A post-texturing method for manufacturing a combined passivation back contact battery
By using a specific polishing slurry and pre-cleaning process, the problem of incomplete texturing in the laser-engaged area was solved, improving the on-state voltage and cell conversion efficiency of the passivated back contact cell, and reducing silicon wafer loss.
Patent Information
- Application Number
- CN202410509617.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-04-26
AI Technical Summary
In the existing technology, the texturing in the laser opening area of the combined passivation back contact battery is incomplete, resulting in poor passivation film quality and affecting the on-state voltage and battery conversion efficiency.
By employing a specific polishing slurry and pre-cleaning process, combined with an appropriate amount of ethylenediaminetetramethylenephosphoric acid, the mask layer is selectively protected, the damaged layer and residual semiconductor layer in the laser opening area are removed, a uniform textured surface is formed, and a high-quality passivation film is formed on the front side.
The damaged and residual layers in the laser-aperture area were removed in a short time, improving passivation performance, enhancing on-state voltage and cell conversion efficiency, while reducing silicon wafer loss.
Smart Images

Figure CN118099290B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of manufacturing a combined passivation back contact battery, and in particular relates to a post-texturing manufacturing method for a combined passivation back contact battery. Background Art
[0002] At present, the post-texturing process of the combined passivation back contact battery is generally as follows:
[0003] S101, providing a silicon wafer with a double-sided polishing structure;
[0004] S102, sequentially coating a first semiconductor layer and a first mask layer on the back side of the silicon wafer, wherein the first semiconductor layer is formed by LPCVD or tubular PECVD, and the first semiconductor layer includes a tunneling oxide layer and a first doped polycrystalline layer;
[0005] S103, laser etching an opening on the back side of the silicon wafer to remove the first mask layer and a portion of the first semiconductor layer to form a second semiconductor opening region;
[0006] S104, texturing and cleaning, forming a texturing surface on the second semiconductor opening area on the back side and the front side, and removing the first mask layer; the texturing and cleaning process includes a texturing process and a cleaning process;
[0007] S105, forming a passivation layer and an anti-reflection layer on the front side of the silicon wafer, and forming a second semiconductor layer on the back side, wherein the second semiconductor layer includes an intrinsic amorphous silicon layer and a second doped amorphous or microcrystalline silicon layer sequentially formed on the back side;
[0008] S106, laser or etching an opening on the back side of the silicon wafer to form a first semiconductor opening region that is alternately arranged with the second semiconductor opening region;
[0009] S107, depositing a conductive film layer on the back side of the silicon wafer;
[0010] S108, forming an insulating groove on the conductive film layer between the first semiconductor opening region and the second semiconductor opening region by laser or etching;
[0011] S109, forming metal electrodes on the outer surface of the conductive film layer in the first semiconductor opening region and the second semiconductor opening region of the silicon wafer.
[0012] In S104 of the above-mentioned prior art, a post-texturing method is adopted to remove the damaged layer and the remaining first semiconductor layer in the laser opening area by texturing, and to form a texture surface in the second semiconductor opening area and the front side at the same time.
[0013] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology.
[0014] The above-mentioned prior art S104 has the following technical problems: 1. The damaged layer and the remaining first semiconductor layer in the laser opening area will block etching, resulting in incomplete local velvet removal, such as Figure 2 As shown; 2. Compared with the suede passivation in the normal area, the suede passivation film layer in the laser opening area has poor quality and low minority carriers, which ultimately affects the opening voltage and battery conversion efficiency. Summary of the invention
[0015] The purpose of the present invention is to overcome the defects of the prior art that the opening voltage and battery conversion efficiency of the combined passivation back contact battery need to be further improved, and to provide a post-texturing production method for a combined passivation back contact battery. The post-texturing production method solves the problem of incomplete texturing after laser opening, and at the same time does not corrode the mask layer, and the silicon wafer loss is small; the quality of the deposited passivation film layer is significantly improved, the passivation performance is improved, thereby improving the opening voltage and battery conversion efficiency.
[0016] In order to achieve the above object, the present invention provides a post-texturing method for a combined passivation back contact battery, comprising the following steps:
[0017] S1, provide double-sided polished silicon wafers;
[0018] S2, forming a first semiconductor layer and a mask layer in sequence on the back side of the silicon wafer; the mask layer has a thickness of 30-90 nm; the first semiconductor layer comprises a tunneling oxide layer and a first doped polycrystalline layer;
[0019] S3, performing a first laser etching on the first semiconductor layer and its corresponding mask layer in a preset area on the back surface obtained in S2, removing the mask layer and a portion of the first semiconductor layer in the preset area, and forming a second semiconductor opening area distributed at intervals;
[0020] S4, texturing and cleaning, forming a texturing surface in the second semiconductor opening region on the back side and on the front side at the same time, and optionally removing the mask layer; the texturing and cleaning process at least includes pre-cleaning, polishing, and texturing;
[0021] The polishing liquid used in the polishing is a mixed solution containing alkali, polishing additives and water, the pH of the polishing liquid is 11-13, the mass concentration of the alkali in the polishing liquid is 1%-3%, the mass concentration of the polishing additive in the polishing liquid is 0.5%-2%, the polishing additive contains ethylenediaminetetramethylenephosphonic acid, and the concentration of ethylenediaminetetramethylenephosphonic acid in the polishing additive is 0.1%-2%;
[0022] The polishing conditions include: reaction temperature of 60°C-85°C, reaction time of 30-300s;
[0023] S5. Form a passivation layer and an anti-reflection layer on the front side of the silicon wafer obtained in S4, and form a second semiconductor layer on the back side, wherein the second semiconductor layer comprises an intrinsic amorphous silicon layer and a second doped silicon layer.
