Silicon nitride and boron doped silicon nitride based amorphous ceramic and high pressure preparation method thereof
Amorphous ceramics are prepared through polymer conversion and high-pressure synthesis methods, which solves the problem of uneven structure caused by sintering aids and achieves the preparation of high-density and high-hardness silicon nitride and boron-doped silicon nitride-based ceramic materials. , simplifying the process and reducing costs.
Patent Information
- Application Number
- CN202410265790.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-08
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-03-08
AI Technical Summary
In the prior art, sintering aids need to be added when preparing amorphous silicon nitride and silicon nitride-based ceramic materials, resulting in problems of uneven structure and insufficient performance.
Amorphous ceramic powder is prepared by polymer conversion method and sintered at low temperature through high-pressure synthesis method. Metal molybdenum foil wrapping and three-stage graphite heating body are used for heating and pressurization, avoiding the use of sintering aids and achieving High density material preparation.
It achieves the preparation of high-quality amorphous silicon nitride and silicon nitride-based ceramic materials without sintering aids, simplifies the process, reduces costs and preparation cycles, and improves the hardness and density of the materials.
Smart Images

Figure CN118206385B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ceramic material preparation, and in particular to a silicon nitride and boron-doped silicon nitride-based amorphous ceramic and a high-pressure preparation method thereof. Background Art
[0002] Amorphous ceramics are considered to be a second state of matter parallel to crystalline ceramics. Compared with crystalline materials, amorphous materials have more distorted crystal structures, high atomic uniformity, composition flexibility, isotropic molecular diffusion and more solid mixture permeation pathways, which give them unique properties in terms of electrical / thermal conductivity, mechanical strength, corrosion resistance and wear resistance, making them an interesting class of structural materials. In addition, compared with polycrystalline materials, bulk amorphous ceramics have no grain boundaries, which can reduce the impact of grain boundaries on material properties. At present, nitrogen-based ceramics such as BN, Si3N4, transition metal nitrides, and ternary and multi-element nitrides (such as SiON, SiAlON, SiBCN, etc.) have shown great application potential in the fields of industry and energy. Among these materials, polycrystalline Si3N4 and BN are the most widely used nitrides due to their chemical stability, low dielectric properties, high thermal conductivity and excellent corrosion resistance over a wide temperature range. However, compared with several polycrystalline silicon nitride and silicon nitride-based composite materials that have been extensively studied in the past two decades, the research on the preparation and properties of amorphous silicon nitride and silicon nitride-based materials is very limited. In the family of amorphous materials, the synthesis of bulk amorphous ceramics is challenging. In particular, amorphous covalent compounds such as Si3N4, BN, and SiC are difficult to solidify at low temperatures due to their low diffusion coefficients, but crystallize at high temperatures.
[0003] Therefore, it is of great scientific significance to find an efficient, convenient and universal method to prepare bulk amorphous silicon nitride and silicon nitride-based ceramics.
[0004] The polymer-derived ceramic (PDC) route is a promising method for preparing amorphous ceramic materials, which has significant advantages over traditional ceramic processing techniques. The PDC route can produce amorphous ceramics (such as SiC, BN, SiCN, SiOC and SiHfN, etc.) with unique phase composition and microstructure by designing pre-ceramic polymers. However, since the pyrolysis of organic functional groups is accompanied by the release of gaseous decomposition products, it is difficult to achieve a completely dense bulk material. Liquid phase sintering assisted by sintering aids is a common method for preparing dense materials, but the addition of sintering aids will cause impurities to be enriched in certain areas, resulting in material embrittlement, which seriously reduces the performance of amorphous ceramics. Without adding sintering aids, it is difficult to eliminate the internal non-uniform structure and achieve high densification. Therefore, it is necessary to innovate the sintering method of silicon nitride amorphous ceramics to eliminate the non-uniform structure and achieve a highly dense structure without adding sintering aids.
[0005] Therefore, designing and developing a new preparation method that combines the advantages of PDC with those of high-density amorphous ceramics to prepare an amorphous ceramic material without sintering aids is of great significance for improving the performance of silicon nitride and silicon nitride-based amorphous ceramic materials and promoting their application. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a high-pressure preparation method for silicon nitride and boron-doped silicon nitride-based amorphous ceramics, so as to solve the problem that conventional preparation methods need to add sintering aids during the preparation process and are prone to uneven structures.
