A three-dimensional molybdenum disulfide nanoflower composite material and its preparation method and application
The preparation of three-dimensional molybdenum disulfide nanoflower composite material through Se doping solved the problem of slow response speed and low sensitivity of two-dimensional molybdenum disulfide nanosheets, achieving high sensitivity detection and good repeatability for NO2 gas, reducing gas sensitivity The cost of the sensor.
Patent Information
- Application Number
- CN202410578194.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-11
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-05-11
AI Technical Summary
As a gas-sensitive material, two-dimensional molybdenum disulfide nanosheets have problems such as slow response speed, low sensitivity and poor repeatability.
Se is used as anionic dopant to prepare three-dimensional molybdenum disulfide nanoflower composites. By controlling the morphology and crystal plane spacing, a channel that is more conducive to gas absorption and desorption is formed, which increases active sites and improves gas sensitivity and selectivity.
It significantly improves the response speed and sensitivity to NO2 gas, shortens the response time, enhances the repeatability, and reduces the cost of gas-sensitive sensors.
Smart Images

Figure CN118255392B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of gas-sensitive materials, and in particular relates to a three-dimensional molybdenum disulfide nanoflower composite material and a preparation method and application thereof. Background Art
[0002] NO2 gas is one of the causes of acid rain and ozone. It can cause acidification of surface water, photochemical smog and other environmental effects, and can also have adverse effects on human health. Therefore, comprehensive monitoring of NO2 gas emissions in the region is of great significance for monitoring air pollution and air quality. Resistive gas sensors are one of the common methods for NO2 gas detection. The main principle is that NO2 in the gas to be measured will capture electrons on the surface of the gas-sensitive material, causing the carrier concentration on its surface to change, thereby causing resistance changes. When the gas-sensitive element is exposed to the NO2 gas environment, the composite material will adsorb and desorb NO2, and this process will cause the resistance value of the gas-sensitive element to change. By monitoring this resistance change, the NO2 concentration can be effectively monitored. Two-dimensional nanomaterials have attracted much attention in the fields of flexible electronic devices, batteries, sensors, etc. because of their rich active sites, high specific surface area, and unique physical and chemical properties. The use of two-dimensional nanomaterials to prepare gas-sensitive materials for gas sensors is an important way to develop high-performance sensors.
[0003] MoS2 nanosheets are a typical transition metal dichalcogenide compound. Their surface has high NO2 gas adsorption strength and high surface area ratio, and are considered to be a gas-sensitive material with great potential. However, low conductivity and strong Mo-S bonds limit the development of MoS2 as a gas-sensitive material. Two-dimensional MoS2 nanosheets have problems of slow response speed, slow recovery speed, and poor repeatability as gas-sensitive materials. The performance of MoS2 nanosheets as gas-sensitive materials can be improved through modification and functionalization strategies such as element doping, defect engineering, surface functionalization, and the formation of heterogeneous structures. However, these modification and functionalization methods usually make the synthesis process of gas-sensitive materials complicated and the cost increases accordingly. Summary of the invention
[0004] In order to solve the problems of slow response speed, low sensitivity and poor repeatability of existing two-dimensional molybdenum disulfide nanosheets as gas-sensitive materials, the present invention provides a three-dimensional molybdenum disulfide nanoflower composite material and a preparation method and application thereof.
[0005] The technical solution of the present invention:
[0006] A three-dimensional molybdenum disulfide nanoflower composite material, the material is a nanoscale three-dimensional flower-like structure, the three-dimensional flower-like structure is composed of a plurality of layer structures, the diameter of the overall three-dimensional flower-like structure is 150 nm to 200 nm, and the specific surface area is 20m 2 / g~60 m2 / g.
[0007] A method for preparing a three-dimensional molybdenum disulfide nanoflower composite material comprises the following steps:
[0008] Step 1: Preparation of molybdenum disulfide precursor:
[0009] Dissolving sodium molybdate dihydrate and L-cysteine in deionized water, stirring to obtain a mixed solution I, placing the mixed solution I in an autoclave for heating, cooling to obtain a mixed solution II, centrifuging the mixed solution II to collect a precipitate, washing, and drying to obtain a molybdenum disulfide precursor;
[0010] Step 2: Preparation of three-dimensional molybdenum disulfide nanoflower composite materials:
[0011] The molybdenum disulfide precursor obtained in step 1 and selenium powder are placed in a tubular furnace, heated in an atmosphere of a mixed gas of hydrogen and argon, and the product is collected to obtain a Se-doped three-dimensional molybdenum disulfide nanoflower composite material.