[0024] In some preferred embodiments of the present invention, the polishing additive further comprises benzoic acid, polyethylene glycol, sodium silicate and water. Based on the total amount of the polishing additive, the concentration of benzoic acid is 0.5%-2%, the concentration of sodium silicate is 0.1%-2%, and the concentration of polyethylene glycol is 0.1%-0.5%.
[0025] In some preferred embodiments of the present invention, the base is potassium hydroxide or sodium hydroxide.
[0026] In some preferred embodiments of the present invention, the single-side corrosion depth is controlled within 1 μm during the polishing.
[0027] In some preferred embodiments of the present invention, when the thickness of the mask layer is 50-69 nm, the concentration of ethylenediaminetetramethylenephosphonic acid in the polishing additive is controlled to be 1.1%-2%; when the thickness of the mask layer is 70-90 nm, the concentration of ethylenediaminetetramethylenephosphonic acid in the polishing additive is controlled to be 0.1%-1.0%.
[0028] In some preferred embodiments of the present invention, the pre-cleaning solution used in the pre-cleaning is a mixed solution containing NH4OH and H2O2 or a mixed solution containing a strong base and H2O2, wherein the strong base is KOH and / or NaOH, and the mass concentration of NH4OH or the strong base in the pre-cleaning solution is 2%-5%, and the mass concentration of H2O2 is 3%-5%; the pre-cleaning conditions include: the reaction temperature is 60-80°C, and the reaction time is 2-4min.
[0029] In some preferred embodiments of the present invention, the texturing liquid used for texturing is a mixed solution of tetramethylammonium hydroxide, a texturing additive and water. Based on the total weight of the texturing liquid, the mass concentration of tetramethylammonium hydroxide is 1%-2%, and the mass concentration of the texturing additive is 0.5%-2%.
[0030] Further preferably, the texturing conditions include: reaction temperature of 60°C-80°C, reaction time of 8-15min, single-side etching depth of silicon wafer after texturing of 2-3μm, and texturing until surface reflectivity is less than 10%.
[0031] In some preferred embodiments of the present invention, the texturing and cleaning process further includes: water washing between pre-cleaning and polishing, and after polishing, sequentially performing water washing, one alkali washing, water washing, texturing, water washing, two alkali washings, and water washing.
[0032] In some more preferred embodiments of the present invention, the alkaline washing solution used in alkaline washing is a mixed solution containing NH4OH and H2O2 or a mixed solution containing a strong base and H2O2, wherein the strong base is KOH and / or NaOH, and the mass concentration of NH4OH or the strong base in the alkaline washing solution is 2%-5%, and the mass concentration of H2O2 is 3%-5%.
[0033] In some preferred embodiments of the present invention, the conditions for alkali washing include: a reaction temperature of 60-80° C. and a reaction time of 2-4 min.
[0034] In some preferred embodiments of the present invention, the texturing and cleaning process further comprises: after the secondary alkaline washing and water washing, acid washing, water washing, HF washing, and water washing are sequentially performed, and whether to perform slow pulling and drying is selected according to demand. The slow pulling process includes slowly lifting the silicon wafer out of the hot water.
[0035] Further preferably, the slow pulling conditions include: the temperature of the hot water is 45-55° C., and the pulling time is 60-120 seconds.
[0036] In some preferred embodiments of the present invention, the pickling solution used in the pickling is a mixed solution containing HCl and H2O2 or a mixed solution containing HCl and O3. Based on the total amount of the pickling solution, the mass concentration of HCl is 2%-5%, the mass concentration of H2O2 is 3%-5%, and the concentration of O3 is 5ppm-10ppm; the pickling conditions include: the reaction temperature is 60-80°C, and the reaction time is 2-4min.
[0037] In some preferred embodiments of the present invention, the mass concentration of HF in the HF solution used for HF washing is 5%-10%.
[0038] Further preferably, the conditions for HF washing include: reaction temperature of 20-35° C., and reaction time of 120-300 s.
[0039] In some preferred embodiments of the present invention, the water washing is pure water overflow, and each water washing time is 90-150s.