[0007] In order to solve the above problems, the present invention provides a high-pressure preparation method of silicon nitride and boron-doped silicon nitride-based amorphous ceramics, comprising the following steps:
[0008] S1: Amorphous ceramic powders with different silicon-boron ratios were prepared by polymer conversion method;
[0009] S2: pre-processing the amorphous ceramic powder prepared in step S1 to obtain a raw material block;
[0010] S3: Wrap the raw material block obtained in step S2 with metal molybdenum foil and load it into the synthesis chamber of a six-sided top press, heat and pressurize it, keep it warm and pressurized, and then cool and release the pressure to obtain amorphous silicon nitride and boron-doped silicon nitride-based ceramic materials.
[0011] As a preferred solution, in the step S1, the amorphous ceramic powder is prepared at 1100° C. by using perhydropolysilazane and borane-modified perhydropolysilazane as a polymer.
[0012] As a preferred solution, in step S2, the pre-processing condition is: processing the amorphous ceramic powder into a cylinder by cold pressing.
[0013] As a preferred solution, in step S3, the heating and pressurizing conditions are: keeping the temperature at a pressure of 5 GPa and a temperature of 1000-1800° C. for 15 minutes and keeping the pressure at a pressure of 20 minutes.
[0014] As a preferred solution, the temperature is 1000-1200°C.
[0015] As a preferred solution, in step S3, the heating method of the chamber is: after the raw material block is placed in a sample crucible, the sample crucible is heated by electrified graphite, and the upper and lower ends of the sample crucible are insulated by magnesium oxide, and the outer wall of the sample crucible is in direct contact with graphite.
[0016] As a preferred solution, the electrically conductive medium is a steel cap and a molybdenum sheet.
[0017] As a preferred solution, the graphite thickness at the upper and lower ends of the sample crucible is smaller than the graphite at the sample crucible (i.e., the graphite on the side wall of the sample crucible), and the thickness of the graphite in direct contact with the sample crucible is thickened. Therefore, the graphite structure of the present invention is a "three-stage heating body".
[0018] As a preferred solution, in step S3, the cooling and decompression method is: after the insulation is completed, wait for the sample to cool naturally to room temperature and then release the pressure.
[0019] The above method of the present invention has a short preparation cycle and does not require a sintering aid. It uses polymer-converted ceramic powder to directly sinter at high pressure and low temperature, and prepares high-quality amorphous silicon nitride and silicon nitride-based ceramic materials by adjusting the synthesis temperature and element content; and the process flow of the present invention is simple, does not require a long sintering time and high temperature and pressure conditions, and prepares high-hardness silicon nitride and boron-doped silicon nitride-based amorphous ceramics by adjusting the temperature and element ratio. The method of the present invention greatly reduces the harsh conditions, cost and cycle for the preparation of silicon nitride and silicon nitride-based amorphous ceramics, and provides a reference for the preparation of other amorphous ceramic materials.
[0020] Another technical problem to be solved by the present invention is to provide a silicon nitride and boron-doped silicon nitride-based amorphous ceramic to solve the problem that conventional amorphous ceramics require sintering aids and have insufficient hardness.
[0021] In order to solve the above problems, the present invention provides a silicon nitride and boron-doped silicon nitride-based amorphous ceramic, wherein the silicon nitride and boron-doped silicon nitride-based amorphous ceramic is prepared by the above preparation method.
[0022] High pressure is considered to be a factor that affects the phase transition and performance of materials in parallel with temperature. The present invention utilizes a high temperature and high pressure method to prepare highly dense amorphous silicon nitride and silicon nitride-based ceramic materials. The method of the present invention does not require the addition of sintering aids and a long sintering time, and the preparation process is simple. The present invention can obtain high-quality amorphous silicon nitride and silicon nitride-based ceramic materials by adjusting the temperature under high pressure. The present invention can lay a foundation for the preparation and application of high-pressure sintering methods in amorphous ceramics. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the XRD pattern of the polymer-converted ceramic powder used in the experiment.
[0024] Figure 2 This is the assembly diagram of the three-stage high temperature and high pressure experiment used in the experiment.
[0025] Figure 3This is the XRD diagram of the Si3N4 (Si:B=1:0) samples synthesized at 1000°C, 1200°C, 1400°C, 1600°C, and 1800°C in Example 1.