[0012] Furthermore, in step 1, the mass ratio of sodium molybdate dihydrate and L-cysteine is 1-10:1; the mass volume ratio of the total mass of sodium molybdate dihydrate and L-cysteine to deionized water is 1.0 g-2.5 g: 35 mL-65 mL; and the stirring time is 30 min-60 min.
[0013] Furthermore, the heating treatment in step 1 is to heat the stainless steel autoclave in a water bath at 160°C to 220°C for 18 h to 24 h.
[0014] Furthermore, the centrifugation condition in step 1 is 5000 r / min~8000 r / min for 5 min~15 min; the washing is washing the precipitate with deionized water and anhydrous ethanol in sequence and collecting the precipitate by centrifugation; the drying is drying at 60°C~90°C for 12 h~24 h.
[0015] Furthermore, in step 2, the mass ratio of the molybdenum disulfide precursor to the selenium powder is 1:1-10, and the volume percentage of hydrogen in the hydrogen and argon mixed gas is 5%-8%.
[0016] Furthermore, the heating treatment in step 2 is performed at a constant temperature of 300°C to 600°C for 0.5 h to 3.5 h.
[0017] Application of a three-dimensional MoS2 nanoflower composite material in NO2 gas detection.
[0018] Furthermore, the application is to prepare a gas sensor using a three-dimensional molybdenum disulfide nanoflower composite material. The preparation method of the gas sensor is to ultrasonically disperse the molybdenum disulfide nanoflower composite material according to claim 1 in 1 to 10 times the volume of an ethanol solution to obtain a uniformly dispersed suspension, and then coat the suspension on an Au interdigital electrode cleaned with ethanol, and place it at 50°C to 90°C to dry for 2 h to 5 h to obtain a gas sensor.
[0019] Furthermore, the application is to place the gas sensor prepared from the three-dimensional molybdenum disulfide nanoflower composite material according to claim 1 under the conditions of 15°C to 35°C and 20% to 80% humidity to detect the NO2 gas concentration in the gas to be tested.
[0020] Beneficial effects of the present invention:
[0021] The present invention uses Se as an anion dopant to prepare a three-dimensional molybdenum disulfide nanoflower composite material, realizes the control of the composite material morphology and inter-crystalline spacing, thereby forming a channel that is more conducive to gas adsorption and desorption, making it easier for NO2 gas to enter the interior of the composite material, and improving the adsorption reversibility of the composite material. During the reaction process, Se doping causes structural distortion, generates abundant sulfur defects, provides more active sites, increases the contact probability between the composite material and NO2 molecules, improves the gas sensitivity of the composite material and the selectivity for NO2 molecules, and further shortens the response time.
[0022] The three-dimensional molybdenum disulfide nanoflower composite material provided by the present invention is used to prepare a gas sensor, and it is used to detect the NO2 gas concentration in the gas to be tested at room temperature. The sensitivity to the NO2 gas with a concentration of 100 ppm is 40.82, and the response time is 5.8 seconds. When the NO2 concentration decreases, the response value also decreases. The minimum detection limit is 0.1ppm, the corresponding response value is 1.2, and the response time is 14.7 seconds. After multiple NO2 adsorption and desorption tests, the repeatability of the three-dimensional molybdenum disulfide nanoflower composite material is still excellent, indicating that the composite material has high sensitivity and good repeatability, and can reduce the cost of gas sensors.