[0040] In some preferred embodiments of the present invention, the post-texturing method for the combined passivation back contact cell further comprises:
[0041] S6, performing a second etching on a portion of the second semiconductor corresponding to the polished area on the back side obtained in S5 to remove the second semiconductor layer and form a first semiconductor opening area;
[0042] S7, forming a conductive film layer to fully cover the back surface obtained in S6;
[0043] S8, performing a third etching on the conductive film layer located between the first semiconductor opening region and the second semiconductor opening region on the back side obtained in S7 to form an insulating groove;
[0044] S9. Form metal electrodes on the outer surfaces of the conductive film layer corresponding to the first semiconductor opening region and the second semiconductor opening region on the back side.
[0045] Beneficial effects:
[0046] The present invention uses the above technical scheme, especially uses pre-cleaning and specific polishing liquid for polishing before etching, which can remove the damaged layer and the residual first semiconductor layer in the laser opening area in a short time, solves the problem of incomplete velvet after laser opening, and at the same time, the appropriate amount of ethylenediaminetetramethylenephosphoric acid contained can be selectively adsorbed on the surface of the mask layer, reducing the corrosion rate of the mask layer by alkali, so that the mask layer is basically not corroded, and the silicon chip loss is small; after polishing and then etching, the edge and middle velvet pyramid size of the laser opening area are uniform, the quality of the passivation film layer is significantly improved, the passivation performance is improved, thereby improving the opening voltage (i.e., open circuit voltage) and battery conversion efficiency. In addition, the present invention can also remove the front winding plating layer at the same time in a short time, and also solves the problem of uneven size of the front velvet and high front reflectivity, the front reflectivity is low, and the short-circuit current of the battery is improved.
[0047] Among them, the polishing of the present invention uses a specific polishing liquid, which does not damage the tunneling oxide layer passivation layer, and effectively removes the damaged layer in the laser opening area and the residual first semiconductor layer under the condition of the minimum etching amount, so that the quality of the passivation film layer of the second semiconductor layer is significantly improved, and the passivation performance is greatly improved. In addition, the polishing liquid uses a low-concentration alkali solution to polish at a lower temperature, which can slow down the drilling corrosion ability of the alkali solution on the mask layer. At the same time, with a specific polishing additive, the mask layer on the back can be protected from corrosion to the greatest extent, thereby not damaging the first semiconductor layer; after polishing, the damaged layer and the first semiconductor layer of the first semiconductor plating area on the front of the silicon wafer and the laser opening area on the back can be quickly removed. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0049] Figure 1 It is a schematic structural diagram of a specific embodiment of the back contact battery of the present invention.
[0050] Figure 2 This is a metallographic picture of incomplete velvet removal after laser opening.
[0051] Figure 3 This is a metallographic picture of the fully velvet-free surface after laser opening in Example 1 of the present invention.
[0052] Description of Reference Numerals
[0053] 1. Silicon wafer, 2. Tunneling oxide layer, 3. First doped polycrystalline layer, 4. Intrinsic amorphous silicon layer, 5. Second doped amorphous silicon layer, 6. Conductive film layer, 7. Passivation layer, 8. Anti-reflection layer, 9. Metal electrode. DETAILED DESCRIPTION
[0054] In the present invention, unless otherwise specified, directional words such as "upper, lower, left, right" are generally understood in conjunction with the directions shown in the drawings and actual applications.
[0055] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0056] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0057] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).
[0058] In the present invention, the area close to the silicon wafer is referred to as the inside, and the area far from the silicon wafer is referred to as the outside.
[0059] The present invention provides a post-texturing method for a combined passivation back contact battery, comprising the following steps:
[0060] S1, provide double-sided polished silicon wafers;
[0061] S2, forming a first semiconductor layer and a mask layer in sequence on the back side of the silicon wafer; the mask layer has a thickness of 30-90 nm, preferably 50-90 nm; the first semiconductor layer comprises a tunneling oxide layer and a first doped polycrystalline layer;
[0062] S3, performing a first laser etching on the first semiconductor layer and its corresponding mask layer in a preset area on the back surface obtained in S2, removing the mask layer and a portion of the first semiconductor layer in the preset area, and forming a second semiconductor opening area distributed at intervals;
[0063] S4, texturing and cleaning, forming a texturing surface in the second semiconductor opening region on the back side and on the front side at the same time, and optionally removing the mask layer (whether to remove the mask layer can be determined according to actual needs); the texturing and cleaning process at least includes pre-cleaning, polishing, and texturing;
[0064] The polishing liquid used in the polishing is a mixed solution containing alkali, polishing additives and water, the pH of the polishing liquid is 11-13, the mass concentration of the alkali in the polishing liquid is 1%-3%, the mass concentration of the polishing additive in the polishing liquid is 0.5%-2%, the polishing additive contains ethylenediaminetetramethylenephosphonic acid, and the concentration of ethylenediaminetetramethylenephosphonic acid in the polishing additive is 0.1%-2%;
[0065] The polishing conditions include: reaction temperature of 60°C-85°C, preferably 60°C-70°C, reaction time of 30-300s, preferably 30-180s;
[0066] S5. Form a passivation layer and an anti-reflection layer on the front side of the silicon wafer obtained in S4, and form a second semiconductor layer on the back side, wherein the second semiconductor layer comprises an intrinsic amorphous silicon layer and a second doped silicon layer.