[0026] Figure 4 These are the XRD patterns of SiBN (Si:B=1:1) samples synthesized at 1000°C, 1200°C, 1400°C, 1600°C, and 1800°C in Example 2.
[0027] Figure 5 These are the XRD patterns of SiBN (Si:B=1:2) samples synthesized at 1000°C, 1200°C, 1400°C, 1600°C, and 1800°C in Example 3.
[0028] Figure 6 These are the XRD patterns of SiBN (Si:B=1:5) samples synthesized at 1000°C, 1200°C, 1400°C, 1600°C, and 1800°C in Example 4.
[0029] Figure 7 It is the hardness of the amorphous SiBN ceramic material prepared at 5 GPa and 1000° C. at different Si / B ratios in Examples 1, 2, 3, and 4. DETAILED DESCRIPTION
[0030] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The present invention provides a high-pressure preparation method of silicon nitride and boron-doped silicon nitride-based amorphous ceramics, comprising the following steps:
[0032] S1: Amorphous ceramic powders with different silicon-boron ratios were prepared by polymer conversion method;
[0033] S2: pre-processing the amorphous ceramic powder prepared in step S1 to obtain a raw material block;
[0034] S3: Wrap the raw material block obtained in step S2 with metal molybdenum foil and load it into the synthesis chamber of a six-sided top press, heat and pressurize it, keep it warm and pressurized, and then cool and release the pressure to obtain amorphous silicon nitride and boron-doped silicon nitride-based ceramic materials.
[0035] Preferably, in the step S1, the amorphous ceramic powder is prepared at 1100° C. by using perhydropolysilazane and borane-modified perhydropolysilazane as a polymer.
[0036] Preferably, in step S2, the pre-processing condition is: processing the amorphous ceramic powder into a cylinder by cold pressing.
[0037] Preferably, in step S3, the heating and pressurizing conditions are: keeping the temperature at a pressure of 5 GPa and a temperature of 1000-1800° C. for 15 minutes and keeping the pressure at a pressure of 20 minutes.
[0038] Preferably, the temperature is 1000-1200°C.
[0039] Preferably, in step S3, the chamber is heated by placing the raw material block in a sample crucible, heating the sample crucible by electrifying graphite, and the upper and lower ends of the sample crucible are insulated by magnesium oxide, and the left and right ends of the sample crucible are in direct contact with graphite.
[0040] Preferably, the electrically conductive medium is a steel cap and a molybdenum sheet.
[0041] Preferably, the graphite thickness at the upper and lower ends of the sample crucible is greater than the graphite at the sample crucible.
[0042] Preferably, in step S3, the cooling and decompression method is: after the insulation is completed, wait for the sample to cool naturally to room temperature and then release the pressure.
[0043] The present invention provides a silicon nitride and boron-doped silicon nitride-based amorphous ceramic, wherein the silicon nitride and boron-doped silicon nitride-based amorphous ceramic is prepared by the above-mentioned preparation method.
[0044] like Figure 2 As shown, Figure 2 The three-stage high-temperature and high-pressure experimental assembly diagram used in the following embodiment of the present invention, that is, the synthesis chamber of the present invention, including pyrophyllite for pressure transmission on the left and right sides, steel caps and molybdenum sheets for electrical conduction at the upper and lower ends, and a graphite heating body for electrical conduction and heating, wherein the graphite includes top graphite, bottom graphite and middle graphite, the inner wall of the middle graphite is connected to the outer wall of the sample crucible, the upper and lower ends of the middle graphite are respectively connected to the top graphite and the bottom graphite, and finally a closed hollow cylindrical graphite is formed, the middle graphite The thickness of graphite is large, the thickness of top and bottom graphite is small, the thickness of top graphite is the same as that of bottom graphite, and in the graphite heating body, magnesium oxide is connected to the top and bottom of the sample crucible, and the side wall of the sample crucible is connected to a part of the inner wall of the graphite. Because in the actual heating process, in order to ensure the uniformity of the temperature of the synthesis cavity, the present invention adopts the above-mentioned segmented external heating method, that is, a three-stage graphite heating body, and the heating is more uniform by controlling the different diameters of the three-stage graphite heating body (top, bottom and middle section graphite).
