A preparation process of hard carbon composite material and its products and applications

Through the hot-pressing composite of sugar hard carbon materials and B and N co-doped porous carbon and the temperature-sensitive gel pore plugging treatment, the problems of density and pore structure stability of hard carbon composite materials were solved, and high-performance hard carbon was realized. Composite material preparation for energy applications such as lithium-ion batteries.

CN118099358BActive Publication Date: 2024-10-08CARBON ONE NEW ENERGY HANGZHOU CO LTD +1
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202410518219.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-10-08
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

Hard carbon composite materials often face problems such as insufficient density, unstable pore structure, and uneven performance during the preparation process. Traditional hot-pressing composite technology is difficult to control the microstructure, and the pore plugging treatment method is complex and inefficient.

Method used

The sugar hard carbon material and B and N co-doped porous carbon are hot-pressed and composited, and the pores are blocked by temperature-sensitive gel, combined with high-temperature carbonization process to control the pore structure and performance.

Benefits of technology

A hard carbon composite material with good battery cycle performance, high rate performance and stability is prepared, which improves the material's specific surface area and adsorption performance and is suitable for energy storage and conversion fields such as secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118099358B_ABST
    Figure CN118099358B_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation process of a hard carbon composite material, its products and applications. A preparation process method of a hard carbon composite material comprises the steps of: preparation of B and N co-doped porous carbon, preparation of hard carbon material, hot pressing composite, pore plugging treatment and the like. The B and N doped porous hard carbon composite material prepared by the method has no obvious volume effect, and has the advantages of good battery cycle performance, high rate performance, good stability, high energy density, etc., and has good application prospects in energy storage and conversion fields such as secondary batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation process of a hard carbon composite material, a product thereof and an application thereof, and belongs to the field of lithium ion batteries. Background Art

[0002] With the increasing demand for energy and the urgent need for environmental protection, the research and application of new energy materials have become a hot topic in the fields of science and industry. As a material with excellent electrochemical properties, hard carbon composites have shown great application potential in energy storage and conversion fields such as lithium-ion batteries and supercapacitors. However, hard carbon composites often face challenges such as insufficient density, unstable pore structure, and uneven performance during the preparation process, which restricts their practical application.

[0003] Hot pressing composite technology is one of the key processes for preparing hard carbon composite materials. Through hot pressing composite, different materials can be well combined under high temperature and high pressure conditions to improve the overall performance of the composite material. In the hot pressing composite process, the control of parameters such as temperature, pressure and time is crucial. Appropriate temperature can promote diffusion and reaction between materials and improve bonding strength; suitable pressure can eliminate the gaps between materials and improve the density of composite materials. However, traditional hot pressing composite technology often finds it difficult to achieve precise control of the microstructure of the material, resulting in instability in the performance of the composite material. In order to solve the problem of unstable pore structure in hard carbon composite materials, pore plugging treatment technology has emerged. Pore plugging treatment mainly improves the stability and performance of the material by filling the pores and reducing the porosity of the material. At present, common pore plugging treatment methods include impregnation method, coating method, etc. Although these methods can improve the pore structure of the material to a certain extent, they often have problems such as complex operation and low efficiency. In addition, the selection of pore plugging materials is also crucial. Different pore plugging materials have different effects on the performance of composite materials. Summary of the invention

[0004] In order to overcome the above technical problems existing in the prior art, the first object of the present invention is to provide a preparation process of a hard carbon composite material.

[0005] The first technical purpose of the present invention is achieved through the following technical solutions:

[0006] A process for preparing a hard carbon composite material, comprising:

[0007] After the sugar hard carbon material is crushed, a conductive agent, B and N co-doped porous carbon are added for hot pressing and compounding, followed by pore blocking and high temperature carbonization to obtain a hard carbon composite material;

[0008] The pore plugging agent used in the pore plugging treatment process includes gel.

[0009] Preferably, the gel comprises a thermosensitive gel; preferably at least one of a chitosan-based thermosensitive gel, a poly N-isopropylacrylamide (PNIPAAm) gel, or a hyaluronic acid (HA)-based thermosensitive gel.

[0010] Preferably, the sugar-based hard carbon material includes at least one of glucose-based hard carbon, sucrose-based hard carbon or starch-based hard carbon;

[0011] Furthermore, the method for preparing the sugar hard carbon material comprises:

[0012] The sugar particles are sieved and dissolved in an appropriate amount of deionized water to form a sugar solution;

[0013] Adding polyvinyl pyrrolidone and polyvinylidene fluoride as auxiliary agents to the sugar solution, followed by freeze drying to remove moisture;

[0014] The freeze-dried sugar sample is carbonized, acid-washed and dried under an inert atmosphere to obtain a sugar hard carbon material.

[0015] Furthermore, the sugar particles are sieved to a particle size of 160-200 mesh;

[0016] Furthermore, the concentration of the sugar solution is 0.01-0.5 mol / L;

[0017] Further, the auxiliary agent includes at least one of polyvinylpyrrolidone or polyvinylidene fluoride;

[0018] Furthermore, the mass ratio of the adjuvant to the sugar is 1:5~11;

[0019] Furthermore, the carbonization treatment is carried out under an inert atmosphere;

[0020] Furthermore, the carbonization treatment temperature is 600~700°C, and the treatment time is 1~5h.

[0021] Preferably, the method for preparing the B and N co-doped porous carbon comprises:

[0022] Take o-phenanthroline, K2B4O7, (CH3COO)2Zn and grind them evenly;

[0023] Under inert atmosphere, high temperature treatment is carried out by step-by-step heating;

[0024] The high temperature reaction product is taken, immersed and stirred in an acid solution, washed and filtered with distilled water, and dried to obtain B and N co-doped porous carbon.

[0025] Furthermore, the mass ratio of o-phenanthroline, K2B4O7, and (CH3COO)2Zn is 1:2~6:1;

[0026] Further, the heating method is: heating to 100~120°C at a heating rate of 0.2~0.8°C / min, and reacting at a constant temperature for 0.1~0.5h; then heating to 320~350°C at a heating rate of 0.4~1.6°C / min, and reacting at a constant temperature for 0.2~0.8h; finally heating to 700~760°C at a heating rate of 2~5°C / min, and reacting at a constant temperature for 1~2h;

[0027] Further, the acid solution is 1-2 mol / L HCl solution, and the immersion stirring time is 30-60 min;

[0028] Furthermore, the drying temperature is 100-120° C., and the drying time is 8-14 h.