[0067] The silicon wafer in S1 can be cleaned after double-sided polishing. The silicon wafer is preferably an N-type single crystal silicon wafer. The silicon wafer can be a Czochralski single crystal silicon wafer or a cast single crystal silicon wafer.
[0068] The first doped polycrystalline layer and the second doped silicon layer, one of which is N-type and the other is P-type. The second doped silicon layer can be doped microcrystalline silicon or doped amorphous silicon.
[0069] The thickness, doping concentration and formation process of each film layer contained in the first semiconductor layer and the second semiconductor layer of the present invention can refer to the prior art and can be used in the present invention. For example, the thickness of the tunneling oxide layer is 1-2nm, the thickness of the first doped polycrystalline layer is 70-300nm, and the effective doping concentration is greater than 1e19cm -3The thickness of the intrinsic amorphous silicon layer is 5-15nm, the thickness of the second doped silicon layer is 5-20nm, and the effective doping concentration is 2e18cm -3 -1e20cm -3 .
[0070] The type and thickness of the mask layer in S2 can refer to the prior art, for example, the type can be at least one of silicon nitride, silicon oxide, and silicon oxynitride, preferably silicon nitride. The thickness of the mask layer can be, for example, 50-90 nm.
[0071] In S4, in some preferred embodiments of the present invention, the polishing additive further comprises benzoic acid, polyethylene glycol, sodium silicate and water. Further preferably, based on the total amount of the polishing additive, the concentration of benzoic acid is 0.5%-2%, the concentration of sodium silicate is 0.1%-2%, and the concentration of polyethylene glycol is 0.1%-0.5%. Using a polishing additive of a specific composition, benzoic acid is used as a pH regulator, and an appropriate amount can adjust the pH value of the polishing additive to maintain the stability of the solution; polyethylene glycol is a surfactant, and an appropriate amount can increase the contact between the polishing liquid and the silicon wafer, making the reaction faster and more uniform; an appropriate amount of sodium silicate can change the viscosity of the polishing liquid, control the reaction rate, and can complex metal ions to ensure the cleanliness of the silicon wafer surface, thereby more conducive to protecting the mask layer from corrosion.
[0072] In some preferred embodiments of the present invention, the base is potassium hydroxide or sodium hydroxide.
[0073] In some preferred embodiments of the present invention, the single-side corrosion depth is controlled within 1 μm during the polishing.
[0074] In some preferred embodiments of the present invention, when the thickness of the mask layer is 50-69nm, the concentration of ethylenediaminetetramethylenephosphonic acid in the polishing additive is controlled to be 1.1%-2%; when the thickness of the mask layer is 70-90nm, the concentration of ethylenediaminetetramethylenephosphonic acid in the polishing additive is controlled to be 0.1%-1.0%. The concentration of ethylenediaminetetramethylenephosphonic acid is specifically adjusted according to the thickness range of the mask layer, which is more conducive to improving the reaction rate while protecting the mask layer, and is conducive to further shortening the process time. Among them, when the thickness of the mask layer is thicker, the protection of the bottom film layer of the mask layer is better, and the concentration of ethylenediaminetetramethylenephosphonic acid contained in the polishing additive is appropriately reduced, so that the reaction rate can be appropriately accelerated without damaging the passivation film layer, shortening the polishing process time.
[0075] The pre-cleaning of the present invention is used to remove dirt and organic matter on the surface of the silicon wafer. In some preferred embodiments of the present invention, the pre-cleaning solution used in the pre-cleaning is a mixed solution containing NH4OH and H2O2 or a mixed solution containing a strong base and H2O2, wherein the strong base is KOH and / or NaOH, and the mass concentration of NH4OH or the strong base in the pre-cleaning solution is 2%-5%, and the mass concentration of H2O2 is 3%-5%.
[0076] In some preferred embodiments of the present invention, the pre-cleaning conditions include: a reaction temperature of 60-80° C. and a reaction time of 2-4 min.
[0077] In some preferred embodiments of the present invention, the texturing liquid used in the texturing is a mixed solution of tetramethylammonium hydroxide, a texturing additive and water, and based on the total weight of the texturing liquid, the mass concentration of tetramethylammonium hydroxide is 1%-2%, and the mass concentration of the texturing additive is 0.5%-2%. Using an appropriate amount of tetramethylammonium hydroxide for texturing further helps to protect the mask layer from corrosion.
