Reconstruction of durable waterproof layer process

The prepared waterproof and mildew-proof sealant solves the problem of mold growth in the presence of moisture, achieving comprehensive waterproofing and leak repair, and extending service life.

CN118257441BActive Publication Date: 2026-11-17GUANGDONG JIUAN WATERPROOF TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410364752.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-27
Publication Date
2026-11-17
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

Existing waterproof sealants are prone to mold growth in the presence of moisture, which affects their waterproof sealing effect and cannot effectively solve the problems of water ingress and leakage.

Method used

A silane-modified polyether sealant is prepared by mixing 6-fluoro-3-(2-propenyl)-2(3H)-benzothiazoline-5-isocyanate with 3-mercaptopropyltriethoxysilane to prepare a modified siloxane, which is then reacted with a polyether polyol to prepare a waterproof and mildew-proof sealant for use in the process of reconstructing a durable waterproof layer.

Benefits of technology

It achieves a completely new waterproof system by forming an internal water-passing channel, automatically sealing the water inlet, replacing the water-passing space with waterproof material, and automatically repairing the inside of the leak point, thus extending the service life and strengthening the waterproof sealing effect.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the technical field of construction measures for existing buildings, specifically disclosing a process for reconstructing a durable waterproof layer. This invention uses perforated grouting to create a new waterproof layer on the water-facing side, thereby repairing water ingress points and completely solving building leakage problems. Compared with existing technologies, this invention, through the synthesis and modification of silane-modified polyether sealant, not only produces a waterproof sealant but also provides anti-mildew effects, thus extending its service life and enhancing its waterproof sealing performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of construction measures for existing buildings, and in particular to a process for reconstructing a durable waterproof layer. Background Technology

[0002] With the increasing scale and number of building construction projects, the development of underground space is becoming more and more common. The rational and full utilization of underground space not only achieves energy conservation and environmental protection, but is also an important means to meet the growing functional needs of the people for buildings. However, due to various complex factors, the problems of water seepage and leakage in basements cannot be effectively solved, affecting the normal use of basements.

[0003] Chinese patent application 202111315146.1 discloses a method for plugging and repairing leaks in the basement structural slab, comprising the following steps: S1. Cleaning the base layer of the leaking area, locating the leak line or leak point, and setting grouting holes along the leak line or at the leak point; S2. Injecting plugging grout into the grouting holes sequentially, wherein the grouting sequence is from the grouting holes on the periphery of the leaking area to the grouting holes in the center, and from the end of the leak line to the middle sequentially; S3. Inserting several anchor rods inside and outside the leaking area, binding a steel mesh between the anchor rods, and pouring concrete on the steel mesh. This invention facilitates timely and smooth drainage of seepage water by grouting from the outside to the inside, which is beneficial to the continuity of grouting; it enhances the anti-seepage effect by setting an anchored reinforced concrete layer on the leaking area, avoiding waterproofing failure; setting inclined grouting holes that intersect with the leak line ensures smooth injection of plugging grout into the cracks; it avoids secondary leakage caused by setting grouting holes and anchor rods; and it is suitable for situations where the leak lines and points are relatively dense.

[0004] Chinese Patent 202110199874.4 relates to the field of building repair. This invention provides a minimally invasive method for reconstructing a waterproof layer, including steps such as sealing cracks, drilling, injecting filler, injecting waterproof sealant, and sealing grouting holes. The invention uses a drilling and injection method to inject a back filler and waterproof sealant into the interior of the building wall, achieving the purpose of reconstructing the waterproof layer. The invention provides methods for preparing the back filler and waterproof sealant; both materials have moderate viscosity, suitable for injection filling, and exhibit good adhesion and excellent waterproof performance after complete curing. The waterproof layer reconstruction method of this invention has simple operation procedures, saves materials and manpower, causes minimal damage to the original wall decoration, has a short construction period, and can efficiently and quickly solve leakage and water seepage problems. Urban buildings often experience water leakage after construction due to various reasons, seriously affecting normal and safe use. This invention combines waterproofing reconstruction with a flexible and rigid approach, adapting to local conditions, and using a comprehensive treatment method to solve the problem of basement water leakage.

[0005] Generally, the water inlet and the leak are not the same point. Traditional leak sealing methods only seal the leak point, failing to address the water inlet and the problem of water seepage. Water continues to corrode the steel reinforcement within the concrete structure, causing steel corrosion and expansion, creating new cracks and new leaks, further compromising structural safety. Reconstructing the waterproof layer can simultaneously address both the water inlet and the leak, completely repairing the seepage. However, existing waterproof sealants are prone to mold growth in the presence of moisture, affecting their sealing effectiveness. Summary of the Invention

[0006] In view of the above-mentioned deficiencies of the prior art, the technical problem to be solved by the present invention is to provide a process for reconstructing a durable waterproof layer.