[0023] The preparation method of the three-dimensional molybdenum disulfide nanoflower composite material provided by the present invention has the characteristics of simple process, low cost, and environmentally friendly and non-toxic production process. The prepared three-dimensional molybdenum disulfide nanoflower composite material can significantly improve the performance of gas sensors and has important application prospects in the field of NO2 gas detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a scanning electron microscope image of the three-dimensional molybdenum disulfide nanoflower composite material prepared in Example 1;
[0025] Figure 2The X-ray diffraction pattern of the three-dimensional molybdenum disulfide nanoflower composite material prepared in Example 1;
[0026] Figure 3 The sensitivity curve of the gas sensor prepared in Example 7 for detecting NO2;
[0027] Figure 4 This is a gas selectivity test diagram of the gas sensor prepared in Example 7 at room temperature;
[0028] Figure 5 The sensitivity curve of the gas sensor prepared in Example 8 for detecting NO2;
[0029] Figure 6 This is a graph showing the repeatability test results of the gas sensor prepared in Example 8 for 100 ppm NO2 at room temperature. DETAILED DESCRIPTION
[0030] The technical solution of the present invention is further described below in conjunction with the embodiments, but it is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention shall be included in the protection scope of the present invention. The process equipment or devices not specifically noted in the following embodiments are all conventional equipment or devices in the art. If not specifically specified, the raw materials used in the embodiments of the present invention can be obtained commercially; if not specifically specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.
[0031] Embodiment 1
[0032] This embodiment provides a method for preparing a three-dimensional molybdenum disulfide nanoflower composite material, comprising the following steps:
[0033] Step 1: Preparation of molybdenum disulfide precursor:
[0034] 1 g of sodium molybdate dihydrate and 0.2 g of L-cysteine were dissolved in 50 mL of deionized water, and stirred for 40 min to obtain a mixed solution I. The obtained mixed solution I was placed in a stainless steel autoclave, and the stainless steel autoclave was heated in a water bath at 200 °C for 20 h, and then the stainless steel autoclave was cooled to room temperature to obtain a mixed solution II. The obtained mixed solution II was centrifuged at 6000 r / min for 10 min to collect the precipitate, and the precipitate obtained by centrifugation was washed with deionized water and anhydrous ethanol successively, and the precipitate was collected by centrifugation at 6000 r / min for 10 min, and the washed precipitate was placed in a vacuum drying oven at 65 °C for 15 h to obtain a molybdenum disulfide precursor.
[0035] Step 2: Preparation of three-dimensional molybdenum disulfide nanoflower composite materials:
[0036] 0.5 g of the molybdenum disulfide precursor obtained in step 1 and 1.5 g of selenium powder were placed in a tubular furnace, and in an atmosphere of a hydrogen and argon mixed gas with a hydrogen volume percentage of 6%, the product was collected after being kept at a constant temperature of 500 ° C for 3 h to obtain a Se-doped three-dimensional molybdenum disulfide nanoflower composite material.
[0037] Figure 1 The scanning electron microscope image of the three-dimensional molybdenum disulfide nanoflower composite material prepared in Example 1 is shown in FIG. 1 . It can be clearly seen from the figure that the three-dimensional flower-like structure is composed of several lamellar structures and has a rich lamellar structure. The diameter of the overall three-dimensional flower-like structure is 150 nm~200 nm, the interlayer spacing is 0.5 nm~0.8 nm, and the specific surface area is 20 m 2 / g~60 m 2 / g. The use of Se as an anion dopant to prepare a three-dimensional MoS2 nanoflower composite material realizes the control of the composite material morphology and interplanar spacing, thereby forming a channel that is more conducive to gas adsorption and desorption, making it easier for NO2 gas to enter the interior of the composite material, and improving the adsorption reversibility of the composite material.
[0038] Figure 2 This is an X-ray diffraction diagram of the three-dimensional molybdenum disulfide nanoflower composite material prepared in Example 1; it can be seen from the figure that the diffraction peaks of the compound, namely the 2θ angle values of 14.4º, 39.5º, 49.8º, 60.1º, and 70.1º, respectively match the (002), (103), (105), (008), and (108) crystal planes of the standard card of molybdenum disulfide, confirming the successful synthesis of the Se-doped molybdenum disulfide composite material. The 2θ angle value at 33.1º is offset compared with the (100) crystal plane of the standard card of molybdenum disulfide, which is caused by Se doping. During the reaction process, Se doping causes structural distortion, produces abundant sulfur defects, provides more active sites, increases the contact probability between the composite material and NO2 molecules, improves the gas sensitivity and selectivity of the composite material to NO2 molecules, and further shortens the response time.
