middle position between the furnace opening and the water channel. Pressure plates are welded on, and a second set of 14 threaded rods are installed to ensure that the threaded rods are on the same plane and to tighten the threaded rods.

[0140] Turn the furnace opening to the front furnace opening position and keep it level. Check the inside of the furnace and only proceed with construction after confirming safety. Clean the inside of the furnace. The welder cuts the pressure plate and lays asbestos board. Then lay clay bricks to restore the copper fitting height to the intersection position. The intersection is built with processed bricks. The furnace opening water channel is wrapped. The gaps are tamped with large material. The small gaps at the furnace opening intersection are filled with magnesium mud. The closing bricks are driven in with a sledgehammer.

[0141] Step 7: Finishing touches;

[0142] Specific location:

[0143] Personnel first entered the furnace to clean the furnace, then laid the end wall bricks, 7.5cm thick, 40cm long and 14cm wide, for the first layer of leveling. The bricks were then tamped tightly with large pieces of material between them and the furnace steel shell. Each layer was tamped before the flue bricks were wrapped.

[0144] When building the end wall, a platform should be built. Pay attention to the gaps around the bricks of the end wall and ensure that the magnesia mortar is full. The finishing bricks should be measured in advance.

[0145] Example 3

[0146] Step 1: Design Planning: Draw design drawings according to the required size of the anode furnace to confirm the final masonry area;

[0147] Step Two: Material Confirmation: This includes material preparation, material inspection, and site leveling;

[0148] Material preparation: Select asbestos boards, clay bricks, wall bricks, furnace bricks, strip bricks, magnesia-chrome bricks, magnesia-chrome mortar, cardboard, threaded rods, copper-coated bricks, and reinforcing plates;

[0149] Material inspection: Check whether each material conforms to the thickness, length, and width drawn in the design drawings, and whether it meets the qualification standards;

[0150] Site leveling: Remove soil and debris from the masonry location, and use quicklime to draw the edge of the masonry area according to the drawings to determine the masonry area. Dig a 0.2m pit within the area, fill it with interlaced steel bars, and pour concrete to fill two-thirds of the pit. After 24 hours, backfill with soil, level and compact it, and then place and fix the furnace body.

[0151] Step 3: One-time furnace loading operation;

[0152] Specifically:

[0153] Personnel enter the furnace and first lay asbestos boards, 3mm thick, 1m long and 1m wide, with 6 boards laid per layer, for a total of 5 layers;

[0154] Lay clay bricks, 4cm thick, 15cm long, and 8cm wide, in layers of 45, for a total of 65 layers. Use clay mortar for the bricklaying, and control the brick joints to be 1.7mm. Lay the first layer of bricks along a line, and use a spirit level to find the center first.

[0155] Next, lay the wall bricks, 9cm thick, 42cm long, and 35cm wide, with 50 bricks at each end. When laying the bricks, the workers should control the angle of the bricks and set up stiffening slabs. The angle of the bricks and the stiffening slabs should be kept on the same plane.

[0156] Then, the furnace body bricks are laid, 7cm thick, 40cm long, and 10cm wide, in 3 layers, with each layer having a joint in the middle. The joint bricks are 8cm thick and laid with magnesium mortar. Three bricks are laid with a small piece of cardboard, and every seven layers are laid with a large piece of cardboard. The mortar joints are kept within 1mm. The bricks are laid with a guide line to ensure that the brick plane is flat and the bricks are in a straight line. There are 65 bricks per layer. The gaps at the joints of the end walls are controlled and the reinforcing plates are covered.

[0157] Step 4: Secondary furnace loading operation;

[0158] Specific location:

[0159] Workers enter the furnace to clean the mud from yesterday's brick surface. The laborers transport the bricks into the furnace, and the senior workers begin to lay the bricks. They lay electrofused and bonded magnesia-chrome bricks, which are 6cm thick, 35cm long, and 10cm wide. They lay 30 layers of bricks, which are 7cm thick, 45cm long, and 12cm wide.

[0160] Lay out electrofused reconstituted magnesia-chrome bricks, 7cm thick, 40cm long, and 13cm wide, in 26 layers. At the 31st brick of the furnace body on the east side, lay out copper-exit bricks, 12cm thick, 45.2cm long, and 22cm wide. Process strip bricks about 10cm long on both sides of the copper-exit. Use J-8 bricks at the top and bottom, with a height of 7.5cm thick, 38cm long, and 20cm wide.