[0078] The texturing additive can refer to the prior art, for example, it can be a commercial product, and will not be described in detail here.
[0079] In some preferred embodiments of the present invention, the texturing conditions include: reaction temperature of 60°C-80°C, reaction time of 8-15min, single-sided etching depth of silicon wafer after texturing of 2-3μm, and texturing until the surface reflectivity is less than 10%.
[0080] In some preferred embodiments of the present invention, the texturing and cleaning process further includes: water washing between pre-cleaning and polishing, and after polishing, sequentially performing water washing, one alkali washing, water washing, texturing, water washing, two alkali washings, and water washing.
[0081] In some preferred embodiments of the present invention, the alkaline washing solution used in alkaline washing is a mixed solution containing NH4OH and H2O2 or a mixed solution containing a strong base and H2O2, wherein the strong base is KOH and / or NaOH, and the mass concentration of NH4OH or the strong base in the alkaline washing solution is 2%-5%, and the mass concentration of H2O2 is 3%-5%.
[0082] In some preferred embodiments of the present invention, the conditions of alkali washing include: reaction temperature of 60-80°C, reaction time of 2-4 minutes. Alkali washing includes primary alkali washing and secondary alkali washing, and the conditions of primary alkali washing and secondary alkali washing can be the same or different.
[0083] After the polishing and texturing steps, alkaline washing under the aforementioned appropriate conditions can effectively remove the organic matter remaining on the surface of the silicon wafer, which is conducive to forming a pyramid velvet surface without water mark imprints.
[0084] In some preferred embodiments of the present invention, the texturing cleaning process further comprises: after secondary alkali washing and water washing, acid washing, water washing, HF washing and water washing are sequentially performed.
[0085] In some preferred embodiments of the present invention, the texturing and cleaning process further includes: after HF washing and water washing, whether to perform slow pulling and drying is selected according to demand. The slow pulling process includes slowly pulling the silicon wafer out of hot water, and the conditions for slow pulling include: the temperature of the hot water is 45-55°C, and the pulling time is 60-120s. The present invention adopts slow pulling mainly to dehydrate the surface of the silicon wafer and facilitate drying.
[0086] In some preferred embodiments of the present invention, the pickling solution used in the pickling is a mixed solution containing HCl and H2O2 or a mixed solution containing HCl and O3. Based on the total amount of the pickling solution, the mass concentration of HCl is 2%-5%, the mass concentration of H2O2 is 3%-5%, and the concentration of O3 is 5ppm-10ppm.
[0087] In some preferred embodiments of the present invention, the acid pickling conditions include: a reaction temperature of 60-80° C. and a reaction time of 2-4 min.
[0088] Pickling under appropriate conditions, including pickling with a specific pickling solution, can remove metal ions on the surface of the silicon wafer and is more conducive to obtaining a clean interface.
[0089] The HF washing of the present invention is used to remove the mask layer. In some preferred embodiments of the present invention, the mass concentration of HF in the HF solution used in the HF washing is 5%-10%.
[0090] In some preferred embodiments of the present invention, the conditions for HF washing include: reaction temperature of 20-35° C., and reaction time of 120-300 s.
[0091] In the HF washing scheme under appropriate solution and conditions of the present invention, the mask layer on the first semiconductor layer can be completely removed in the HF washing step, and the interface of the second semiconductor opening region can be chemically passivated.
[0092] In some preferred embodiments of the present invention, the water washing is pure water overflow, and each water washing time is 90-150s. The water washing here refers to any water washing in the texturing cleaning process, and the water washing conditions after different processes can be selected within this range, and can be the same or different. The water washing after the corresponding solution used in each special process can completely remove the chemical solution remaining on the surface of the silicon wafer.
[0093] The types and thicknesses of the passivation layer and the anti-reflection layer on the front side in S5 of the present invention can refer to the prior art and can be used in the present invention.
[0094] In some preferred embodiments of the present invention, the post-texturing method for the combined passivation back contact cell further comprises:
[0095] S6, performing a second etching on a portion of the second semiconductor corresponding to the polished area on the back side obtained in S5 to remove the second semiconductor layer and form a first semiconductor opening area;
[0096] S7, forming a conductive film layer to fully cover the back surface obtained in S6;
[0097] S8, performing a third etching on the conductive film layer located between the first semiconductor opening region and the second semiconductor opening region on the back side obtained in S7 to form an insulating groove;
[0098] S9. Form metal electrodes on the outer surfaces of the conductive film layer corresponding to the first semiconductor opening region and the second semiconductor opening region on the back side.
[0099] The second etching of the present invention can be performed by laser or mask etching, as long as the corresponding semiconductor opening area can be formed. The laser can be ultraviolet or green laser, and preferably the pulse width of the laser is less than 100ns.