[0039] Embodiment 2
[0040] This embodiment provides a method for preparing a three-dimensional molybdenum disulfide nanoflower composite material, comprising the following steps:
[0041] Step 1: Preparation of molybdenum disulfide precursor:
[0042] 1 g of sodium molybdate dihydrate and 0.2 g of L-cysteine were dissolved in 50 mL of deionized water, and stirred for 40 min to obtain a mixed solution I. The obtained mixed solution I was placed in a stainless steel autoclave, and the stainless steel autoclave was heated in a water bath at 210 °C for 20 h, and then the stainless steel autoclave was cooled to room temperature to obtain a mixed solution II. The obtained mixed solution II was centrifuged at 6000 r / min for 10 min to collect the precipitate, and the precipitate obtained by centrifugation was washed with deionized water and anhydrous ethanol successively, and the precipitate was collected by centrifugation at 6000 r / min for 10 min, and the washed precipitate was placed in a vacuum drying oven at 65 °C for 15 h to obtain a molybdenum disulfide precursor.
[0043] Step 2: Preparation of three-dimensional molybdenum disulfide nanoflower composite materials:
[0044] 0.5 g of the molybdenum disulfide precursor obtained in step 1 and 3 g of selenium powder were placed in a tubular furnace, and in an atmosphere of a hydrogen and argon mixed gas with a hydrogen volume percentage of 7%, the product was collected after constant temperature at 550 ° C for 2 h to obtain a Se-doped three-dimensional molybdenum disulfide nanoflower composite material.
[0045] Embodiment 3
[0046] This embodiment provides a method for preparing a three-dimensional molybdenum disulfide nanoflower composite material, comprising the following steps:
[0047] Step 1: Preparation of molybdenum disulfide precursor:
[0048] 1 g of sodium molybdate dihydrate and 1.0 g of L-cysteine were dissolved in 65 mL of deionized water, and stirred for 60 min to obtain a mixed solution I. The obtained mixed solution I was placed in a stainless steel autoclave, and the stainless steel autoclave was heated in a water bath at 180 °C for 24 h, and then the stainless steel autoclave was cooled to room temperature to obtain a mixed solution II. The obtained mixed solution II was centrifuged at 5000 r / min for 15 min to collect the precipitate, and the precipitate obtained by centrifugation was washed with deionized water and anhydrous ethanol successively, and the precipitate was collected by centrifugation at 5000 r / min for 15 min, and the washed precipitate was placed in a vacuum drying oven at 70 °C for 12 h to obtain a molybdenum disulfide precursor.
[0049] Step 2: Preparation of three-dimensional molybdenum disulfide nanoflower composite materials:
[0050] 0.5 g of the molybdenum disulfide precursor obtained in step 1 and 0.5 g of selenium powder were placed in a tubular furnace, and in an atmosphere of a hydrogen and argon mixed gas with a hydrogen volume percentage of 5%, the product was collected after constant temperature at 600 ° C for 3.5 h to obtain a Se-doped three-dimensional molybdenum disulfide nanoflower composite material.
[0051] Embodiment 4
[0052] This embodiment provides a method for preparing a three-dimensional molybdenum disulfide nanoflower composite material, comprising the following steps:
[0053] Step 1: Preparation of molybdenum disulfide precursor:
[0054] 1 g of sodium molybdate dihydrate and 0.3 g of L-cysteine were dissolved in 60 mL of deionized water, and stirred for 50 min to obtain a mixed solution I. The obtained mixed solution I was placed in a stainless steel autoclave, and the stainless steel autoclave was heated in a water bath at 190 °C for 22 h, and then the stainless steel autoclave was cooled to room temperature to obtain a mixed solution II. The obtained mixed solution II was centrifuged at 5000 r / min for 15 min to collect the precipitate, and the precipitate obtained by centrifugation was washed with deionized water and anhydrous ethanol successively, and the precipitate was collected by centrifugation at 7000 r / min for 15 min, and the washed precipitate was placed in a vacuum drying oven at 80 °C for 18 h to obtain a molybdenum disulfide precursor.