[0161] The workers then began laying electrofused magnesia-chrome bricks, 6cm thick, 30cm long, and 10cm wide, in 12 layers. They then started installing threaded rods, 14 in a row, 80cm long each. Next, they laid asbestos boards, 5mm thick, 1m long, and 1.5m wide, 9 boards per layer, for a total of four layers. Finally, they laid clay bricks, 6.5cm thick, 23cm long, and 11.4cm wide, 45 bricks per layer, for a total of 18 layers.

[0162] Step 5: Brick transportation and construction;

[0163] Specifically:

[0164] Organize personnel to transport bricks into the furnace. Before rotating the furnace, personnel inside the furnace must evacuate. Construction can only begin after the furnace has been rotated to the correct angle and safety has been confirmed. Personnel enter the furnace to lay bricks, which are 6cm thick, 25cm long, and 15cm wide, and are laid in 8 layers.

[0165] Lay two layers of asbestos board, then build 15 layers of bricks, with 35 bricks on each side, for a total of 25 layers.

[0166] Step Six: Converter Inspection;

[0167] Specifically:

[0168] Once the furnace is rotated to the rear opening, the scaffolders are contacted to secure the platform behind the furnace. Before entering the furnace, personnel must check the lead screw and confirm that the furnace is safe. Then, the furnace body bricks are laid. When the furnace opening is 50cm below the opening, bricks are laid to match the furnace opening position. During the laying process, the gaps between the bricks and the water channels are tamped with large pieces of material to prevent molten copper from entering.

[0169] The furnace opening is constructed by using bricks to cover the water channels on both sides of the furnace opening. The bricks are 6cm thick, 32cm long, and 25cm wide.

[0170] The furnace body on both sides is built with bricks at the middle position between the furnace opening and the water channel. Pressure plates are welded on, and a second set of threaded rods is installed. There are a total of 13 threaded rods to ensure that the threaded rods are on the same plane and to tighten the threaded rods.

[0171] Turn the furnace opening to the front furnace opening position and keep it level. Check the inside of the furnace and only proceed with construction after confirming safety. Clean the inside of the furnace. The welder cuts the pressure plate and lays asbestos board. Then lay clay bricks to restore the copper fitting height to the intersection position. The intersection is built with processed bricks. The furnace opening water channel is wrapped. The gaps are tamped with large material. The small gaps at the furnace opening intersection are filled with magnesium mud. The closing bricks are driven in with a sledgehammer.

[0172] Step 7: Finishing touches;

[0173] Specific location:

[0174] Personnel first entered the furnace to clean the furnace, then laid the end wall bricks, 8cm thick, 45cm long, and 16cm wide, as the first layer for leveling. The bricks were then tamped tightly with large pieces of material between them and the furnace steel shell. Each layer was tamped before the flue bricks were wrapped.

[0175] When building the end wall, a platform should be built. Pay attention to the gaps around the bricks of the end wall and ensure that the magnesia mortar is full. The finishing bricks should be measured in advance.

[0176] The anode furnace includes a cylinder, end caps, oxidation-reduction inlet, copper inlet, furnace opening, dilute oxygen burner inlet, flue gas outlet, flue gas pipe, and furnace opening cover. The cylinder is 75mm in diameter, the end caps on both sides of the furnace are 425mm in diameter, and are combined with magnesia-chrome bricks in an alternating manner. The oxidation-reduction inlet includes tuyere bricks, which are 400mm in diameter, and two tuyere bricks are provided, two of which are perforated. The copper inlet bricks are 450mm in diameter, and two copper inlet bricks are provided, both of which are perforated. The dilute oxygen burner inlet area is made of magnesia-chrome castable material. The flue gas outlet and flue gas pipe are covered with 10mm aluminum silicate fiberboard.

[0177] In summary, by planning and pre-leveling the refractory environment to ensure a more stable foundation, and by combining multiple furnace operations to install the refractory materials in batches, the furnace lining can be successfully constructed. This ensures stable furnace temperature after the main refractory materials are installed, allowing the furnace lining to withstand the intense mechanical erosion of the high-temperature melt during the blowing process. This reduces the degree of slag and quartz flux erosion, stabilizes the furnace temperature periodically, and reduces the drawbacks of mechanical collisions and wear during furnace mouth cleaning and oxidation-reduction port maintenance. This optimizes operating conditions, shortens the maintenance cycle, and effectively increases production capacity.