[0045] Example 1
[0046] This embodiment provides a silicon nitride and boron-doped silicon nitride-based amorphous ceramic and a high-pressure preparation method thereof, the preparation method comprising the following steps:
[0047] S1: Amorphous ceramic powder (Si3N4, Si:B=1:0) was prepared at 1100°C by using perhydropolysilazane and borane-modified perhydropolysilazane as a polymer;
[0048] S2: The amorphous ceramic powder (Si3N4, Si:B=1:0) prepared by polymer conversion was cold pressed into a cylinder with a diameter of 6 mm and a height of 3 mm;
[0049] S3: Wrap with metal molybdenum foil and put into high temperature and high pressure synthesis block. The assembled cavity is externally heated by a three-section graphite tube, the synthesis pressure is 5GPa, the synthesis temperature is 1000℃, 1200℃, 1400℃, 1600℃, 1800℃, the temperature is kept for 15min, the pressure is kept for 20min, after the temperature is kept, the sample is naturally cooled to room temperature and then the pressure is released. The X-ray diffraction results of the samples prepared under different temperature conditions are shown in Figure 2 , hardness results are shown in Figure 7 .
[0050] Example 2
[0051] This embodiment provides a silicon nitride and boron-doped silicon nitride-based amorphous ceramic and a high-pressure preparation method thereof, the preparation method comprising the following steps:
[0052] S1: Amorphous ceramic powder was prepared at 1100°C by using perhydropolysilazane and borane-modified perhydropolysilazane as a polymer;
[0053] S2: The amorphous ceramic powder (SiBN, Si:B=1:1) prepared by polymer conversion was cold pressed into a cylinder with a diameter of 6 mm and a height of 3 mm;
[0054] S3: Wrapped with metal molybdenum foil and placed in a high-temperature and high-pressure synthesis block, the assembled cavity is externally heated using a three-section graphite tube. The synthesis pressure is 5 GPa, the synthesis temperature is 1000℃, 1200℃, 1400℃, 1600℃, 1800℃, and the temperature is kept for 15 minutes and the pressure is kept for 20 minutes. After the temperature is kept, the sample is naturally cooled to room temperature and then the pressure is released. The X-ray diffraction results of the samples prepared under different temperature conditions are shown in Figure 3 , hardness results are shown in Figure 7 .
[0055] Example 3
[0056] This embodiment provides a silicon nitride and boron-doped silicon nitride-based amorphous ceramic and a high-pressure preparation method thereof, the preparation method comprising the following steps:
[0057] S1: Amorphous ceramic powder was prepared at 1100°C by using perhydropolysilazane and borane-modified perhydropolysilazane as a polymer;
[0058] S2: The amorphous ceramic powder (SiBN, Si:B=1:2) prepared by polymer conversion was cold pressed into a cylinder with a diameter of 6 mm and a height of 3 mm;
[0059] S3: Wrapped with metal molybdenum foil and placed in a high-temperature and high-pressure synthesis block, the assembled cavity is externally heated using a three-section graphite tube. The synthesis pressure is 5 GPa, the synthesis temperature is 1000℃, 1200℃, 1400℃, 1600℃, 1800℃, the temperature is kept for 15 minutes, and the pressure is kept for 20 minutes. After the temperature is kept, the sample is naturally cooled to room temperature and then the pressure is released. The X-ray diffraction results of the samples prepared under different temperature conditions are shown in Figure 4 , hardness results are shown in Figure 7 .
[0060] Example 4
[0061] This embodiment provides a silicon nitride and boron-doped silicon nitride-based amorphous ceramic and a high-pressure preparation method thereof, the preparation method comprising the following steps:
[0062] S1: Amorphous ceramic powder was prepared at 1100°C by using perhydropolysilazane and borane-modified perhydropolysilazane as a polymer;
[0063] S2: The amorphous ceramic powder (SiBN, Si:B=1:5) prepared by polymer conversion was cold pressed into a cylinder with a diameter of 6 mm and a height of 3 mm;
[0064] S3: Wrapped with metal molybdenum foil and placed in a high-temperature and high-pressure synthesis block, the assembled cavity is externally heated using a three-section graphite tube. The synthesis pressure is 5 GPa, the synthesis temperature is 1000℃, 1200℃, 1400℃, 1600℃, 1800℃, the temperature is kept for 15 minutes, and the pressure is kept for 20 minutes. After the temperature is kept, the sample is naturally cooled to room temperature and then the pressure is released. The X-ray diffraction results of the samples prepared under different temperature conditions are shown in Figure 5 , hardness results are shown in Figure 7 .
