Preparation method and application of micro-arc oxidation film-HKUST-1-pGOLDHs composite film on magnesium alloy surface

By preparing HKUST-1-pGOLDHs composite films on magnesium alloy surfaces, the growth of HKUST-1 is guided by the reaction of graphene oxide and p-aminophenol and amide bonds, thereby sealing the pores of the micro-arc oxide film and solving the corrosion resistance and stability problems of the magnesium alloy micro-arc oxide film, thus improving its self-healing performance.

CN118127510BActive Publication Date: 2026-11-17ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410055791.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-15
Publication Date
2026-11-17
Estimated Expiration
2044-01-15

AI Technical Summary

Technical Problem

Existing magnesium alloy micro-arc oxidation films contain micropores and cracks, which cannot provide long-term corrosion protection in corrosive environments and have poor stability.

Method used

After preparing a micro-arc oxidation film on the magnesium alloy surface, an HKUST-1-pGOLDHs composite film was grown in situ. The carboxyl groups on the surface of graphene oxide reacted with p-aminophenol to dope and grow a pGO/LDHs film. The HKUST-1 was nucleated and grown on its surface through amide bonds, thereby achieving the sealing and self-repair of pores.

Benefits of technology

This method improves the density and self-healing properties of the micro-arc oxidation film on magnesium alloys, extends the invasion path of corrosive media, enhances the corrosion resistance of magnesium alloys, and is simple and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118127510B_ABST
    Figure CN118127510B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a micro-arc oxidation film-HKUST-1-pGOLDHs composite film on a magnesium alloy surface, comprising the following steps: A1) firstly, preparing a micro-arc oxidation film layer on the magnesium alloy surface; A2) in-situ growing an HKUST-1-pGO / LDHs film on the micro-arc oxidized magnesium alloy surface; A3) repeatedly cleaning the magnesium alloy film layer after the in-situ growth reaction in step A2) 2-5 times, and then drying it overnight. This invention also discloses the application of this micro-arc oxidation film-HKUST-1-pGOLDHs composite film on a magnesium alloy surface. This invention modifies GO with p-aminophenol to obtain a pGO composite loaded with an organic corrosion inhibitor. Then, a one-step hydrothermal method is used to achieve in-situ growth of pGO / LDHs composite nanosheets on the surface of a magnesium alloy micro-arc oxidation film. At the same time, the surface amide bonds are used to induce the in-situ growth of HKUST-1 to seal the pores on the surface of the pGO / LDHs film, thereby improving the compactness of the micro-arc oxidation film, extending the path of corrosive media intrusion, and repairing damaged areas of the film to compensate for film defects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal surface protection treatment technology, specifically relating to a method for preparing a magnesium alloy surface micro-arc oxide film-HKUST-1-pGOLDHs composite film that can effectively fill the pores of the magnesium alloy micro-arc oxide film layer, enhance the corrosion resistance of the magnesium alloy, and endow the film layer with self-healing properties under green and environmentally friendly conditions, as well as its application. Background Technology

[0002] Magnesium alloys are known as "green engineering materials of the 21st century" due to their low density (1.8 g / cm³). 3 Magnesium alloys (approximately) are characterized by high strength, large elastic modulus, good heat dissipation, good shock absorption, greater impact load capacity than aluminum alloys, good resistance to organic and alkaline corrosion, and good electrical and thermal conductivity and damping properties.

[0003] However, magnesium alloys possess high chemical and electrochemical activity and extremely low standard electrode potential, making them highly susceptible to corrosion and significantly limiting their widespread application. Currently, research on corrosion prevention for magnesium alloys mainly falls into two categories: the first focuses on improving the bulk corrosion resistance of magnesium alloys, such as reducing harmful impurities, increasing alloy purity, and employing rapid solidification methods; the second utilizes surface treatment technologies, such as the relatively mature anodic oxidation films and micro-arc oxidation films. Micro-arc oxidation technology, a surface treatment process that has received considerable attention in recent years, involves in-situ growth of ceramic layers on non-ferrous metals and is commonly used for aluminum alloys, magnesium alloys, titanium alloys, and other alloys suitable for anodic oxidation, such as zinc and nickel.