[0029] Preferably, the hot pressing composite process comprises taking a sugar-based hard carbon material, adding a conductive agent and mixing, then adding B and N co-doped porous carbon material, and performing hot pressing composite after pre-pressing;

[0030] Furthermore, the sugar hard carbon material is crushed and sieved to a particle size of 160-200 mesh;

[0031] Furthermore, the mass ratio of the sugar hard carbon material to the conductive agent is 1:0.2~1;

[0032] Furthermore, the mass ratio of the sugar hard carbon material containing the conductive agent to the B and N co-doped porous carbon material is 1:0.8~1.5;

[0033] Further, the conductive agent includes at least one of graphene, conductive graphite, conductive carbon black, conductive carbon fiber, carbon nanotubes, Ketjen black or acetylene black;

[0034] Furthermore, the pre-pressing temperature is 20-35°C, the pre-pressing pressure is 10-20 MPa, and the pre-pressing time is 10-20 min;

[0035] Furthermore, the hot pressing composite temperature is 800-1200° C., the hot pressing composite pressure is 30-50 MPa, and the hot pressing composite time is 30-60 min.

[0036] Preferably, the pore plugging treatment process includes applying a pore plugging agent to the hard carbon material after hot pressing and compounding, causing a phase change under a set temperature and electric field to complete the pore plugging treatment;

[0037] Furthermore, the mass ratio of the pore plugging agent to the hard carbon product after hot pressing is 0.5~1.5:1;

[0038] Further, the plugging treatment temperature is 25-40°C;

[0039] Furthermore, the electric field strength is 50-110 V / cm.

[0040] Preferably, the high-temperature carbonization process parameters include a carbonization temperature of 1100-1500° C., a heating rate of 2-5° C. / min, and a constant temperature time of 2-5 h.

[0041] The present invention prepares a hard carbon composite material, which has the advantages of good battery cycle performance, high rate performance and good stability, high energy density, etc., and has good application prospects in the field of energy storage and conversion such as secondary batteries.

[0042] A second object of the present invention is to provide a hard carbon composite product.

[0043] The second technical purpose of the present invention is achieved through the following technical solutions:

[0044] A hard carbon composite material, prepared according to the preparation method of the hard carbon composite material;

[0045] The hard carbon composite material has a particle size D50 of 5 to 8 μm and a specific surface area of ​​7 to 13 m 2 / g, tap density is 0.4~0.8g / cm 3 , closed pore volume is 0.10~0.25cm 3 / g.

[0046] A third object of the present invention is to provide an application of a hard carbon composite material.

[0047] The third technical objective of the present invention is achieved through the following technical solutions:

[0048] A negative electrode sheet comprises a hard carbon material prepared from the hard carbon composite material.

[0049] A lithium ion battery comprises the negative electrode sheet.

[0050] An electrochemical device comprises the lithium-ion battery.

[0051] In summary, the beneficial effects of the present invention are:

[0052] 1. The present invention uses B and N co-doped porous carbon as one of the main raw materials for preparing hard carbon composite materials. The incorporation of B and N can regulate the pore structure of porous carbon, making it have a more uniform pore size distribution and a higher specific surface area, effectively improving the conductivity of porous carbon and enhancing the chemical stability of porous carbon. Moreover, the addition of B and N co-doped porous carbon may also enhance the mechanical properties of hard carbon composite materials.

[0053] 2. The present invention uses sugar as a raw material to prepare hard carbon materials, which contain multiple hydroxyl groups and can form a rich cross-linked structure during the carbonization process, thereby preparing hard carbon materials with different pore structures and morphologies. At the same time, polyvinyl pyrrolidone is used as an auxiliary agent in the preparation of sugar hard carbon, which can act as a template or catalyst in the subsequent carbonization process, helping to form a hard carbon material with a specific structure or performance.

[0054] 3. The present invention creatively uses gel, especially thermosensitive gel such as chitosan-based thermosensitive gel as a pore plugging agent, which can undergo phase change at a specific temperature, making the pore plugging process more precise and controllable. The thermosensitive gel has good adhesion and filling properties, making the pore plugging effect more uniform and reliable, reducing porosity, increasing the uniformity and connectivity of the pores, and improving its specific surface area and adsorption performance.

[0055] Therefore, the hard carbon composite material provided by the present invention has the advantages of good battery cycle performance, high rate performance, good stability, high energy density, etc., and has good application prospects in energy storage and conversion fields such as secondary batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0057] Figure 1 is a process flow chart of the preparation of the hard carbon composite material in Example 1;

[0058] Figure 2 is a SEM image of the hard carbon composite material prepared in Example 1. DETAILED DESCRIPTION

[0059] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0060] The present invention provides a preparation process of a hard carbon composite material, which specifically comprises the following steps:

[0061] Step (1) Preparation of B and N co-doped porous carbon

[0062] S11 Take o-phenanthroline, K2B4O7, and (CH3COO)2Zn and grind them evenly in a mortar (weigh and grind under vacuum), and transfer them to a tube furnace;

[0063] S12 is heated to a suitable temperature at a certain heating rate and kept at a constant temperature for a period of time;

[0064] S13 is then heated to a higher temperature at a certain heating rate and reacted at a constant temperature for a period of time;

[0065] S14 is finally heated to a higher temperature at a certain heating rate, reacted at a constant temperature for a period of time, and then gradually cooled to room temperature in a nitrogen environment;

[0066] S15 Take out the high temperature reaction product, add an appropriate amount of HCl solution, seal and stir for a period of time, then wash and filter with distilled water, wash several times until the pH value of the filtrate is close to neutral;

[0067] S16 drying the washed product in an oven for a period of time to obtain B and N co-doped porous carbon;

[0068] Preferably, the preparation of B and N co-doped porous carbon in step (1) comprises the following steps: S11, o-phenanthroline, K2B4O7 and (CH3COO)2Zn are taken in a mortar in a mass ratio of 1:2-6:1, and ground evenly (weighed and ground in a vacuum environment), and then transferred to a tube furnace; S12, nitrogen is introduced, and the mixture is heated to 100-120°C at a heating rate of 0.2-0.8°C / min, and the mixture is reacted at a constant temperature for 0.1-0.5h; S13, the mixture is heated to 320-350°C at a heating rate of 0.4-1.6°C / min, and the mixture is reacted at a constant temperature for 0.2-0.8h; S14, the mixture is heated to 700-760°C at a heating rate of 2-5°C / min, and the mixture is reacted at a constant temperature for 1-2h, and then the mixture is gradually cooled to room temperature in a nitrogen environment; S15, the high temperature reaction product is taken out, 1-2mol / L The HCl solution is sealed and stirred for 30-60 min, then washed and filtered with distilled water for 3-6 times until the pH value of the filtrate is close to neutral; S16 The washed product is dried in an oven at 100-120°C for 8-14 h to obtain B and N co-doped porous carbon.