[0065] The experiments involved in the above embodiments were completed in a 6mm experimental assembly of a domestic hinged six-sided hydraulic press, and the heating body adopted a three-section graphite heating body.
[0066] like Figure 1 As shown, Figure 1 is the XRD spectrum of the polymer-converted ceramic powder used in the above embodiment of the present invention; Figure 3-Figure 6As shown, it can be seen from the XRD diagrams in the above Examples 1, 2, 3 and 4 that: at 5 GPa, when the temperature reaches 1000-1200°C, the raw materials are converted into high-density silicon nitride and boron-doped silicon nitride-based amorphous ceramic materials in a relatively short period of time.
[0067] Figure 7 The hardness of the amorphous SiBN ceramic material prepared at 5 GPa and 1000°C at different Si / B ratios in Examples 1, 2, 3, and 4 is shown in FIG. Figure 7 It can be concluded that when the Si / B ratio is 1:2, the hardness of the amorphous SiBN ceramic material is the highest.
[0068] It can be seen from the above Examples 1-4 and the test results that higher pressure, lower synthesis temperature and appropriate boron content are important factors for preparing high-quality amorphous silicon nitride and silicon nitride-based ceramic materials.
[0069] Although the disclosure is disclosed as above, the protection scope of the disclosure is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the disclosure, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A high pressure preparation method for silicon nitride or boron-doped silicon nitride-based amorphous ceramics, characterized in that: The following steps are involved: S1: Amorphous ceramic powders with different silicon-boron ratios were prepared by polymer conversion method; S2: pre-processing the amorphous ceramic powder prepared in step S1 to obtain a raw material block; S3: wrapping the raw material block obtained in step S2 with metal molybdenum foil and loading it into the synthesis chamber of a six-sided top press, heating and pressurizing it and keeping it warm and pressurized, then cooling and releasing the pressure to obtain amorphous silicon nitride or boron-doped silicon nitride-based ceramic material; in step S3, the heating and pressurizing conditions are: keeping warm for 15 minutes and keeping the pressure for 20 minutes under the conditions of a pressure of 5 GPa and a temperature of 1000-1200°C.
2. The high pressure preparation method of silicon nitride or boron-doped silicon nitride-based amorphous ceramics according to claim 1, characterized in that: In the step S1, the amorphous ceramic powder is prepared at 1100° C. by using perhydropolysilazane and borane-modified perhydropolysilazane as a polymer.
3. The high pressure preparation method of silicon nitride or boron-doped silicon nitride-based amorphous ceramics according to claim 1, characterized in that: In the step S2, the pre-processing condition is: processing the amorphous ceramic powder into a cylinder by cold pressing.
4. The high pressure preparation method of silicon nitride or boron-doped silicon nitride-based amorphous ceramics according to claim 1, characterized in that: In step S3, the chamber is heated in the following manner: after placing the raw material block in a sample crucible, the sample crucible is heated by electrifying graphite, and the upper and lower ends of the sample crucible are insulated by magnesium oxide, and the left and right ends of the sample crucible are in direct contact with graphite.
5. The high pressure preparation method of silicon nitride or boron-doped silicon nitride-based amorphous ceramics according to claim 4, characterized in that: The graphite thickness at the upper and lower ends of the sample crucible is smaller than the graphite thickness at the side wall of the sample crucible.
6. The high pressure preparation method of silicon nitride or boron-doped silicon nitride-based amorphous ceramics according to claim 1, characterized in that: In step S3, the cooling and decompression method is: after the heat preservation is completed, the sample is allowed to cool naturally to room temperature before decompression.
7. A silicon nitride or boron-doped silicon nitride-based amorphous ceramic, characterized in that: The silicon nitride or boron-doped silicon nitride-based amorphous ceramic is prepared by any one of the preparation methods of claims 1-6.
Citation Information
Patent Citations
Ceramics of containing powder body of cubic silicon nitride, and preparation method
CN101050115A
Method for preparing nano / nano-type Si3N4 / SiC nano multi-phase ceramic
CN101265106A
High-pressure fast preparation method of high-heat-conduction rate and high-compactness silicon nitride material
CN108191434A
Silicon nitride-based composite ceramic and process for producing same
WO2010113555A1