[0004] Among current surface treatment methods for magnesium alloys, micro-arc oxidation (MAO) technology is widely used due to its high hardness, good wear resistance, and corrosion resistance in the films prepared on magnesium alloy surfaces. The ceramic structure of the MAO film on magnesium alloys consists of a porous outer layer and an internal isolation layer. The porous outer layer exhibits typical structural characteristics of micropores and microcracks, which can become channels for the penetration of corrosive media. Once the MAO film is damaged during the intrusion of corrosive media, it will cause severe corrosion to the magnesium alloy substrate, and the area of ​​film detachment will gradually increase. Therefore, it is of great significance to effectively enhance the self-healing and corrosion resistance of the MAO film by employing post-treatment sealing processes and applying corrosion inhibitors. Summary of the Invention

[0005] This invention aims to at least partially solve one of the technical problems in related technologies. Therefore, the main objective of this invention is to provide a method for preparing a micro-arc oxidation film-HKUST-1-pGOLDHs composite film on magnesium alloy surfaces, aiming to overcome the shortcomings of existing magnesium alloy micro-arc oxidation films, such as micropores and cracks, inability to provide long-term corrosion protection in corrosive environments, and poor stability. This invention also provides applications of this magnesium alloy micro-arc oxidation film-HKUST-1-pGOLDHs composite film.

[0006] The objective of this invention is achieved through the following technical solution:

[0007] In a first aspect, a method for preparing a micro-arc oxidation film-HKUST-1-pGOLDHs composite film on a magnesium alloy surface includes the following steps:

[0008] A1) First, prepare a micro-arc oxide film on the surface of the magnesium alloy;

[0009] A2) In-situ growth of HKUST-1-pGO / LDHs film on the surface of magnesium alloy after micro-arc oxidation;

[0010] A3) After the in-situ growth reaction in step A2), the magnesium alloy film layer is repeatedly cleaned 2-5 times and dried overnight.

[0011] In some specific embodiments, step A2) specifically includes the following steps:

[0012] A21) Dissolve p-aminophenol powder in deionized water to obtain an alkaline solution of p-aminophenol; dilute the GO solution with the alkaline solution of p-aminophenol, adjust the pH value, heat under reflux, centrifuge, wash, and dry to obtain pGO powder.

[0013] A22) Dissolve pGO powder in sodium nitrate solution, adjust the pH value, and obtain pGO composite suspension;

[0014] A23) The magnesium alloy after micro-arc oxidation is placed in pGO composite suspension for in-situ growth to obtain a magnesium alloy with a micro-arc oxidation film-pGO / LDHs film layer on the surface.

[0015] A24) was then placed in a mixed solution of copper acetate and 1,3,5-benzenetricarboxylic acid for in-situ growth to obtain a magnesium alloy with a micro-arc oxide film-HKUST-1-pGO / LDHs composite film on the surface.

[0016] In some specific embodiments, the bath solution for preparing the micro-arc oxidation film layer in step A1) includes sodium aluminate and sodium hydroxide by mass-volume concentration, wherein the mass-volume concentration of sodium aluminate is 3-6 g / L and the mass-volume concentration of sodium hydroxide is 6-10 g / L.

[0017] In some specific embodiments, step A21) involves preparing pGO powder as follows: dissolving p-aminophenol in deionized water, diluting the GO solution to 0.05-0.2 mg / mL with an alkaline p-aminophenol solution, adjusting the pH of the mixed solution to 8-9 with a 0.5-1.5 mol / L NaOH solution, refluxing the mixed solution, and stirring in an oil bath at 80-90°C for 10-15 h; after the reaction is complete, centrifuging the pGO and washing it several times with deionized water and ethanol, and drying it overnight at 60-80°C to obtain pGO powder;

[0018] In some specific embodiments, in step A22), the preparation of the pGO composite suspension specifically involves: placing pGO powder in NaNO3 with a concentration of 0.5-1.5 mol / L to prepare a pGO concentration of 0.05-0.15 mg / mL suspension and sonicating for 1 hour; adjusting the pH of the pGO composite solution to 10-11 with 2-4 mol / L NaOH to obtain the pGO composite suspension.

[0019] In some specific embodiments, the concentration of the alkaline solution of p-aminophenol is 20-40 mg / mL.

[0020] In some specific embodiments, the copper acetate has a mass concentration of 30-40 mg / mL, and the 1,3,5-benzenetricarboxylic acid has a mass concentration of 35-50 mg / mL.

[0021] In some specific embodiments, in step A23), the process conditions for in-situ growth are: a reaction temperature of 418K and a reaction time of 10-15h; in step A24), the process conditions for in-situ growth are: a growth environment of room temperature and a reaction time of 40-60h.

[0022] In some specific embodiments, in step A3), the cleaning is performed using ethanol and deionized water under ultrasonic conditions; the drying conditions are overnight in a forced-air drying oven at 40-80°C.

[0023] Secondly, the application of the aforementioned method for preparing a micro-arc oxidation film-HKUST-1-pGOLDHs composite film on the surface of magnesium alloys in the surface treatment of magnesium alloys.

[0024] The product obtained by the aforementioned method for preparing a micro-arc oxidation film-HKUST-1-pGOLDHs composite film on the surface of magnesium alloy has applications in aerospace, automotive, and electronic communications fields.