[0100] The widths of the first semiconductor opening region and the second semiconductor opening region can be determined according to the range of the prior art and actual needs. For example, the width W1 of the second semiconductor opening region can be 400-800 μm, and the width W2 of the first semiconductor opening region can be 100-350 μm.
[0101] S7 The formation of the conductive film layer and its thickness and type can refer to the methods of the prior art, for example, physical vapor deposition technology (PVD) or activated plasma deposition technology (RPD) can be used. Exemplarily, the thickness of the conductive film layer is 40-80nm, and the material of the conductive film layer can be an indium oxide-based film doped with at least one of tin, tungsten, titanium, and zinc, or an aluminum and / or boron-doped zinc oxide-based film.
[0102] S8 The third etching can refer to the existing method, for example, mask etching or laser etching can be used. After etching, the resistance between the first semiconductor opening area and the second semiconductor opening area is greater than 1 kΩ. The width of the insulating groove can be, for example, 20-100 μm.
[0103] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0104] Example 1
[0105] A combined passivated back contact cell, such as Figure 1 As shown, the steps of the subsequent velvet making method are as follows:
[0106] S1, providing a double-sided polished silicon wafer 1;
[0107] The N-type single crystal silicon wafer 1 is double-sided polished and cleaned, and the silicon wafer 1 is a Czochralski single crystal silicon wafer.
[0108] S2, forming a first semiconductor layer and a mask layer in sequence on the back side, wherein the first semiconductor layer includes a tunneling oxide layer 2 and an N-type first doped polycrystalline layer 3 formed in sequence on the back side;
[0109] The thickness of the tunnel oxide layer 2 is 1.5 nm, the thickness of the first doped polycrystalline layer 3 is 100 nm, and the effective doping concentration is 1e20 cm -3 .
[0110] The mask layer is silicon nitride and has a thickness of 70 nm.
[0111] S3, performing a first laser etching on the back side of the first semiconductor layer to remove the mask layer and a portion of the first semiconductor layer, thereby forming second semiconductor opening regions distributed at intervals;
[0112] The laser used in the first laser etching is an ultraviolet laser with a pulse width of 10 ns. The width W1 of the formed second semiconductor opening region is 500 μm.
[0113] S4, texturing and cleaning, forming a velvet surface in the second semiconductor opening area on the back and on the front at the same time; the steps of texturing and cleaning are: pre-cleaning - water washing - polishing - water washing - primary alkaline washing - water washing - texturing - water washing - secondary alkaline washing - water washing - acid washing - water washing - HF - water washing - slow pulling - drying, the HF cleaning process removes the mask layer. The slow pulling process is to slowly pull the silicon wafer out of the hot water, and the conditions for slow pulling include: the temperature of the hot water is 50°C, and the pulling time is 90s. The metallographic picture of the second semiconductor opening area after this step is as follows Figure 3 As shown, it can be seen that the laser opening area is completely free of velvet and the velvet is evenly removed.
[0114] The pre-cleaning solution used is a mixed aqueous solution containing NH4OH and H2O2, the mass concentration of NH4OH is 3.5%, the concentration of H2O2 is 5%, the reaction temperature is 80°C, and the reaction time is 2 minutes.
[0115] The polishing liquid is a mixed solution of alkali, polishing additive and water, wherein the alkali is potassium hydroxide with a mass concentration of 2%, the mass concentration of the polishing additive is 1.5%, and the pH of the polishing liquid is 12. The reaction temperature is 65°C, the reaction time is 90s, and the single-sided corrosion depth is within 1μm. The components of the polishing additive are: based on the total mass of the polishing additive, 0.8% benzoic acid, 0.5% ethylenediaminetetramethylenephosphoric acid, 0.2% polyethylene glycol, 0.5% sodium silicate, and the balance is pure water.
[0116] The conditions of the first and second alkaline washings are the same: the alkaline washing solution is a mixed aqueous solution of NH4OH and H2O2, the mass concentration of NH4OH is 3.5%, the mass concentration of H2O2 is 5%, the reaction temperature is 80°C, and the reaction time is 4 minutes.
[0117] The texturing solution is a mixed solution of 2% tetramethylammonium hydroxide (TMAH), 1% texturing additive and water. The texturing conditions are: reaction temperature 70°C, reaction time 12 minutes, single-sided etching depth of silicon wafer after texturing is 2-3μm, and surface reflectivity is less than 10%.
[0118] The pickling solution is a mixed aqueous solution of HCl and H2O2, with a mass concentration of HCl of 4.8% and a mass concentration of H2O2 of 5%. The pickling conditions are: reaction temperature of 60°C and reaction time of 4 minutes.
[0119] The mass concentration of HF solution is 8%, the reaction temperature is 30°C, and the reaction time is 240s.
[0120] The water washing is performed by overflow of pure water, and the water washing time is 120 seconds. The water washing after each step of solution can completely remove the chemical solution remaining on the surface of the silicon wafer 1.