[0055] Step 2: Preparation of three-dimensional molybdenum disulfide nanoflower composite materials:
[0056] 0.5 g of the molybdenum disulfide precursor obtained in step 1 and 2.5 g of selenium powder were placed in a tubular furnace, and in an atmosphere of a hydrogen and argon mixed gas with a hydrogen volume percentage of 6%, the product was collected after constant temperature at 550 ° C for 3 h to obtain a Se-doped three-dimensional molybdenum disulfide nanoflower composite material.
[0057] Embodiment 5
[0058] This embodiment provides a method for preparing a three-dimensional molybdenum disulfide nanoflower composite material, comprising the following steps:
[0059] Step 1: Preparation of molybdenum disulfide precursor:
[0060] 1 g of sodium molybdate dihydrate and 0.15 g of L-cysteine were dissolved in 40 mL of deionized water, and stirred for 40 min to obtain a mixed solution I. The obtained mixed solution I was placed in a stainless steel autoclave, and the stainless steel autoclave was heated in a water bath at 220 °C for 18 h, and then the stainless steel autoclave was cooled to room temperature to obtain a mixed solution II. The obtained mixed solution II was centrifuged at 8000 r / min for 5 min to collect the precipitate, and the precipitate obtained by centrifugation was washed with deionized water and anhydrous ethanol successively, and the washed precipitate was placed in a vacuum drying oven at 70 °C for 20 h to obtain a molybdenum disulfide precursor.
[0061] Step 2: Preparation of three-dimensional molybdenum disulfide nanoflower composite materials:
[0062] 0.5 g of the molybdenum disulfide precursor obtained in step 1 and 4 g of selenium powder were placed in a tubular furnace, and in an atmosphere of a mixed gas of hydrogen and argon with a hydrogen volume percentage of 7%, the product was collected after being kept at a constant temperature of 500 °C for 2 h to obtain a Se-doped three-dimensional molybdenum disulfide nanoflower composite material.
[0063] Embodiment 6
[0064] This embodiment provides a method for preparing a three-dimensional molybdenum disulfide nanoflower composite material, comprising the following steps:
[0065] Step 1: Preparation of molybdenum disulfide precursor:
[0066] 1 g of sodium molybdate dihydrate and 0.1 g of L-cysteine were dissolved in 35 mL of deionized water, and stirred for 30 min to obtain a mixed solution I. The obtained mixed solution I was placed in a stainless steel autoclave, and the stainless steel autoclave was heated in a water bath at 170 °C for 22 h, and then the stainless steel autoclave was cooled to room temperature to obtain a mixed solution II. The obtained mixed solution II was centrifuged at 8000 r / min for 5 min to collect the precipitate, and the precipitate obtained by centrifugation was washed with deionized water and anhydrous ethanol successively, and the precipitate was collected by centrifugation at 8000 r / min for 5 min, and the washed precipitate was placed in a vacuum drying oven at 60 °C for 24 h to obtain a molybdenum disulfide precursor.
[0067] Step 2: Preparation of three-dimensional molybdenum disulfide nanoflower composite materials:
[0068] 0.5 g of the molybdenum disulfide precursor obtained in step 1 and 5 g of selenium powder were placed in a tubular furnace, and in an atmosphere of a hydrogen and argon mixed gas with a hydrogen volume percentage of 8%, the product was collected after constant temperature at 600 ° C for 0.5 h to obtain a Se-doped three-dimensional molybdenum disulfide nanoflower composite material.
[0069] Embodiment 7
[0070] This embodiment provides a gas sensing element made of the three-dimensional molybdenum disulfide nanoflower composite material prepared in Example 1 as a gas sensing material.
[0071] The specific preparation method of the gas sensor in this embodiment is:
[0072] The three-dimensional molybdenum disulfide nanoflower composite material prepared in Example 1 was ultrasonically dispersed in 5 times the volume of anhydrous ethanol solution to obtain a uniformly dispersed suspension, and then the suspension was spin-coated on the Au interdigital electrode washed with ethanol and dried at 60°C for 4 h to obtain a gas sensor.