[0025] Compared with the prior art, the present invention has at least the following advantages:

[0026] 1) In the preparation method provided by this invention, the graphene oxide (GO) surface used has abundant oxygen-containing functional groups, as well as high specific surface area and mechanical properties, making it a good carrier for loading organic corrosion inhibitors. The carboxyl groups on the graphene oxide (GO) surface can undergo an amination reaction with p-aminophenol, achieving effective fixation of p-aminophenol. After p-aminophenol doping, GO can be used in a one-step hydrothermal method to achieve the doping growth of pGO / LDHs on the surface of magnesium alloy micro-arc oxidation film. Simultaneously, the presence of amide bonds in the pGO / LDHs film can guide the nucleation and growth of the metal framework organic polymer HKUST-1 on its surface, generating an HKUST-1-pGO / LDHs composite film on the magnesium alloy micro-arc oxidation surface. This effectively seals the pores on the pGO / LDHs composite film surface, endowing the film with self-healing properties and enhancing the corrosion resistance of the magnesium alloy.

[0027] 2) The method for preparing the magnesium alloy micro-arc oxidation film-HKUST-1-pGOLDHs composite film provided by this invention involves modifying GO with p-aminophenol to obtain a pGO composite loaded with an organic corrosion inhibitor. Then, a one-step hydrothermal method is used to achieve in-situ growth of pGO / LDHs composite nanosheets on the surface of the magnesium alloy micro-arc oxidation film. Simultaneously, the in-situ growth of HKUST-1 is induced by surface amide bonds, sealing the pores on the pGO / LDHs film surface, improving the density of the micro-arc oxidation film, extending the path of corrosive media intrusion, and repairing damaged areas of the film to compensate for defects. Therefore, this preparation method fundamentally achieves the surface protection and self-healing properties of magnesium alloys. Furthermore, the process is simple, convenient, and environmentally friendly, making it a safe and green preparation process for enhancing the corrosion resistance of magnesium alloy micro-arc oxidation films.

[0028] 3) The magnesium alloy surface micro-arc oxidation film-HKUST-1-pGOLDHs composite film obtained by the present invention can be widely used in aviation, automotive, electronic communication and other fields. Attached Figure Description

[0029] To more clearly illustrate the specific embodiments of the present invention, the accompanying drawings used in the description of the specific embodiments or the prior art will be briefly introduced below.

[0030] Figure 1These are scanning electron microscope images of the micro-arc oxidation film layer on the surface of the magnesium alloy obtained in Example 1 after micro-arc oxidation;

[0031] Figure 2 These are scanning electron microscope images of the LDHs film layer on the surface of the magnesium alloy micro-arc oxidation film obtained in Example 2;

[0032] Figure 3 This is the XRD pattern of the LDHs film layer on the surface of the magnesium alloy micro-arc oxidation film obtained in Example 2;

[0033] Figure 4 This is the Bode pattern of the LDHs film layer on the surface of the micro-arc oxidation film obtained in Example 2;

[0034] Figure 5 This is the Phase pattern of the LDHs film layer on the surface of the micro-arc oxidation film obtained in Example 2;

[0035] Figure 6 These are scanning electron microscope images of the GO / LDHs film layer on the surface of the magnesium alloy micro-arc oxidation film obtained in Example 3;

[0036] Figure 7 These are XPS spectra of the GO / LDHs film on the surface of the magnesium alloy micro-arc oxidation film obtained in Example 3 and the pGO / LDHs film on the surface of the magnesium alloy micro-arc oxidation film obtained in Example 4.

[0037] Figure 8 These are the Bode spectra of the micro-arc oxidation film, LDHs film, and GO / LDHs composite film obtained in Example 3;

[0038] Figure 9 These are the phase patterns of the micro-arc oxidation film, LDHs film, and GO / LDHs composite film obtained in Example 3;

[0039] Figure 10 This is a scanning electron microscope image of the pGO / LDHs composite film layer on the surface of the magnesium alloy micro-arc oxidation film obtained in Example 4;

[0040] Figure 11 These are the Tafel polarization curves of the micro-arc oxidation film, LDHs film, GO / LDHs film, and pGO / LDHs film obtained by an electrochemical workstation in Example 4.

[0041] Figure 12 This is a scanning electron microscope image of the magnesium alloy surface micro-arc oxidation film-HKUST-1-pGO / LDHs composite film obtained in Example 5;

[0042] Figure 13The XRD pattern of the HKUST-1-pGO / LDHs film obtained in Example 5;

[0043] Figure 14 The impedance spectra of the micro-arc oxidation film, LDHs film, GO / LDHs film, pGO / LDHs film, and HKUST-1-pGO / LDHs film, measured by an electrochemical workstation in Example 5, are shown in the Bode spectrum (left) and Phase spectrum (right).