[0178] Although the invention has been described above with reference to embodiments, various modifications can be made and components can be replaced with equivalents without departing from the scope of the invention. In particular, features in the embodiments disclosed herein can be combined in any way, provided there is no structural conflict. The lack of an exhaustive description of these combinations in this specification is merely for brevity and resource conservation. Therefore, the invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A method for constructing an anode furnace, characterized in that: The steps of this method are as follows: Step 1: Design Planning: Draw design drawings according to the required size of the anode furnace to confirm the final masonry area; Step Two: Material Confirmation: This includes material preparation, material inspection, and site leveling; Material preparation: Select asbestos boards, clay bricks, wall bricks, furnace bricks, strip bricks, magnesia-chrome bricks, magnesia-chrome mortar, cardboard, threaded rods, copper-coated bricks, and reinforcing plates; Material inspection: Check whether each material conforms to the thickness, length, and width drawn in the design drawings, and whether it meets the qualification standards; Site leveling: Remove soil and debris from the masonry location, and use quicklime to draw the edge of the masonry area according to the drawings to determine the masonry area. Dig a pit 0.2m to 0.5m deep within the area, fill it with interlaced steel bars, and pour concrete to fill two-thirds of the pit. After 24H to 48H, backfill with soil, level and compact it, and then place and fix the furnace body. Step 3: One-time furnace loading operation; Specifically: When personnel enter the furnace, they first lay asbestos boards, which are 3mm to 5mm thick, 1m to 1.5m long, and 1m to 1.5m wide. Six to nine boards are laid in one layer, and five to eight layers are laid in total. Lay clay bricks with a thickness of 4cm to 6.5cm, a length of 15cm to 23cm, and a width of 8cm to 11.4cm. Lay 45 to 52 bricks per layer and build 65 to 72 layers. Use clay mortar for the bricklaying and control the brick joints to be 1.5mm to 1.7mm. Lay the first layer of bricks with a line in mind and use a spirit level to find the center first. Next, lay the wall bricks, with a thickness of 7.5cm to 9cm, a length of 40cm to 45.46cm, and a width of 25cm to 37.2cm. Lay 45 to 60 bricks at each end. When laying the bricks, the workers should control the angle of the bricks and set up stiffening slabs. The angle of the bricks and the stiffening slabs should be kept on the same plane. Then, the furnace body bricks are laid, with a thickness of 6cm to 8.03cm, a length of 35cm to 45cm, and a width of 10cm to 15cm. 3 to 5 layers are laid, with joints in the middle of each layer. The joint bricks are 8cm to 10cm thick and laid with magnesium mortar. Three bricks are laid with a small piece of cardboard, and every seven layers are laid with a large piece of cardboard. The mortar joints are kept within 1mm to 2mm. The bricks are laid with a guide line to ensure that the brick surface is flat and the bricks are in a straight line. There are 65 to 80 bricks per layer. The gaps at the joints of the end walls are controlled and the reinforcing plates are covered. Step 4: Secondary furnace loading operation; Specific location: Workers enter the furnace to clean the mud from yesterday's surface of the bricks. The laborers carry the bricks into the furnace, and the senior workers begin to lay the bricks. They lay electrofused magnesia-chrome bricks with a thickness of 6cm to 8.03cm, a length of 35cm to 45cm, and a width of 10cm to 15cm, laying 25 to 35 layers. Lay electrofused rebonded magnesia-chrome bricks, 6cm-8.03cm thick, 30cm-45cm long, and 12cm-15cm wide, in 22-30 layers. At the 30th-32nd brick of the furnace body on the east side, lay copper-exit bricks, 10cm-15cm thick, 45.2cm long, and 20.26-24.9cm wide. Process strip bricks about 10cm long on both sides of the copper-exit, and use J-8 bricks at the top and bottom, with a height of 7.5cm thick, 38cm long, and 18-20cm wide. Lay electrofused magnesia-chrome bricks, 6cm-8.03cm thick, 30cm-45cm long, and 10cm-15cm wide, in 12-14 layers. Then, install threaded rods, 12-14 rods per row, 70cm-80cm long. First, lay asbestos boards, 3mm-5mm thick, 1m-1.5m long and 1m-1.5m wide, 6-9 boards per layer, for four layers. Then, lay clay bricks, 5cm-6.5cm thick, 13cm-23cm long, and 8cm-11.4cm wide, 40-52 bricks per layer, for 15-20 layers. Step 5: Brick transportation and construction; Specifically: Organize personnel to transport bricks into the furnace. Before rotating the furnace, personnel inside the furnace must be evacuated. Construction can only begin after the furnace has been rotated to the correct angle and safety has been confirmed. Personnel enter the furnace to lay bricks, with a thickness of 6cm to 8.03cm, a length of 25cm to 38cm, and a width of 10cm to 15cm, in 8 to 10 layers. Lay two layers of asbestos board, then lay 15 to 20 layers of bricks, with 30 to 40 bricks on each side, for a total of 25 to 30 layers; Step Six: Converter Inspection; Specifically: Once the furnace is rotated to the rear opening, the scaffolders are contacted to secure the platform behind the furnace. Before entering the furnace, personnel must check the lead screw and confirm that the furnace is safe. Then, the furnace body bricks are laid. When the furnace opening is 35cm to 50cm below the opening, bricks are laid to match the furnace opening position. During the laying process, the gaps between the bricks and the water channels are tamped with large pieces of material to prevent molten copper from entering. The furnace opening is constructed by using bricks to cover the water channels on both sides. The bricks are 6cm to 10cm thick, 25 to 38cm long, and 20cm to 30cm wide. The furnace body is built on both sides, with the bricks laid at the middle of the furnace opening and water channel. Pressure plates are welded on, and a second set of threaded rods is installed. There are a total of 12 to 16 threaded rods to ensure that the threaded rods are on the same plane and to tighten the threaded rods. Turn the furnace opening to the front furnace opening position and keep it level. Check the inside of the furnace and only proceed with construction after confirming safety. Clean the inside of the furnace. The welder cuts the pressure plate and lays asbestos board. Then lay clay bricks to restore the copper fitting height to the intersection position. The intersection is built with processed bricks. The furnace opening water channel is wrapped. The gaps are tamped with large material. The small gaps at the furnace opening intersection are filled with magnesium mud. The closing bricks are driven in with a sledgehammer. Step 7: Finishing touches; Specific location: Personnel first enter the furnace to clean the furnace, then lay the end wall bricks, 7.5cm-8cm thick, 30cm-45cm long, and 15cm-16cm wide. The first layer is leveled, and the bricks are tamped tightly with large pieces of material between them and the furnace body steel shell. Each layer is tamped and then laid, and the flue bricks are wrapped. When building the end wall, a platform should be built. Pay attention to the gaps around the bricks of the end wall and ensure that the magnesia mortar is full. The finishing bricks should be measured in advance.