[0073] The prepared gas-sensitive element was subjected to gas-sensitive detection by the static gas distribution method. The specific steps were as follows: first, the gas-sensitive element to be tested was installed in the gas chamber and connected to the information acquisition and analysis equipment. At a detection temperature of 25 °C and a detection humidity of 25%, 100 ppm of NO2 was injected. When the gas-sensitive response was observed to be stable according to the information fed back by the data acquisition system, an air pump was used to evacuate the gas to desorb NO2, and the device to be tested returned to its initial state, completing a gas injection cycle. Then, 100 ppm, 50 ppm, 30 ppm, 10 ppm, 5 ppm, 3 ppm, 1 ppm, 0.5 ppm and 0.3 ppm, 0.1 ppm NO2 gas injection cycles were performed in sequence. After completing the gas injection cycle, the following is obtained: Figure 3 The sensitivity curve of the gas sensor prepared in this embodiment for detecting nitrogen dioxide is shown. The sensitivity to the gas with a NO2 concentration of 100 ppm is 40.82, and the sensitivity to the gas with a NO2 concentration as low as 0.1 ppm is 1.2. In addition, the material has a fast response speed and good adsorption reversibility.
[0074] Table 1 shows the sensitivity and response time of the gas sensor prepared in this example under different nitrogen dioxide concentrations, where sensitivity S=R a / R g , R a is the resistance of the sensor in air, R g is the resistance of the sensor in NO2 atmosphere. During gas adsorption and desorption, the time required for the resistance to change by 90% is the response time.
[0075] Table 1
[0076]
[0077] Figure 4 This is a gas selectivity test diagram of the gas sensor prepared in this embodiment at room temperature, wherein the test gases include: NO2, H2S, NH3, SO2 and N2O. Except for NO2 with an injection concentration of 100 ppm, the injection concentrations of the other gases are 10000 ppm. Figure 4 The results show that the gas sensor made of the three-dimensional molybdenum disulfide nanoflower composite material prepared in Example 1 as a gas-sensitive material has excellent selectivity for NO2 at room temperature.
[0078] Embodiment 8
[0079] This embodiment provides a gas sensing element made of the three-dimensional molybdenum disulfide nanoflower composite material prepared in Example 2 as a gas sensing material.
[0080] The specific preparation method of the gas sensor in this embodiment is:
[0081] The three-dimensional molybdenum disulfide nanoflower composite material prepared in Example 2 was ultrasonically dispersed in 5 times the volume of anhydrous ethanol solution to obtain a uniformly dispersed suspension, and then the suspension was spin-coated on the Au interdigital electrode cleaned with ethanol and dried at 60°C for 4 h to obtain a gas sensor.
[0082] The prepared gas-sensitive element was subjected to gas-sensitive detection by the static gas distribution method. The specific steps were as follows: first, the gas-sensitive element to be tested was installed in the gas chamber and connected to the information acquisition and analysis equipment. At a detection temperature of 30 °C and a detection humidity of 35%, 100 ppm of NO2 was injected. When the gas-sensitive response was observed to be stable according to the information fed back by the data acquisition system, an air pump was used to evacuate the gas to desorb NO2, and the device to be tested returned to its initial state, completing a gas injection cycle. Then, 100 ppm, 50 ppm, 30 ppm, 10 ppm, 5 ppm, 3 ppm, 1 ppm, 0.5 ppm, 0.3 ppm, and 0.1 ppm of NO2 gas injection cycles were performed in sequence. After completing the gas injection cycle, the following is obtained: Figure 5 The sensitivity curve of the gas sensor prepared in this embodiment for detecting nitrogen dioxide shows that the sensitivity to the gas with a NO2 concentration of 100 ppm is 24.1, and the sensitivity to the gas with a NO2 concentration as low as 0.1 ppm is 1.2.
[0083] Figure 6 The figure is the repeatability test result of the gas sensor prepared in this embodiment for 100 ppm NO2 at room temperature. As can be seen from the figure, after the sensitive film formed by the three-dimensional molybdenum disulfide nanoflower composite material prepared by Se doping adsorbs NO2, the resistance value decreases rapidly, and after 7 consecutive cycles of adsorption-desorption of 100 ppm NO2, the repeatability is good.