[0069] In this method, B and N co-doped porous carbon is used as one of the main raw materials for preparing hard carbon composites. The incorporation of B and N can effectively improve the electrical conductivity of porous carbon, which is crucial for the application of hard carbon composites in the field of electrochemistry. The improvement of electrical conductivity helps to enhance the electrochemical properties of composites; the incorporation of B and N can enhance the chemical stability of porous carbon, so that it can still maintain good performance under high temperature or strong acid and alkali environment; the incorporation of B and N can regulate the pore structure of porous carbon, so that it has a more uniform pore size distribution and a higher specific surface area. Moreover, the addition of B and N co-doped porous carbon can enhance the mechanical properties of hard carbon composites, such as hardness, flexural strength, etc. This helps to improve the stability and reliability of composite materials in practical applications.

[0070] Step (2) Preparation of sugar hard carbon material

[0071] S21 takes glucose particles and sieves them to obtain glucose particles of suitable particle size;

[0072] S22 dissolves glucose powder in an appropriate amount of deionized water to form a glucose solution, and stirs continuously;

[0073] S23 adding an appropriate amount of polyvinyl pyrrolidone as an auxiliary agent to the glucose solution;

[0074] S24 freeze-drying the glucose solution to remove water therein;

[0075] S25 placing the freeze-dried glucose sample in a carbonization furnace for carbonization treatment under an inert atmosphere;

[0076] After the carbonization in S26, the sample was allowed to cool naturally to room temperature, and was acid-washed with an appropriate amount of hydrochloric acid, and then dried to obtain a sugar hard carbon material;

[0077] Preferably, the preparation of the sugar hard carbon material in step (2) comprises the following steps: S21 taking glucose particles and sieving to obtain glucose particles of 160-200 mesh; S22 dissolving glucose powder in an appropriate amount of deionized water to form a glucose solution with a concentration of 0.02-0.5 mol / L, and stirring continuously; S23 adding polyvinyl pyrrolidone as an auxiliary agent to the glucose solution, wherein the mass ratio of the auxiliary agent to glucose is 1:5-11; S24 freeze-drying the glucose solution for 2-8 hours to remove moisture therein; S25 placing the freeze-dried glucose sample in a carbonization furnace and carbonizing it at 600-750°C under an inert atmosphere for 1-5 hours; S26 after the carbonization is completed, allowing the sample to cool naturally to room temperature, and pickling it with 50-80 mL of 0.8-1.2 mol / L hydrochloric acid, and then drying it to obtain the sugar hard carbon material.

[0078] In this method, in the process of using glucose and other sugars as raw materials to prepare hard carbon materials, polyvinyl pyrrolidone is used as an auxiliary agent, which can act as a template or catalyst in the subsequent carbonization process, helping to form hard carbon materials with specific structures or properties, and freezing the glucose solution. This freeze-drying can maintain the original structure of the solution and avoid cracks or deformation during the drying process. In addition, glucose molecules contain multiple hydroxyl groups, which can form rich cross-linked structures during the carbonization process, thereby preparing hard carbon materials with different pore structures and morphologies.

[0079] Step (3) Hot pressing and lamination

[0080] S31: crushing the sugar hard carbon material and sieving it to obtain sugar hard carbon particles with a suitable particle size;

[0081] S32 adding graphene to sugar hard carbon particles and mixing them thoroughly;

[0082] S33: placing the sugar hard carbon mixed raw material after graphene and the B and N co-doped porous carbon material into a hot pressing mold, first pre-pressing, and then hot-pressing and compounding the whole;

[0083] Preferably, step (3) hot pressing composite includes the following steps: S31: crushing the sugar hard carbon material, and obtaining 160-200 mesh sugar hard carbon particles through screening; S32: adding graphene to the hard carbon particles, with the mass ratio of the sugar hard carbon material to the graphene being 1:0.2-1, and fully mixing; S33: placing the hard carbon mixed raw material after graphene and the B and N co-doped porous carbon material into a hot pressing mold at a mass ratio of 1:0.8-1.5, first pre-pressing at 20-35°C, 10-20MPa, 10-20min, and then completing the overall hot pressing composite at 800-1200°C, 30-50MPa, 30-60min. The specific surface area of ​​the product obtained in this step is 185-210m 2 / g.

[0084] In this method, the hot pressing composite technology can promote the interface bonding between the hard carbon material and the B, N co-doped porous carbon through the action of high temperature and high pressure, making the contact between the two closer and forming a stronger chemical bond or physical adsorption. This enhanced interface bonding helps to improve the mechanical strength, electrical conductivity and thermal stability of the composite material. During the hot pressing composite process, the pore structure of the B, N co-doped porous carbon can be further optimized. Moreover, the conditions of high temperature and high pressure can promote the rearrangement between carbon atoms and the shrinkage of the pore structure, thereby obtaining a more uniform, fine pore size distribution and a higher specific surface area. This helps to improve the adsorption performance and ion transfer efficiency of the composite material. Through hot pressing composite, the B, N co-doped porous carbon can be evenly dispersed in the hard carbon material to form a stable composite material structure. This structure can resist the influence of the external environment (such as high temperature, oxidation, etc.) and improve the stability of the composite material.

[0085] Step (4) Hole plugging

[0086] Take an appropriate amount of chitosan-based thermosensitive gel as a pore plugging agent and fully apply it on the hard carbon material after hot pressing and compounding. Then, a phase change occurs at a certain temperature and in a certain electric field to complete the pore plugging treatment.

[0087] Preferably, the pore plugging treatment process in step (4) comprises: taking chitosan-based thermosensitive gel as a pore plugging agent by mass, and fully applying the chitosan-based thermosensitive gel on the hard carbon material after hot pressing and compounding, wherein the mass ratio of the chitosan-based thermosensitive gel to the hard carbon product after hot pressing and compounding is 0.5-1.5:1, and then a phase change occurs at 25-40°C and within an electric field strength of 50-110V / cm to complete the pore plugging treatment.