[0121] S5, forming a passivation layer 7 and an anti-reflection layer 8 on the front side, and forming a second semiconductor layer on the back side, wherein the second semiconductor layer includes an intrinsic amorphous silicon layer 4 and a P-type second doped amorphous silicon layer 5 sequentially formed on the back side;
[0122] The thickness of the intrinsic amorphous silicon layer 4 is 10 nm, the thickness of the second doped amorphous silicon layer 5 is 15 nm, and the effective doping concentration is 1e19 cm -3 .
[0123] S6. Perform a second etching on the second semiconductor layer corresponding to the polishing area on the back side to remove the second semiconductor layer and form a first semiconductor opening area; the width W2 of the first semiconductor opening area is 300 μm.
[0124] S7, forming a conductive film layer 6 on the back surface to fully cover the back surface;
[0125] The transparent conductive film layer 6 has a thickness of 60 nm and is made of a tin-doped indium oxide-based thin film.
[0126] S8, performing a third etching on the conductive film layer 6 on the back side to form an insulating groove;
[0127] The width W3 of the insulating groove is 50 μm, and the resistance between the first semiconductor opening region and the second semiconductor opening region after etching is greater than 1 kΩ.
[0128] S9, forming metal electrodes 9 on the outer surfaces of the first semiconductor opening region and the second semiconductor opening region on the back side respectively.
[0129] Example 2
[0130] The method of Example 1 is referred to, except that the composition of the polishing additive is different, wherein the concentration of ethylenediaminetetramethylenephosphonic acid is 2%, the contents of benzoic acid, polyethylene glycol and sodium silicate are unchanged, and the pH of the polishing liquid is 12.
[0131] Example 3
[0132] The method of Example 1 is used, except that the polishing time is 300 s.
[0133] Example 4
[0134] The method of Example 1 is referred to, except that the thickness of the mask layer is 30 nm.
[0135] Example 5
[0136] The method of Example 1 is followed, except that instead of performing an alkali wash and a subsequent water wash, texturing - water wash - secondary alkali wash - water wash - acid wash - water wash - HF - water wash - slow pulling - drying are directly performed after polishing and water wash.
[0137] Example 6
[0138] The method of Example 1 was followed, except that the polishing temperature was 85°C.
[0139] Comparative Example 1
[0140] The method of Example 1 is referred to, except that polishing is not performed in S4, texturing and cleaning.
[0141] Comparative Example 2
[0142] The method of Example 1 is referred to, except that the concentration of ethylenediaminetetramethylenephosphonic acid in the polishing additive is 0.01%, and the contents of benzoic acid, polyethylene glycol and sodium silicate remain unchanged.
[0143] Test Case
[0144] The combined passivation back contact cells obtained in the above examples and comparative examples were subjected to performance tests, and the results are shown in Table 1.
[0145] Table 1
[0146]
[0147] It can be seen from the above results that, compared with the comparative example, the embodiment of the present invention can solve the problem of incomplete velvet after laser opening, which is beneficial to improve the opening voltage, short-circuit current and battery conversion efficiency.
[0148] Furthermore, according to Example 1 and Examples 2-6, it can be seen that the use of the preferred manufacturing process of the present invention is more conducive to improving the opening voltage, short-circuit current and battery conversion efficiency.
[0149] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A post-texturing method for a combined passivation back contact battery, characterized in that: The steps include: S1, provide double-sided polished silicon wafers; S2, forming a first semiconductor layer and a mask layer in sequence on the back side of the silicon wafer; the mask layer has a thickness of 30-90 nm; the first semiconductor layer comprises a tunneling oxide layer and a first doped polycrystalline layer; S3, performing a first laser etching on the first semiconductor layer and its corresponding mask layer in a preset area on the back surface obtained in S2, removing the mask layer and a portion of the first semiconductor layer in the preset area, and forming a second semiconductor opening area distributed at intervals; S4, texturing and cleaning, forming a texturing surface in the second semiconductor opening region on the back side and on the front side at the same time, and removing the mask layer; the texturing and cleaning process at least includes pre-cleaning, polishing, and texturing; The polishing liquid used in the polishing is a mixed solution containing alkali, polishing additives and water, the pH of the polishing liquid is 11-13, the mass concentration of the alkali in the polishing liquid is 1%-3%, the mass concentration of the polishing additive in the polishing liquid is 0.5%-2%, the polishing additive contains ethylenediaminetetramethylenephosphonic acid, benzoic acid, polyethylene glycol and sodium silicate and water, based on the total amount of the polishing additive, the concentration of ethylenediaminetetramethylenephosphonic acid in the polishing additive is 0.1%-2%, the concentration of benzoic acid is 0.5%-2%, the concentration of sodium silicate is 0.1%-2%, and the concentration of polyethylene glycol is 0.1%-0.5%; The polishing conditions include: reaction temperature of 60°C-85°C, reaction time of 30-300s; S5. Form a passivation layer and an anti-reflection layer on the front side of the silicon wafer obtained in S4, and form a second semiconductor layer on the back side, wherein the second semiconductor layer comprises an intrinsic amorphous silicon layer and a second doped silicon layer.