Claims
1. A three-dimensional molybdenum disulfide nanoflower composite material, characterized in that: The material is a nanometer-scale three-dimensional flower-like structure, which is composed of a number of lamellae. The diameter of the whole three-dimensional flower-like structure is 150nm-200nm, and the specific surface area is 20m 2 / g~60m 2 / g; The preparation method of the three-dimensional molybdenum disulfide nanoflower composite material comprises the following steps: Step 1: Preparation of molybdenum disulfide precursor: Dissolving sodium molybdate dihydrate and L-cysteine in deionized water, stirring to obtain a mixed solution I, placing the mixed solution I in an autoclave for heating, cooling to obtain a mixed solution II, centrifuging the mixed solution II to collect a precipitate, washing, and drying to obtain a molybdenum disulfide precursor; Step 2: Preparation of three-dimensional molybdenum disulfide nanoflower composite materials: The molybdenum disulfide precursor and selenium powder obtained in step 1 are placed in a tubular furnace and heated in an atmosphere of a mixed gas of hydrogen and argon. The heating treatment is performed at a constant temperature of 300°C to 600°C for 0.5h to 3.5h. The product is collected to obtain a Se-doped three-dimensional molybdenum disulfide nanoflower composite material.
2. A three-dimensional molybdenum disulfide nanoflower composite material according to claim 1, characterized in that: In step 1, the mass ratio of sodium molybdate dihydrate and L-cysteine is 1-10:1; the mass volume ratio of the total mass of sodium molybdate dihydrate and L-cysteine to deionized water is 1.0g-2.5g:35mL-65mL; and the stirring time of the stirring is 30min-60min.
3. A three-dimensional molybdenum disulfide nanoflower composite material according to claim 1 or 2, characterized in that: The heating treatment in step 1 is to heat the stainless steel autoclave in a water bath at 160° C. to 220° C. for 18 h to 24 h.
4. A three-dimensional molybdenum disulfide nanoflower composite material according to claim 3, characterized in that: The centrifugal conditions of step 1 are 5000r / min~8000r / min for 5min~15min; the washing is washing the precipitate with deionized water and anhydrous ethanol in turn and collecting the precipitate by centrifugation; the drying is drying at 60℃~90℃ for 12h~24h.
5. A three-dimensional molybdenum disulfide nanoflower composite material according to claim 4, characterized in that: In step 2, the mass ratio of the molybdenum disulfide precursor to the selenium powder is 1:1-10, and the volume percentage of hydrogen in the hydrogen and argon mixed gas is 5%-8%.
6. An application of the three-dimensional molybdenum disulfide nanoflower composite material as claimed in claim 1 in NO2 gas detection.
7. The use of the three-dimensional molybdenum disulfide nanoflower composite material in NO2 gas detection according to claim 6, characterized in that: The application is to prepare a gas sensor with a three-dimensional molybdenum disulfide nanoflower composite material. The preparation method of the gas sensor is to ultrasonically disperse the molybdenum disulfide nanoflower composite material described in claim 1 in 1 to 10 times the volume of an ethanol solution to obtain a uniformly dispersed suspension, and then coat the suspension on an Au interdigital electrode cleaned with ethanol, and place it at 50°C to 90°C for 2h to 5h to obtain a gas sensor.
8. The use of the three-dimensional molybdenum disulfide nanoflower composite material in NO2 gas detection according to claim 7, characterized in that: The application is to place the gas sensor prepared from the three-dimensional molybdenum disulfide nanoflower composite material according to claim 1 under the conditions of 15°C to 35°C and 20% to 80% humidity to detect the NO2 gas concentration in the gas to be tested.
Citation Information
Patent Citations
Method for hydro-thermally synthesizing MoS<2> nanoflower with sulfur-containing biological reagent as sulfur source
CN105366725A
Molybdenum disulfide / ferroferric oxide magnetic nanocomposite material and preparation method and application thereof
CN109806889A
MoS2-xSex graded gas-sensitive material with high activity performance at room temperature and preparation method of MoS2-xSex graded gas-sensitive material
CN114477103A
Cited By
Three-dimensional nanoflower composite gas sensitive material, preparation method and application thereof
CN120097383B