[0088] In this method, chitosan-based thermosensitive gel is creatively used as a pore plugging agent. Chitosan-based thermosensitive gel can undergo a phase change at a specific temperature, from liquid to solid or semi-solid. This temperature responsiveness makes the pore plugging process more precise and controllable, thereby optimizing the performance of the composite material. Chitosan-based thermosensitive gel has good adhesion and filling properties, can fit tightly to the pores on the surface of porous carbon, and effectively fill the pores. This characteristic makes the pore plugging effect more uniform and reliable, and improves the overall performance of the composite material. The pore plugging process can accurately control the pore structure of porous carbon, including pore size, pore morphology and pore distribution. By plugging the pores, the porosity can be reduced, the uniformity and connectivity of the pores can be increased, thereby optimizing the pore structure of the composite material and improving its specific surface area and adsorption performance. The pore plugging treatment can enhance the structural stability of porous carbon and reduce defects and stress concentration points inside the pores. This helps to improve the creep resistance, thermal shock resistance and long-term stability of the composite material, so that it can still maintain good performance in harsh environments such as high temperature and high humidity.

[0089] Step (5) Preparation of hard carbon composite material

[0090] The product after the pore plugging treatment is subjected to high-temperature carbonization treatment in an inert atmosphere and under specific temperature conditions to obtain a hard carbon composite material.

[0091] Preferably, step (5) of preparing the hard carbon composite material comprises: taking the product after the pore plugging treatment and pyrolyzing it for 2 to 5 hours in an inert atmosphere at a temperature of 1100 to 1500° C. and a heating rate of 2 to 5° C. / min to obtain the hard carbon composite material.

[0092] Another object of the present invention is to provide a hard carbon composite material, wherein the particle size D50 of the hard carbon composite material is 5-8 μm, and the specific surface area is 7-13 m 2 / g, tap density is 0.4~0.8g / cm 3 , closed pore volume is 0.10~0.25cm 3 / g.

[0093] The chitosan-based thermosensitive gel used in the examples of the present invention was ordered from Xi'an Qiyue Biotechnology Co., Ltd. and was in a low-viscosity flow state at room temperature; the PEG-based gel used was purchased from Shanghai Yuanye Biotechnology Co., Ltd., item number S28550.

[0094] Example 1

[0095] The present invention provides a method for preparing a hard carbon composite material, the process flow is as follows Figure 1 As shown, the specific steps include:

[0096] Step (1) Preparation of B and N co-doped porous carbon

[0097] S11 Take 4g of o-phenanthroline, 18g of K2B4O7, and 4g of (CH3COO)2Zn and grind them evenly in a mortar (weigh and grind under vacuum), and transfer them to a tube furnace;

[0098] S12 was introduced with nitrogen, heated to 100°C at a heating rate of 0.2°C / min, and kept at this temperature for 0.1h;

[0099] S13 was then heated to 320°C at a heating rate of 0.4°C / min and kept at this temperature for 0.2h;

[0100] S14 was finally heated to 700 °C at a heating rate of 2 °C / min, kept at this temperature for 1 h, and then gradually cooled to room temperature in a nitrogen environment;

[0101] S15 Take out the high temperature reaction product, add 1 mol / L HCl solution, seal and stir for 30 min, then wash and filter with distilled water for 3 times until the pH value of the filtrate is close to neutral;

[0102] S16 The washed product was dried in an oven at 100°C for 8 h to obtain B and N co-doped porous carbon;

[0103] Step (2) Preparation of sugar hard carbon material

[0104] S21 takes glucose particles and sieves them to obtain glucose particles of 160 mesh;

[0105] S22 Dissolve 8 g of glucose powder in an appropriate amount of deionized water to form a glucose solution with a concentration of 0.5 mol / L, stirring continuously;

[0106] S23 Add 1 g of polyvinyl pyrrolidone as an adjuvant to the glucose solution;

[0107] S24 freeze-drying the glucose solution for 2 h to remove water therein;

[0108] S25 The freeze-dried glucose sample was placed in a carbonization furnace and carbonized at 600 °C for 3 h under an inert atmosphere;

[0109] After the carbonization in S26, the sample was allowed to cool naturally to room temperature, and was acid-washed with 50 mL of 1 mol / L hydrochloric acid, and then dried to obtain the sugar hard carbon material;

[0110] Step (3) Hot pressing and lamination

[0111] S31: taking 2 g of sugar hard carbon material, crushing it, and sieving it to obtain 160 mesh sugar hard carbon particles;

[0112] S32: Add 1 g of graphene to the sugar hard carbon particles and mix them thoroughly;

[0113] S33: placing the sugar hard carbon mixed raw material after adding graphene and the B and N co-doped porous carbon material into a hot pressing mold in a mass ratio of 1:1, first pre-pressing at 20° C., 10 MPa, 10 min, and then completing the overall hot pressing compounding at 800° C., 30 MPa, 30 min;

[0114] Step (4) Hole plugging

[0115] Chitosan-based thermosensitive gel was used as a pore plugging agent and was fully applied to the hard carbon material after hot pressing (the mass ratio of chitosan-based thermosensitive gel to the hard carbon product after hot pressing was 0.85:1), and then a phase change occurred at 25°C and within an electric field strength of 50V / cm to complete the pore plugging treatment;

[0116] Step (5) Preparation of hard carbon composite material

[0117] The product after the plugging treatment was pyrolyzed in a nitrogen atmosphere at 1200°C with a heating rate of 3°C / min for 3 h to obtain a hard carbon composite material. The SEM characterization data are as follows: Figure 2 shown.

[0118] Example 2

[0119] Step (1) Preparation of B and N co-doped porous carbon

[0120] S11 Take 5g of o-phenanthroline, 20g of K2B4O7, and 5g of (CH3COO)2Zn and grind them evenly in a mortar (weigh and grind under vacuum), and transfer them to a tube furnace;

[0121] S12 was introduced with nitrogen, heated to 105°C at a heating rate of 0.6°C / min, and kept reacting at this temperature for 0.2h;

[0122] S13 was then heated to 330°C at a heating rate of 0.8°C / min and kept at this temperature for 0.4h;

[0123] S14 was finally heated to 720°C at a heating rate of 3°C / min, kept at this temperature for 1.3h, and then gradually cooled to room temperature under nitrogen atmosphere;

[0124] S15 Take out the high temperature reaction product, add 1.4 mol / L HCl solution, seal and stir for 40 min, then wash and filter with distilled water for 5 times until the pH value of the filtrate is close to neutral;