2. The post-texturing method for manufacturing a combined passivation back contact cell according to claim 1, characterized in that: The alkali is potassium hydroxide or sodium hydroxide.
3. The post-texturing method for manufacturing a combined passivation back contact cell according to claim 1, characterized in that: During the polishing, the single-side corrosion depth is controlled to be within 1 μm; And / or, when the thickness of the mask layer is 50-69 nm, the concentration of ethylenediaminetetramethylenephosphonic acid in the polishing additive is controlled to be 1.1%-2%; when the thickness of the mask layer is 70-90 nm, the concentration of ethylenediaminetetramethylenephosphonic acid in the polishing additive is controlled to be 0.1%-1.0%.
4. The post-texturing method for manufacturing a combined passivation back contact cell according to claim 1, characterized in that: The pre-cleaning solution used in the pre-cleaning is a mixed solution containing NH4OH and H2O2 or a mixed solution containing a strong base and H2O2, wherein the strong base is KOH and / or NaOH, and the mass concentration of NH4OH or the strong base in the pre-cleaning solution is 2%-5%, and the mass concentration of H2O2 is 3%-5%; the pre-cleaning conditions include: a reaction temperature of 60-80°C and a reaction time of 2-4min; and / or, The texturing liquid used in the texturing is a mixed solution of tetramethylammonium hydroxide, a texturing additive and water. Based on the total weight of the texturing liquid, the mass concentration of tetramethylammonium hydroxide is 1%-2%, and the mass concentration of the texturing additive is 0.5%-2%. The texturing conditions include: the reaction temperature is 60℃-80℃, the reaction time is 8-15min, the single-sided corrosion depth of the silicon wafer after texturing is 2-3μm, and the surface reflectivity is less than 10% after texturing.
5. The post-texturing method for manufacturing a combined passivation back contact cell according to any one of claims 1 to 4, characterized in that: The texturing and cleaning process also includes: water washing between pre-cleaning and polishing, and after polishing, water washing, one alkali washing, water washing, texturing, water washing, two alkali washings, and water washing are sequentially performed.
6. The post-texturing method for manufacturing a combined passivation back contact cell according to claim 5, characterized in that: The alkaline washing solution used in alkaline washing is a mixed solution containing NH4OH and H2O2 or a mixed solution containing a strong base and H2O2, wherein the strong base is KOH and / or NaOH, and the mass concentration of NH4OH or the strong base in the alkaline washing solution is 2%-5%, and the mass concentration of H2O2 is 3%-5%; And / or, the conditions for alkaline washing include: reaction temperature of 60-80° C., reaction time of 2-4 min.
7. The post-texturing method for manufacturing a combined passivation back contact cell according to claim 5, characterized in that: The texturing and cleaning process also includes: after the secondary alkaline washing and water washing, acid washing, water washing, HF washing, and water washing are performed in sequence, and whether to perform slow pulling and drying is selected according to demand. The slow pulling process includes slowly pulling the silicon wafer out of the hot water. The conditions for slow pulling include: the temperature of the hot water is 45-55°C, and the pulling time is 60-120s.
8. The post-texturing method for manufacturing a combined passivation back contact cell according to claim 7, characterized in that: The pickling solution used in the pickling is a mixed solution containing HCl and H2O2 or a mixed solution containing HCl and O3. Based on the total amount of the pickling solution, the mass concentration of HCl is 2%-5%, the mass concentration of H2O2 is 3%-5%, and the concentration of O3 is 5ppm-10ppm; the pickling conditions include: a reaction temperature of 60-80°C and a reaction time of 2-4min; and / or, The mass concentration of HF in the HF solution used for the HF washing is 5%-10%. The conditions for the HF washing include: a reaction temperature of 20-35° C. and a reaction time of 120-300 s.
9. The post-texturing method for manufacturing a combined passivation back contact cell according to claim 5, characterized in that: The water washing is pure water overflow, and each washing time is 90-150s.
10. The post-texturing method for manufacturing a combined passivation back contact cell according to claim 1, characterized in that: The post-texturing method for the combined passivation back contact cell also includes: S6, performing a second etching on a portion of the second semiconductor corresponding to the polished area on the back side obtained in S5 to remove the second semiconductor layer and form a first semiconductor opening area; S7, forming a conductive film layer to fully cover the back surface obtained in S6; S8, performing a third etching on the conductive film layer located between the first semiconductor opening region and the second semiconductor opening region on the back side obtained in S7 to form an insulating groove; S9. Form metal electrodes on the outer surfaces of the conductive film layer corresponding to the first semiconductor opening region and the second semiconductor opening region on the back side.