[0044] Figure 15 The impedance spectra of the micro-arc oxidation film, LDHs film, GO / LDHs film, pGO / LDHs film, and HKUST-1-pGO / LDHs film, measured by an electrochemical workstation in Example 5, are shown in the Bode spectrum (left) and Phase spectrum (right). Detailed Implementation

[0045] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. The following embodiments are merely descriptive and not limiting, and should not be construed as limiting the scope of protection of the present invention.

[0046] When a quantity, concentration, or other value or parameter is described as a range, preferred range, or preferred upper and lower limits, it should be understood that it is equivalent to specifically disclosing any range by combining any pair of upper or preferred values ​​with any lower or preferred values, regardless of whether the range is specifically disclosed. Unless otherwise stated, the numerical range values ​​listed herein include the endpoints of the range and all integers and fractions within that range.

[0047] Unless otherwise stated, all percentages, parts, ratios, etc. in this document are by weight.

[0048] The materials, methods, and embodiments described herein are exemplary and should not be construed as limiting unless otherwise stated.

[0049] Experimental methods not specified in the examples are generally performed under standard conditions or as recommended by the manufacturer.

[0050] Example 1

[0051] A method for preparing a MAO film on a magnesium alloy surface, comprising the following steps:

[0052] 1) Micro-arc oxidation

[0053] Micro-arc oxidation bath solution: Prepare the bath solution according to 7.14 g / L sodium hydroxide and 4 g / L sodium aluminate;

[0054] Micro-arc oxidation procedure: A square pulsed AC power supply is used as the micro-arc oxidation power source. AZ31 magnesium alloy (taking AZ31 magnesium alloy as an example) is used as the working electrode, and a stainless steel plate is used as the cathode. A condensation circulation system is used to maintain the temperature of the micro-arc oxidation bath at 25±5℃. The working time is 5 minutes, the pulse width is 100μs, and the frequency is 500Hz. After the operation, the magnesium alloy sample is removed, rinsed repeatedly with deionized water and alcohol, and then dried with a hair dryer. Figure 1 These are scanning electron microscope images of the surface of a magnesium alloy after micro-arc oxidation. Figure 1 As can be seen, the surface morphology of the magnesium alloy AZ31 micro-arc oxide film layer obtained in Example 1 exhibits many holes and protrusions of varying sizes, forming a porous and rough surface morphology. This micro-arc oxide film layer (MAO layer) has strong adhesion and high stability.

[0055] Example 2

[0056] A method for preparing an LDHs film layer on the surface of a magnesium alloy micro-arc oxidation film, comprising the following steps:

[0057] 1) Micro-arc oxidation

[0058] Step 1) of the micro-arc oxidation is the same as in Example 1;

[0059] 2) In-situ growth of LDHs membranes

[0060] A 1 mol / L NaNO3 solution was prepared, and the pH was adjusted to 10.8 using a 3.0 mol / L NaOH solution. The magnesium alloy with a MAO film (magnesium alloy AZ31 with a micro-arc oxidation film obtained by the preparation method in Example 1) and the NaNO3 solution were placed together in a reaction vessel, and the reaction vessel was sealed tightly. Finally, it was placed in a forced-air drying oven for in-situ growth at a reaction temperature of 418 K and a constant temperature time of 12 h. Figure 2 These are scanning electron microscope images of the magnesium alloy LDHs film obtained in Example 2; from Figure 2 It can be seen that the LDHs film layer on the surface of the magnesium alloy AZ31 micro-arc oxidation film obtained in Example 2 exhibits a thin sheet appearance that grows perpendicular to the substrate. This is because metal ions and hydrated oxide ions are rapidly accumulated along a certain direction during crystal growth.

[0061] 3) Cleaning and drying

[0062] The magnesium alloy prepared in step 2) is first rinsed with deionized water, then placed in anhydrous ethanol and ultrasonicated for 10 minutes in an ultrasonic cleaner to remove surface residues. It is then rinsed with deionized water, dried with a hair dryer, and stored in a dry environment for further testing of morphology, structure, corrosion resistance, etc.

[0063] in Figure 3 The XRD pattern of the magnesium alloy micro-arc oxidation film LDHs film obtained in Example 2 shows that the film sample has typical characteristic peaks of 003 and 006 at positions of 11.5° and 23.2°, respectively, indicating that an LDHs composite sealing film was successfully formed on the surface of the magnesium alloy micro-arc oxidation film. Figure 4 and Figure 5 The electrochemical impedance spectroscopy (EIS) obtained by an electrochemical workstation after immersing the micro-arc oxidation film and LDH film in 3.5 wt% NaCl solution for 30 minutes in Example 2 mainly includes Bode and Phase spectra. Typically, the low-frequency impedance value (|Z|) is... 0.01Hz The phase angle (Z) can reflect the corrosion resistance of the coating. Furthermore, a higher impedance value indicates better corrosion protection. Simultaneously, when the coating is defect-free, the phase angle value is consistently the highest (approximately -90°) and remains within a wide frequency range. The |Z| of LDH films... 0.01Hz Reached 10 5 Ωcm 2 Furthermore, the phase angle is greater than that of the magnesium alloy MAO film, indicating that after the magnesium alloy micro-arc oxidation film is modified with LDHs, the pores on the surface of the micro-arc oxidation film are effectively sealed, thus improving the corrosion resistance of the film.