[0125] S16 The washed product is dried in an oven at 105°C for 10 h to obtain B and N co-doped porous carbon;

[0126] Step (2) Preparation of sugar hard carbon material

[0127] S21 takes glucose particles and sieves them to obtain glucose particles of 170 mesh;

[0128] S22: dissolve 9 g of glucose powder in an appropriate amount of deionized water to form a glucose solution with a concentration of 0.3 mol / L, and stir continuously;

[0129] S23 1.3 g of polyvinyl pyrrolidone was added to the glucose solution as an adjuvant;

[0130] S24 freeze-drying the glucose solution for 4 h to remove water therein;

[0131] S25 The freeze-dried glucose sample was placed in a carbonization furnace and carbonized at 650 °C for 2.5 h under an inert atmosphere;

[0132] After the carbonization in S26, the sample was allowed to cool naturally to room temperature, and was acid-washed with 60 mL of 1 mol / L hydrochloric acid, and then dried to obtain the sugar hard carbon material;

[0133] Step (3) Hot pressing and lamination

[0134] S31: 3 g of sugar hard carbon material is crushed and sieved to obtain 170 mesh hard carbon particles;

[0135] S32: 1.3 g of graphene was added to the sugar hard carbon particles and mixed thoroughly;

[0136] S33: placing the sugar hard carbon mixed raw material after adding graphene and the B and N co-doped porous carbon material into a hot pressing mold at a mass ratio of 1:1.2, first pre-pressing at 25° C., 14 MPa, 14 min, and then completing the overall hot pressing compounding at 900° C., 35 MPa, 40 min;

[0137] Step (4) Hole plugging

[0138] Chitosan-based thermosensitive gel was used as a pore plugging agent and was fully applied to the hard carbon material after hot pressing (the mass ratio of chitosan-based thermosensitive gel to the hard carbon product after hot pressing was 1:1), and then a phase change occurred at 30°C and within an electric field strength of 70V / cm to complete the pore plugging treatment;

[0139] Step (5) Preparation of hard carbon composite material

[0140] The product after the pore plugging treatment was pyrolyzed for 4 h in a nitrogen atmosphere at 1100°C with a heating rate of 4°C / min to obtain a hard carbon composite material.

[0141] Example 3

[0142] Step (1) Preparation of B and N co-doped porous carbon

[0143] S11 Take 6g of o-phenanthroline, 22g of K2B4O7, and 6g of (CH3COO)2Zn and grind them evenly in a mortar (weigh and grind under vacuum), and transfer them to a tube furnace;

[0144] S12 was introduced with nitrogen, heated to 115°C at a heating rate of 0.6°C / min, and kept reacting at this temperature for 0.4h;

[0145] S13 was then heated to 340°C at a heating rate of 1.2°C / min and kept at this temperature for 0.6h;

[0146] S14 was finally heated to 750°C at a heating rate of 4°C / min, kept at this temperature for 1.6 h, and then gradually cooled to room temperature under a nitrogen environment;

[0147] S15 Take out the high temperature reaction product, add 1.6 mol / L HCl solution, seal and stir for 50 min, then wash and filter with distilled water for 5 times until the pH value of the filtrate is close to neutral;

[0148] S16 The washed product was dried in an oven at 115°C for 10 h to obtain B and N co-doped porous carbon;

[0149] Step (2) Preparation of sugar hard carbon material

[0150] S21 takes glucose particles and sieves them to obtain glucose particles of 180 mesh;

[0151] S22 Dissolve 10 g of glucose powder in an appropriate amount of deionized water to form a glucose solution with a concentration of 0.4 mol / L, stirring continuously;

[0152] S23 1.6 g of polyvinyl pyrrolidone was added to the glucose solution as an adjuvant;

[0153] S24 freeze-drying the glucose solution for 6 h to remove water therein;

[0154] S25 The freeze-dried glucose sample was placed in a carbonization furnace and carbonized at 700 °C for 2 h under an inert atmosphere;

[0155] After the carbonization in S26, the sample was allowed to cool naturally to room temperature, and was acid-washed with 70 mL of 1 mol / L hydrochloric acid, and then dried to obtain the sugar hard carbon material;

[0156] Step (3) Hot pressing and lamination

[0157] S31: taking 4 g of sugar hard carbon material, crushing it, and sieving it to obtain sugar hard carbon particles of 180 mesh;

[0158] S32: 1.6 g of graphene is added to the sugar hard carbon particles and mixed thoroughly;

[0159] S33: placing the sugar hard carbon mixed raw material after adding graphene and the B and N co-doped porous carbon material into a hot pressing mold at a mass ratio of 1:0.9, first pre-pressing at 30° C., 18 MPa, 18 min, and then completing the overall hot pressing composite at 1100° C., 45 MPa, 50 min;

[0160] Step (4) Hole plugging

[0161] Chitosan-based thermosensitive gel was used as a pore plugging agent and was fully applied to the hard carbon material after hot pressing (the mass ratio of chitosan-based thermosensitive gel to the hard carbon product after hot pressing was 1.1:1), and then a phase change occurred at 35°C and within an electric field strength of 90V / cm to complete the pore plugging treatment;

[0162] Step (5) Preparation of hard carbon composite material

[0163] The product after the pore plugging treatment was pyrolyzed for 2.5 h in an inert atmosphere at 1300°C with a heating rate of 3°C / min to obtain a hard carbon composite material.

[0164] Example 4

[0165] Step (1) Preparation of B and N co-doped porous carbon

[0166] S11 Take 7g of o-phenanthroline, 24g of K2B4O7, and 7g of (CH3COO)2Zn and grind them evenly in a mortar (weigh and grind under vacuum), and transfer them to a tube furnace;

[0167] S12 was introduced with nitrogen, heated to 120°C at a heating rate of 0.8°C / min, and kept reacting at this temperature for 0.5h;

[0168] S13 was then heated to 350°C at a heating rate of 1.6°C / min and kept at this temperature for 0.8h;

[0169] S14 was finally heated to 760°C at a heating rate of 5°C / min, kept at this temperature for 2 h, and then gradually cooled to room temperature under a nitrogen environment;

[0170] S15 Take out the high temperature reaction product, add 2 mol / L HCl solution, seal and stir for 60 min, then wash and filter with distilled water for 6 times until the pH value of the filtrate is close to neutral;

[0171] S16 The washed product was dried in an oven at 120°C for 14 h to obtain B and N co-doped porous carbon;

[0172] Step (2) Preparation of sugar hard carbon material

[0173] S21 takes glucose particles and sieves them to obtain 200-mesh glucose particles;