2. The anode furnace construction method according to claim 1, characterized in that: The anode furnace includes a cylinder, end caps, oxidation-reduction port, copper port, furnace opening, dilute oxygen burner port, flue gas port, flue gas pipe and furnace opening cover, and the cylinder has a specification of 65mm to 80mm.

3. The anode furnace construction method according to claim 2, characterized in that: The furnace body has end caps on both sides with a size of 325mm to 425mm, and is bonded with magnesia-chrome bricks at intervals.

4. The anode furnace construction method according to claim 2, characterized in that: The oxidation-reduction port includes an eyelet brick, which is 350mm to 450mm in size, and 1 to 3 eyelet bricks are provided, of which 1 to 2 are perforated.

5. The anode furnace construction method according to claim 2, characterized in that: The copper-fitted bricks are 350mm to 450mm in size, and 1 to 3 copper-fitted bricks are provided, all of which are perforated.

6. The anode furnace construction method according to claim 2, characterized in that: The rarefied oxygen burner nozzle area is made of magnesium-chromium casting material.

7. The anode furnace construction method according to claim 2, characterized in that: A 5mm to 10mm thick aluminum silicate fiberboard is installed on the smoke exhaust outlet and smoke exhaust pipe.

Citation Information

Patent Citations

  • Method for building coke oven

    CN107429166A

  • Method for replacing redox port brick of rotary anode furnace in hot state