[0064] Example 3

[0065] A method for preparing a GO / LDHs film on the surface of a magnesium alloy micro-arc oxidation film, comprising the following steps:

[0066] 1) Micro-arc oxidation

[0067] Step 1) of the micro-arc oxidation is the same as in Example 1;

[0068] 2) In-situ growth of GO / LDHs membranes

[0069] First, prepare the GO solution: Dissolve 5g of phosphorus pentoxide and 5g of potassium persulfate in 25mL of concentrated sulfuric acid at 80℃; add 6g of graphite powder, stir for 4.5h, cool to room temperature, dilute the solution with 1L of deionized water and let stand overnight, filter, wash and dry with 0.5L of water, add it to 230mL of concentrated sulfuric acid solution, and add 30g of KMnO4; keep the temperature of the solution below 5℃ throughout the reaction; then cool in an ice bath and dilute with dihydrate; stir for 4h, add 1.4L of deionized water and 25mL of H2O2 solution (30%) again; filter, adjust the pH of the suspension to 6 with 2.5L of 10% hydrochloric acid; obtain a GO solution with a concentration of 5mg / mL.

[0070] A 1 mol / L NaNO3 solution was prepared, and the GO solution was diluted to 0.1 mg / mL using the NaNO3 solution. Then, the pH value was adjusted to 10.8 using a 3.0 mol / L NaOH solution. The magnesium alloy with a MAO film layer (magnesium alloy AZ31 with a micro-arc oxidation film layer obtained by the preparation method in Example 1) and the NaNO3 solution were placed together in a reaction vessel, and the reaction vessel was sealed tightly. Finally, it was placed in a forced-air drying oven for in-situ growth. The reaction temperature was 418 K, and the constant temperature time was set to 12 h. Figure 6 These are scanning electron microscope images of the magnesium alloy GO / LDHs sealing film obtained in Example 3;

[0071] In Example 3, the magnesium alloy micro-oxide film was subjected to a hydrothermal reaction in a GO solution. The resulting GO / LDHs composite film nanosheets showed a tendency to grow in different directions. Furthermore, due to the amorphous nanosheet structure of GO, the GO / LDHs composite nanosheets exhibited a wavy and edge-curled appearance, which contrasted with the surface morphology of Example 2 and changed the traditional state of LDHs growing perpendicular to the substrate.

[0072] 3) Cleaning and drying

[0073] The magnesium alloy prepared in step 2) is first rinsed with deionized water, then placed in anhydrous ethanol and ultrasonicated for 10 minutes in an ultrasonic cleaner to remove surface residues. It is then rinsed with deionized water, dried with a hair dryer, and stored in a dry environment for further testing of morphology, structure, corrosion resistance, etc.

[0074] Figure 7 a is the XPS spectrum of the GO / LDHs film obtained in Example 3. It can be seen that a new CO peak was observed at 286.7 eV in the film sample. This peak is due to GO doping, indicating that GO has been successfully embedded in the LDHs phase.

[0075] Figure 8 and Figure 9 Examples 3 show the Bode and Phase spectra of the micro-arc oxidation film, LDHs film, and GO / LDHs composite film after immersing them in a 3.5 wt% NaCl solution for 30 minutes; the impedance spectrum shows high frequencies (10... 2 -10 5 The value of (Hz) reflects the characteristics of the outer layer of the film, while the value of the mid-frequency (10 Hz) reflects the characteristics of the outer layer of the film. 0 -10 2 The Hz value reflects the characteristics of the inner layer of the film, while the value in the low-frequency range (less than 10 Hz) reflects the characteristics of the inner layer of the film. 0 The Hz (high frequency) reflects the interface between the substrate and the coating. The spectrum shows that in the high-frequency range, the impedance modulus of the GO / LDHs composite film is greater than that of the LDHs film sample, increasing to 10.5.5 Ωcm 2 Meanwhile, the phase angle is increased to 60°. This indicates that the addition of GO changes the growth state of traditional LDH nanosheets, resulting in multi-directional growth, which prolongs the invasion path of corrosive media and enhances the corrosion resistance of the film.