[0174] S22 Dissolve 11 g of glucose powder in an appropriate amount of deionized water to form a glucose solution with a concentration of 0.2 mol / L, stirring continuously;

[0175] S23 Add 2 g of polyvinyl pyrrolidone as an adjuvant to the glucose solution;

[0176] S24 freeze-drying the glucose solution for 8 h to remove water therein;

[0177] S25 The freeze-dried glucose sample was placed in a carbonization furnace and carbonized at 750 °C for 1.5 h under an inert atmosphere;

[0178] After the carbonization in S26, the sample was allowed to cool naturally to room temperature, and was acid-washed with 80 mL of 1 mol / L hydrochloric acid, and then dried to obtain the sugar hard carbon material;

[0179] Step (3) Hot pressing and lamination

[0180] S31: taking 5 g of sugar hard carbon material, crushing it, and sieving it to obtain 200-mesh sugar hard carbon particles;

[0181] S32 Add 2 g of graphene to the sugar hard carbon particles and mix them thoroughly;

[0182] S33: placing the sugar hard carbon mixed raw material after adding graphene and the B and N co-doped porous carbon material into a hot pressing mold at a mass ratio of 1:1.05, first pre-pressing at 35° C., 20 MPa, 20 min, and then completing the overall hot pressing compounding at 1200° C., 50 MPa, 60 min;

[0183] Step (4) Hole plugging

[0184] Chitosan-based thermosensitive gel was used as a pore plugging agent and was fully applied to the hard carbon material after hot pressing (the mass ratio of chitosan-based thermosensitive gel to the hard carbon product after hot pressing was 1.3:1), and then a phase change occurred at 40°C and within an electric field strength of 110V / cm to complete the pore plugging treatment;

[0185] Step (5) Preparation of hard carbon composite material

[0186] The product after the pore plugging treatment was pyrolyzed for 3.5 h in an inert atmosphere at 1100°C with a heating rate of 5°C / min to obtain a hard carbon composite material.

[0187] Embodiment 5:

[0188] The preparation of the hard carbon composite material is different from that of Example 1 in that PEG-based gel is used instead of chitosan-based thermosensitive gel; wherein, the specific operation of the pore plugging treatment is as follows: 6 g of PEG-based gel is taken as a pore plugging agent, and it is fully applied on the hard carbon material after hot pressing and compounding, and then a phase change occurs at 25°C to complete the pore plugging treatment.

[0189] Comparative Example 1

[0190] Step (1) Preparation of B and N co-doped porous carbon

[0191] S11 Take 4g of o-phenanthroline, 18g of K2B4O7, and 4g of (CH3COO)2Zn and grind them evenly in a mortar (weigh and grind under vacuum), and transfer them to a tube furnace;

[0192] S12 was heated to 700 °C at a heating rate of 2 °C / min, kept at this temperature for 1 h, and then gradually cooled to room temperature in a nitrogen environment;

[0193] S13 Take out the high temperature reaction product, add 1 mol / L HCl solution, seal and stir for 30 min, then wash and filter with distilled water for 3 times until the pH value of the filtrate is close to neutral;

[0194] S14 drying the washed product in an oven at 100°C for 8 h to obtain B and N co-doped porous carbon;

[0195] Step (2) Preparation of sugar hard carbon material

[0196] S21 takes glucose particles and sieves them to obtain glucose particles of 160 mesh;

[0197] S22 Dissolve 8 g of glucose powder in an appropriate amount of deionized water to form a glucose solution with a concentration of 0.5 mol / L, stirring continuously;

[0198] S23 freeze-drying the glucose solution for 2 h to remove water therein;

[0199] S24: placing the freeze-dried glucose sample in a carbonization furnace and carbonizing it at 600°C for 3 h under an inert atmosphere;

[0200] After the S25 carbonization, the sample was allowed to cool naturally to room temperature, and was acid-washed with 50 mL of 1 mol / L hydrochloric acid, and then dried to obtain the sugar hard carbon material;

[0201] Step (3) Hot pressing and lamination

[0202] S31: taking 2 g of sugar hard carbon material, crushing it, and sieving it to obtain 160 mesh sugar hard carbon particles;

[0203] S32: placing sugar hard carbon particles and B and N co-doped porous carbon materials in a mass ratio of 1:1 into a hot pressing mold, first pre-pressing at 20°C, 10MPa, 10min, and then completing the overall hot pressing composite at 800°C, 30MPa, 30min;

[0204] Step (4) Hole plugging

[0205] Take PEG-based gel as a pore plugging agent and fully apply it on the hard carbon material after hot pressing and compounding (the mass ratio of gel to the hard carbon product after hot pressing and compounding is 0.85:1), and then phase change occurs at 25°C to complete the pore plugging treatment;

[0206] Step (5) Preparation of hard carbon composite material

[0207] The product after the pore plugging treatment was pyrolyzed for 3 h in a nitrogen atmosphere at 1200°C with a heating rate of 3°C / min to obtain a hard carbon composite material.

[0208] Comparative Example 2

[0209] Step (1) Preparation of B and N co-doped porous carbon

[0210] S11 Take 7g of o-phenanthroline, 24g of K2B4O7, and 7g of (CH3COO)2Zn and grind them evenly in a mortar (weigh and grind under vacuum), and transfer them to a tube furnace;

[0211] S12 was heated to 760°C at a heating rate of 5°C / min, kept at this temperature for 2 h, and then gradually cooled to room temperature under a nitrogen atmosphere;

[0212] S13 Take out the high temperature reaction product, add 2 mol / L HCl solution, seal and stir for 60 min, then wash and filter with distilled water for 6 times until the pH value of the filtrate is close to neutral;

[0213] S14 drying the washed product in an oven at 120°C for 14 h to obtain B and N co-doped porous carbon;

[0214] Step (2) Preparation of sugar hard carbon material

[0215] S21 takes glucose particles and sieves them to obtain 200-mesh glucose particles;

[0216] S22 Dissolve 11 g of glucose powder in an appropriate amount of deionized water to form a glucose solution with a concentration of 0.2 mol / L, stirring continuously;

[0217] S23 freeze-drying the glucose solution for 8 hours to remove water therein;

[0218] S24 The freeze-dried glucose sample was placed in a carbonization furnace and carbonized at 750°C for 1.5 h under an inert atmosphere;

[0219] After the carbonization in S25, the sample was allowed to cool naturally to room temperature, and was acid-washed with 80 mL of 1 mol / L hydrochloric acid, and then dried to obtain the sugar hard carbon material;

[0220] Step (3) Hot pressing and lamination

[0221] S31: taking 5 g of sugar hard carbon material, crushing it, and sieving it to obtain 200-mesh sugar hard carbon particles;

[0222] S32 puts the sugar hard carbon particles and the B and N co-doped porous carbon material into a hot pressing mold at a mass ratio of 1:1.05, first pre-presses at 35°C, 20MPa, and 20min, and then completes the overall hot pressing composite at 1200°C, 50MPa, and 60min;

[0223] Step (4) Hole plugging

[0224] A PEG-based gel was used as a pore plugging agent and was fully applied to the hard carbon material after hot pressing (the mass ratio of the gel to the hard carbon product after hot pressing was 1.3:1), and then a phase change occurred at 40°C to complete the pore plugging treatment, and finally a hard carbon composite material was prepared;

[0225] Step (5) Preparation of hard carbon composite material

[0226] The product after the pore plugging treatment was pyrolyzed for 3.5 h in an inert atmosphere at 1100°C with a heating rate of 5°C / min to obtain a hard carbon composite material.

[0227] Comparative Example 3:

[0228] The preparation of the hard carbon composite material is different from that of Example 1 in that: resorcinol formaldehyde resin is used instead of chitosan-based thermosensitive gel; its pore plugging treatment is specifically as follows: resorcinol formaldehyde resin is dissolved in 75% mass concentration ethanol aqueous solution at a concentration of 5 mg / mL, and then the product after hot pressing composite is added (with a mass ratio of 1:2 to resorcinol formaldehyde resin), and stirred with a magnetic stirrer for 10 minutes; then the ethanol and deionized water in the solution are removed by spray drying.

[0229] Test example:

[0230] Preparation of a negative electrode sheet. A hard carbon composite material and PTFE (mass ratio of 85%:15%) are mixed into a slurry. Subsequently, the slurry is repeatedly rolled into a thin sheet using a glass rod, and then the thin sheet is made into a circular carbon sheet with a diameter of 12 mm using a puncher. Finally, the carbon sheet is placed in a vacuum drying oven at 110°C and dried for 2 hours, and then taken out to obtain a negative electrode sheet.

[0231] An electrochemical device. The prepared negative electrode sheet is used as the working electrode, the metal lithium sheet is used as the counter electrode, a polyethylene and polypropylene composite diaphragm is used, and a LIB315 commercial lithium-ion battery electrolyte is used. Oxygen and water are removed in a glove box before assembly. The assembly sequence is as follows: lay the positive electrode shell open upward on a platform; clamp the nickel foam as a current collector and place it in the positive electrode shell; then put the graphite electrode sheet in, and use a rubber-tipped dropper to absorb a small amount of electrolyte and apply it on the electrode sheet; then place the diaphragm soaked in the electrolyte on the electrode sheet, and add a small amount of electrolyte again; then place the lithium sheet, the nickel foam and the negative electrode shell in turn and compact them, and finally package them on a hydraulic sealing machine to obtain an electrochemical device containing the lithium-ion battery.

[0232] The hard carbon composite materials obtained in Examples 1-5 and the products of Comparative Examples 1-3, i.e., the lithium ion batteries thereof, were tested. The specific testing methods are as follows:

[0233] Rate performance test

[0234] Use LT1000 battery charge and discharge test instrument, set the charge and discharge voltage to 0-2.5 V at room temperature, and perform constant current charge and discharge test at a rate of 1C.

[0235] Specific surface area test

[0236] The Brunauer-Emmett-Teller test method was used to test the hard carbon composite materials of the embodiments and comparative examples. The materials were first degassed at a certain temperature and then nitrogen adsorbed. The nitrogen adsorption amount under different pressures was measured. The experimental data was fit using the BET equation to calculate the specific surface area of ​​the material.

[0237] The particle size was measured by laser method using Malvern laser particle size analyzer MS2000.

[0238] The tap density test was carried out using a tap density tester FZS4-4B by tapping method.

[0239] Closed pore volume test The closed pore volume was determined by gas adsorption method.

[0240] Table 1 Rate performance test results

[0241] Example Specific capacity (mAh / g) Specific capacity retention rate after 300 cycles (%) 1 415.8 96.7 2 424.3 97.3 3 438.6 96.5 4 449.5 97.8 5 410.4 95.4 Comparative Example 1 289.7 88.3 Comparative Example 2 299.5 87.9 Comparative Example 3 403.2 93.5

[0242] As can be seen from Table 1, the rate performance of the hard carbon composite materials prepared in Examples 1-5 is better than that of the hard carbon composite materials prepared in Comparative Examples 1 and 2. This is because in the examples, a distributed temperature rise multi-stage reaction mode is implemented in the preparation process of the B and N co-doped porous carbon materials to generate the reaction, so that the prepared B and N co-doped porous carbon materials have better performance. In addition, graphene is added in the preparation process. Graphene has excellent electrical conductivity. Adding it to the hard carbon composite material can significantly improve the electrical conductivity of the material, thereby improving the rate performance and cycle stability of the battery.

[0243] When Example 1 and Example 5 are compared with Comparative Example 3, the specific capacity and cycle capacity retention rate of the hard carbon composite material are significantly improved, indicating that the use of thermosensitive gel as a pore plugging agent for pore plugging treatment can effectively improve the rate performance and cycle stability of the hard carbon composite material compared with traditional pore plugging agents.

[0244] Table 2 Structural parameter test results

[0245] Example <![CDATA[Specific surface area of the hot-pressed composite product (m 2 / g)]]> <![CDATA[Specific surface area of the product (m 2 / g)]]> D50 (μm) <![CDATA[Tap density (g / cm 3 )]]> <![CDATA[Closed pore volume (cm 3 / g)]]> 1 189.6 8.5 5.8 0.67 0.146 2 193.7 7.6 6.3 0.75 0.173 3 197.5 9.9 7.1 0.58 0.151 4 203.4 11.5 7.5 0.51 0.130 5 190.6 12.7 6.0 0.49 0.201 Comparative Example 1 145.3 5.0 14.4 0.82 0.094 Comparative Example 2 147.9 4.3 13.6 1.03 0.253 Comparative Example 3 184.8 4.6 10.2 0.77 0.082