[0076] Example 4

[0077] A method for preparing a pGO / LDHs micro-arc oxidation film on the surface of a magnesium alloy, comprising the following steps:

[0078] 1) Micro-arc oxidation

[0079] Step 1) of the micro-arc oxidation is the same as in Example 1;

[0080] 2) In-situ growth of pGO / LDHs membranes

[0081] First, pGO powder was prepared: 2g of p-aminophenol was dissolved in 600mL of deionized water, and the GO solution (the preparation method of the GO solution is the same as in Example 3) was diluted to 0.1mg / mL with an alkaline p-aminophenol solution. The pH of the mixed solution was adjusted to 8.5 with a 1mol / L NaOH solution. The mixed solution was refluxed and stirred in an oil bath at 90℃ for 12h. After the reaction, the pGO was centrifuged and washed several times with deionized water and ethanol. It was then dried overnight at 70℃ to obtain pGO powder.

[0082] pGO powder was placed in 1 mol / L NaNO3 to prepare a pGO suspension with a concentration of 0.1 mg / mL and sonicated for 1 h. The pH of the pGO composite solution was adjusted to 10.8 with 3.0 mol / L NaOH to obtain a pGO composite suspension. The pGO suspension was then poured into a reaction vessel and the reaction vessel was tightly sealed. Finally, it was placed in a forced-air drying oven for in-situ growth at a reaction temperature of 418 K and a constant temperature time of 12 h. Figure 10 This is a scanning electron microscope image of the pGO / LDHs sealing film layer coated with micro-arc oxide film obtained in this embodiment.

[0083] Compared to the looser nanosheets of the GO / LDHs coating, the pGL / LDHs film obtained in Example 3 exhibits a denser sheet-like structure. The addition of the pGO composite also alters the straight-leaf morphology of the LDHs, increasing the coating density and providing a significant potential for extending the penetration path of corrosive media.

[0084] 3) Cleaning and drying

[0085] The magnesium alloy prepared in step 2 was first rinsed with deionized water, then placed in anhydrous ethanol and ultrasonicated for 10 minutes in an ultrasonic cleaner to remove surface residues. It was then rinsed with deionized water, dried with a hair dryer, and stored in a dry environment for further testing of morphology, structure, corrosion resistance, etc.

[0086] Figure 7 b is the XPS spectrum of the magnesium alloy micro-arc oxidation film pGO / LDHs obtained in Example 4. Compared with the GO / LDHs film, it can be seen that the film sample has new binding energy peaks at 287.9 ​​eV and 285.8 eV, which can be attributed to amide bonds (C=O-NH) and carbon-nitrogen bonds (CN), fully demonstrating that p-aminophenol and GO underwent an amide reaction. Figure 11 These are the Tafel polarization curves of the MAO film, LDHs film, GO / LDHs film, and pGO / LDHs film after immersion in 3.5 wt% NaCl solution for 30 min, measured by an electrochemical workstation in Example 4; generally, the corrosion current density (i corr The lower the value, the better the corrosion resistance (the lower the corrosion dynamic rate); the corrosion current density of the pGO / LDHs film sample after condition treatment in Example 4 was 3.99 × 10⁻⁶. -9 A cm -2 The corrosion current density (i) of the treated sample corr The minimum value is relative to the i value of the MAO film sample. corr This represents a reduction of three orders of magnitude. The above results can be explained by the fact that the pGO / LDHs nanosheets seal the pores and gaps in the micro-arc oxidation film, forming a relatively dense surface film layer, thus effectively sealing it off.

[0087] Example 5

[0088] A method for preparing an HKUST-1-pGO / LDHs self-healing film layer on the surface of a magnesium alloy micro-arc oxidation film, the specific steps of which are as follows:

[0089] 1. Micro-arc oxidation

[0090] Step 1) of the micro-arc oxidation is the same as in Example 1;

[0091] 2) In-situ growth of HKUST-1-pGO / LDHs film

[0092] 2g of p-aminophenol was dissolved in 600mL of deionized water, and the GO solution (prepared as in Example 3) was diluted to 0.1mg / mL using an alkaline p-aminophenol solution. The pH of the mixed solution was adjusted to 8.5 with a 1mol / L NaOH solution. The mixed solution was refluxed and stirred in an oil bath at 90°C for 12h. After the reaction, the pGO was centrifuged and washed several times with deionized water and ethanol, and dried overnight at 70°C to obtain pGO powder. The pGO powder was placed in a 1mol / L NaNO3 solution to prepare a pGO suspension with a concentration of 0.1mg / mL and sonicated for 1h. The pH of the pGO composite solution was adjusted to 10.8 with 3.0mol / L NaOH to obtain the pGO composite suspension.