[0246] As can be seen from Table 2, the specific surface areas of the hard carbon composite materials prepared in Examples 1-5 are higher than the specific surface areas of the hard carbon composite materials prepared in Comparative Examples 1 and 2. In the preparation of the hard carbon material, polyvinyl pyrrolidone is added as an auxiliary agent in the embodiment, which can act as a template or catalyst in the subsequent carbonization process, and is helpful to form a hard carbon material with a specific structure or performance, and the glucose solution is frozen. This freeze-drying can maintain the original structure of the solution and avoid cracks or deformation during the drying process. In addition, the glucose molecule contains multiple hydroxyl groups, which can form a rich cross-linked structure during the carbonization process, thereby preparing graphene with a large specific surface area. After adding hot pressing to the hard carbon composite material, the specific surface area of ​​the hot pressing composite product can be increased, providing more active sites for the electrochemical reaction, thereby improving the capacity and energy density of the battery. In the final pore plugging process, chitosan-based thermosensitive gel with good temperature-controlled phase change performance is also added as a pore plugging agent in the embodiment, which has good adhesion and filling properties, can fit closely to the pores on the porous carbon surface, and effectively fill the pores, thereby improving the performance of the material.

[0247] The hard carbon composite material prepared in Example 1-5 has a particle size D50 of 5-8 μm and a specific surface area of ​​7-13 m 2 / g, tap density is 0.4~0.8g / cm 3 , closed pore volume is 0.10~0.25cm 3 / g. Comparing Example 1 and Example 5 with Comparative Example 3, the specific surface areas of the hard carbon composite materials are significantly increased, indicating that the use of the thermosensitive gel as a pore plugging agent for pore plugging treatment can effectively improve the pore structure of the product, enrich the micropore structure, effectively regulate the pore size structure, increase the specific surface area of ​​the material, and be more conducive to ion diffusion and electron transmission efficiency, thereby effectively improving the electrochemical properties of the hard carbon composite material.

[0248] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art can make non-creative modifications to the present embodiment as needed, but they are protected by patent law as long as they are within the scope of the claims of the present invention.

Claims

1. A process for preparing a hard carbon composite material, characterized in that include: After the sugar hard carbon material is crushed, a conductive agent, B and N co-doped porous carbon are added for hot pressing and compounding, followed by pore blocking and high temperature carbonization to obtain a hard carbon composite material; The pore plugging treatment process includes applying a pore plugging agent to the hard carbon material after hot pressing and compounding, causing a phase change at 25-40° C. and an electric field of 50-110 V / cm to complete the pore plugging treatment; The pore plugging agent used in the pore plugging treatment process includes gel, and the gel includes a thermosensitive gel; the thermosensitive gel includes at least one of chitosan-based thermosensitive gel, poly N-isopropylacrylamide gel, or hyaluronic acid-based thermosensitive gel; the sugar hard carbon material includes at least one of glucose-based hard carbon, sucrose-based hard carbon, or starch-based hard carbon; The mass ratio of the sugar hard carbon material to the conductive agent is 1:0.2-1; the mass ratio of the sugar hard carbon material containing the conductive agent to the B and N co-doped porous carbon material is 1:0.8-1.

5.

2. The process for preparing the hard carbon composite material according to claim 1, characterized in that: Contains at least one of the following characteristics (1) to (6): (1) The conductive agent includes at least one of graphene, conductive graphite, conductive carbon black, conductive carbon fiber, and carbon nanotubes; (2) The specific surface area of ​​the product obtained by hot pressing is 185~210m 2 / g; (3) The particle size D50 of the hard carbon composite material is 5-8 μm; (4) The specific surface area of ​​the hard carbon composite material is 7 to 13 m 2 / g; (5) The tap density of the hard carbon composite material is 0.4-0.8 g / cm 3 ; (6) The closed pore volume of the hard carbon composite material is 0.10~0.25cm 3 / g.

3. The process for preparing the hard carbon composite material according to claim 1, characterized in that: The method for preparing the sugar hard carbon material comprises: The sugar particles are sieved and dissolved in an appropriate amount of deionized water to form a sugar solution; Adding adjuvants to the sugar solution followed by freeze drying to remove water; The freeze-dried sugar sample is carbonized, acid-washed and dried under an inert atmosphere to obtain a sugar hard carbon material.

4. The process for preparing the hard carbon composite material according to claim 1, characterized in that: The method for preparing the B and N co-doped porous carbon comprises: Take o-phenanthroline, K2B4O7, (CH3COO)2Zn and grind them evenly; Under inert atmosphere, high temperature treatment is carried out by step-by-step heating; The high temperature reaction product is taken, immersed and stirred in an acid solution, washed and filtered with distilled water, and dried to obtain B and N co-doped porous carbon.

5. The process for preparing the hard carbon composite material according to claim 1, characterized in that: The hot pressing composite process includes taking a sugar-based hard carbon material, adding a conductive agent and mixing, then adding B and N co-doped porous carbon material, and performing hot pressing composite after pre-pressing.

6. The process for preparing the hard carbon composite material according to claim 5, characterized in that: Contains at least one of the following characteristics (1) to (3): (1) The sugar hard carbon material has a particle size of 160-200 mesh after crushing and screening; (2) The pre-pressing temperature is 20-35°C, the pre-pressing pressure is 10-20 MPa, and the pre-pressing time is 10-20 min; (3) The hot pressing composite temperature is 800-1200°C, the hot pressing composite pressure is 30-50MPa, and the hot pressing composite time is 30-60min.

7. A hard carbon composite material, characterized in that: The hard carbon composite material is prepared by the preparation process according to any one of claims 1 to 6, characterized in that it comprises at least one of the following features (1) to (3): (1) The particle size of the hard carbon composite material is D50 = 5~8μm; (2) The specific surface area of ​​hard carbon composite materials is 7~13m 2 / g; (3) The tap density of hard carbon composite materials is 0.4~0.8g / cm 3 , closed pore volume is 0.10~0.25cm 3 / g.

8. A negative electrode sheet, characterized in that: The negative electrode sheet comprises the hard carbon composite material as claimed in claim 7.

Citation Information

Patent Citations

  • Spherical core-shell structure mixed graphite @ hard carbon composite material as well as preparation method and application thereof

    CN109616638A

  • Preparation method and application of nitrogen-doped porous carbon material with high specific surface area

    CN112850708A

  • Preparation of graded porous carbon and application of graded porous carbon in sodium ion battery

    CN114477128A

  • Hard carbon composite material for lithium ion battery and preparation method of hard carbon composite material

    CN115663157A

  • Preparation and application of three-dimensional porous hard carbon material