[0093] Then, the pGO composite suspension was poured into the reactor and the reactor was sealed tightly. Finally, it was placed in a forced-air drying oven for in-situ growth. The reaction temperature was 418K and the constant temperature time was set to 12h to obtain the pGO / LDHs membrane sample.

[0094] The pGO / LDHs film sample was placed in a mixed solution of copper acetate and 1,3,5-benzenetriacrylic acid. The in-situ growth temperature was room temperature, and the growth time was 48 h.

[0095] Figure 12 This is a scanning electron microscope image of the HKUST-1-pGO / LDHs composite film layer on the surface of the magnesium alloy micro-arc oxidation film obtained in Example 5.

[0096] In Example 5, after HKUST-1 nanoparticles were grown in situ on the surface of the pGO / LDHs composite film, the surface morphology of the film changed significantly. The irregular voids in the pGL / MAO film disappeared completely, and an irregular particle distribution appeared on the surface, indicating that the polyhedral HKUST-1 crystals had been successfully fixed and grown on the surface of the pGL / MAO film.

[0097] 3) Cleaning and drying

[0098] The magnesium alloy prepared in step 2 was first rinsed with deionized water, then placed in anhydrous ethanol and ultrasonicated for 10 minutes in an ultrasonic cleaner to remove surface residues. After rinsing with deionized water and drying with a hair dryer, it was stored in a dry environment for further testing of morphology, corrosion resistance, self-healing properties, etc.

[0099] Figure 13The image shows the XRD pattern of the magnesium alloy micro-arc oxidation film HKUST-1-pGO / LDHs obtained in Example 5. The H-pGL / MAO film showed a diffraction peak of 200° at 6.6°, which is in good agreement with the simulated XRD pattern of the powdered HKUST-1 material, thus confirming the successful in-situ growth of the HKUST-1 crystal structure on the pGL / MAO film.

[0100] Figure 14 These are the impedance spectra of MAO films, LDHs films, GO / LDHs films, pGO / LDHs films, and HKUST-1-pGO / LDHs films after immersion in 3.5 wt% NaCl solution for 7 days, measured by an electrochemical workstation in Example 5; |Z| of the HKUST-1-pGO / LDHs film after immersion for 7 days. 0.01Hz Reduced to 1.95×10 6 Ωcm 2 As the corrosive medium gradually penetrates into the interior of the film, the corrosion resistance of the film decreases.

[0101] Figure 15 The impedance spectra of MAO film, LDHs film, GO / LDHs film, pGO / LDHs film, and HKUST-1-pGO / LDHs obtained by electrochemical workstation in Example 5 after immersion in 3.5wt% NaCl solution for 14 days are shown below. The |Z| values ​​after further immersion for another 14 days are also included. 0.01Hz The value further increased to 5.37 × 10 6 Ωcm 2 This indicates that when the film layer is subjected to corrosive media and causes surface corrosion, it can react in time to the corroded area, release corrosion inhibitors, compensate for surface defects, prevent the spread of corrosion, and has excellent self-healing function.

[0102] Furthermore, the HKUST-1-pGO / LDHs film did not exhibit any special capacitive behavior over a wide frequency range, and the maximum phase angle remained unchanged during immersion. Throughout the immersion process, the phase angle of the HKUST-1-pGO / LDHs film at the highest frequency was consistently greater than that of other films. All results indicate that the barrier properties of the HKUST-1-pGO / LDHs film did not change during immersion, while HKUST-1 nanoparticles can seal the pores on the film surface, significantly improving the film's density and barrier properties. Additionally, the |Z| of the HKUST-1-pGO / LDHs film... 0.01Hz The value consistently remained at the highest level among all samples, indicating that the membrane has good compactness and optimal protective performance, and demonstrating that the HKUST-1-pGO / LDHs membrane has good self-healing properties.

[0103] Through extensive experimental research, the inventors discovered that HKUST-1-pGO / LDHs films can be prepared on the surface of magnesium alloy micro-arc oxidation films. The organic corrosion inhibitor p-aminophenol is loaded onto the GO surface using an amide reaction, and pGO / LDHs nanosheets are doped and grown using a one-step hydrothermal method. Subsequently, HKUST-1 nucleation and crystallization growth is induced through amide bonds, resulting in an HKUST-1 film on the surface. This successfully achieved the construction of the HKUST-1-pGO / LDHs film on the surface of magnesium alloy micro-arc oxidation films. The addition of the organic corrosion inhibitor p-aminophenol endows the film with self-healing properties, enabling it to respond to corrosion and repair damaged areas, exhibiting a self-healing effect. Furthermore, the in-situ growth of HKUST-1 nanoparticles seals the pores of the pGO / LDHs film itself, greatly improving the film's density and extending the intrusion path of corrosive media. At the same time, it protects the organic corrosion inhibitor p-aminophenol, preventing premature leakage of the inhibitor. This achieves long-term stability and good self-healing ability of the magnesium alloy, while fundamentally improving the protective performance of the magnesium alloy.

[0104] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be covered within the scope of the claims and specification of the present invention.

Claims

1. A method for preparing a micro-arc oxidation film-HKUST-1-pGOLDHs composite film on a magnesium alloy surface, characterized in that, Includes the following steps: A1) First, prepare a micro-arc oxidation film on the surface of the magnesium alloy; A2) In-situ growth of HKUST-1-pGOLDHs film on the surface of magnesium alloy after micro-arc oxidation; A3) Repeatedly clean the magnesium alloy film layer after the in-situ growth reaction in step A2) 2-5 times, and then dry it overnight; wherein, the in-situ growth in step A2) specifically includes the following steps: A21) Dissolve p-aminophenol powder in deionized water to obtain an alkaline solution of p-aminophenol; A22) The GO solution was diluted with an alkaline solution of p-aminophenol to prepare a pGO composite suspension; A23) The magnesium alloy after micro-arc oxidation was placed in pGO composite suspension for in-situ growth to obtain a magnesium alloy with a micro-arc oxidation film-pGOLDHs film layer on the surface. A24) was then placed in a mixed solution of copper acetate and 1,3,5-benzenetricarboxylic acid for in-situ growth to obtain a magnesium alloy with a micro-arc oxide film-HKUST-1-pGOLDHs composite film on the surface.

2. The method for preparing the micro-arc oxidation film-HKUST-1-pGOLDHs composite film on the surface of magnesium alloy according to claim 1, characterized in that, The bath solution used in step A1) to prepare the micro-arc oxidation film includes sodium aluminate and sodium hydroxide by mass-volume concentration, wherein the mass-volume concentration of sodium aluminate is 3-6 g / L and the mass-volume concentration of sodium hydroxide is 6-10 g / L.

3. The method for preparing the micro-arc oxidation film-HKUST-1-pGOLDHs composite film on the surface of magnesium alloy according to claim 1, characterized in that, In step A21), the preparation of pGO powder is specifically as follows: p-aminophenol is dissolved in deionized water, and the GO solution is diluted to 0.05-0.2 mg / mL with an alkaline p-aminophenol solution, the pH is adjusted to 8-9, the mixed solution is refluxed and stirred in an oil bath at 80-90 ℃ for 10-15 h; after the reaction is completed, the pGO is centrifuged and washed several times with deionized water and ethanol, and dried overnight at 60-80 ℃ to obtain pGO powder.

4. The method for preparing the micro-arc oxidation film-HKUST-1-pGOLDHs composite film on the surface of magnesium alloy according to claim 2 or 3, characterized in that, In step A22), the preparation of the pGO composite suspension is specifically as follows: pGO powder is placed in NaNO3 with a concentration of 0.5-1.5 mol / L to prepare a pGO concentration of 0.05-0.15 mg / mL suspension and sonicated for 0.5-1.5 h. The pH of the pGO composite solution is adjusted to 10-11 to obtain the pGO composite suspension.

5. The method for preparing the micro-arc oxidation film-HKUST-1-pGOLDHs composite film on the surface of magnesium alloy according to claim 1, characterized in that, The concentration of the alkaline solution of p-aminophenol is 20-40 mg / mL.

6. The method for preparing the micro-arc oxidation film-HKUST-1-pGOLDHs composite film on the surface of magnesium alloy according to claim 1, characterized in that, The copper acetate has a mass concentration of 30-40 mg / mL, and the 1,3,5-benzenetricarboxylic acid has a mass concentration of 35-50 mg / mL.

7. The method for preparing the micro-arc oxidation film-HKUST-1-pGOLDHs composite film on the surface of magnesium alloy according to claim 1, characterized in that, In step A23), the process conditions for in-situ growth are: reaction temperature of 418 K and reaction time of 10-15 h; in step A24), the process conditions for in-situ growth are: growth environment of room temperature and reaction time of 40-60 h.

8. The application of the method for preparing the micro-arc oxidation film-HKUST-1-pGOLDHs composite film on magnesium alloy surface according to any one of claims 1-7 in the surface treatment of magnesium alloys.

9. The application of the product obtained by the preparation method of the magnesium alloy surface micro-arc oxidation film-HKUST-1-pGOLDHs composite film according to any one of claims 1-7 in the fields of aviation, automobile, and electronic communication.

Citation Information

Patent Citations

  • Self assembly laminated infrared film material and preparation method of self assembly laminated infrared film material

    CN102876287A

  • GO-g-8-Hq (graphene oxide grafted 8-hydroxyquinoline) fluorescent complex and intercalated layered double hydroxide fluorescent composite thereof

    CN108329910A