[0007] Silane-modified polyether sealant is a novel, high-performance adhesive and sealing material developed in recent years. It combines the advantages of polyurethane and silicone sealants, exhibiting good storage stability, high elasticity, flexibility, excellent adhesion, paintability, environmental friendliness, and no substrate contamination. In this invention, a modified siloxane is obtained by mixing 6-fluoro-3-(2-propenyl)-2(3H)-benzothiazoline-5-isocyanate with 3-mercaptopropyltriethoxysilane, followed by reaction with a polyether polyol to obtain the silane-modified polyether sealant. Due to the modified siloxane... The benzothiazole heterocycle in the alkyl group exhibits excellent antibacterial activity. The benzothiazole ring can interact with multiple targets of bacteria, thereby inactivating them. The strong electron-withdrawing groups and halogen atoms on 6-fluoro-3-(2-propenyl)-2(3H)-benzothiazolin-5-isocyanate further enhance its antibacterial activity. Mixing it with 3-mercaptopropyltriethoxysilane yields a modified siloxane, which is then used to prepare a silane-modified polyether sealant. This not only provides a waterproof sealant but also has anti-mildew properties, extending its service life and strengthening its waterproof sealing effect. The reconstructed durable waterproof layer process of this invention can achieve multi-point and multi-layer formation, creating a completely new, integrated waterproof system within the internal water-channeling system. This achieves automatic sealing at water inlets, replacement of water-channeling spaces with waterproof material, and automatic repair of leaks on the inside.

[0008] To achieve the above objectives, the present invention provides a process for reconstructing a durable waterproof layer, comprising the following steps:

[0009] S1. Locate the leak and treat the cracks;

[0010] S2. Drill holes in the treated surface to penetrate the protective layer and insert grouting needles;

[0011] S3. Inject back filler through the grouting needle, with the injection volume based on the injection of this needle, and grout exiting from other pressure relief holes within the corresponding area;

[0012] S4. Inject waterproof and mildew-proof sealant through the grouting needle. The injection volume is based on the injection of this needle, and the grout comes out of other pressure relief holes in the corresponding area.

[0013] S5. Seal the grouting holes and restore the finish to complete the reconstruction of the waterproof layer.

[0014] Furthermore, the number of grouting needles is 3 to 5 per meter. 2 .

[0015] Furthermore, the back filler is epoxy acrylate.

[0016] The preparation method of the waterproof and mildew-proof sealant includes the following steps:

[0017] X1. 6-fluoro-3-(2-propenyl)-2(3H)-benzothiazoline-5-isocyanate and 3-mercaptopropyltriethoxysilane were added to anhydrous ethanol, and then azobisisobutyronitrile was added. The mixture was heated and stirred. After stirring, the mixture was cooled to room temperature and concentrated under reduced pressure to dryness to obtain modified siloxane.

[0018] X2. After mixing polyether diol and modified siloxane, heat and stir. After stirring, silane-modified polyether is obtained.

[0019] X3. After mixing the filler and plasticizer, heat and dehydrate them. Then add silane-modified polyether, silane coupling agent, catalyst, and dehydrating agent, mix and stir until uniform, and then discharge to obtain waterproof and mildew-proof sealant.

[0020] Furthermore, in step X1, the heating and stirring temperature is 70–90°C, and the time is 2–5 hours.

[0021] Furthermore, in step X2, the heating and stirring temperature is 80–90°C, and the time is 12–16 hours.

[0022] Furthermore, the filler is one of light calcium carbonate, nano zinc oxide, or kaolin.

[0023] Furthermore, the plasticizer is dioctyl phthalate.

[0024] Furthermore, the silane coupling agent is (3-aminopropyl)trimethoxysilane.

[0025] Furthermore, the catalyst is dibutyltin dilaurate.

[0026] Furthermore, the dehydrating agent is vinyltris(2-methoxyethoxy)silane.

[0027] Furthermore, the mass ratio of the silane-modified polyether to the filler, plasticizer, silane coupling agent, catalyst, and dehydrating agent is 5-15:5-16:1-5:0.1-0.5:0.01-0.04:0.1-0.2.

[0028] Preferably, the preparation method of the waterproof and mildew-proof sealant includes the following steps:

[0029] X1. Add 4-8 parts by weight of 6-fluoro-3-(2-propenyl)-2(3H)-benzothiazoline-5-isocyanate and 4-10 parts by weight of 3-mercaptopropyltriethoxysilane to 50-100 parts by weight of anhydrous ethanol, then add 0.01-0.2 parts by weight of azobisisobutyronitrile, heat to 70-90℃ and stir for 2-5 hours. After stirring, cool to room temperature and concentrate under reduced pressure to dryness to obtain modified siloxane.

[0030] X2. Mix 100-150 parts by weight of polyether diol and 9-15 parts by weight of modified siloxane, heat to 80-90℃ and stir for 12-16 hours. After stirring, silane-modified polyether is obtained.

[0031] X3. After mixing the filler and plasticizer, heat to 110-130℃ to dehydrate. Then add silane-modified polyether, silane coupling agent, catalyst, and dehydrating agent and mix for 30-60 minutes. The mass ratio of silane-modified polyether to filler, plasticizer, silane coupling agent, catalyst, and dehydrating agent is 5-15:5-16:1-5:0.1-0.5:0.01-0.04:0.1-0.2. After mixing evenly, discharge to obtain the waterproof and mildew-proof sealant.

[0032] The beneficial effects of this invention are:

[0033] 1. Compared with the prior art, the reconstructed durable waterproof layer process of the present invention can achieve multi-point forming and multi-sheet forming, forming a brand-new whole-surface waterproof system in the internal water channel; achieving the effect of automatic sealing of water inlet points, replacement of water channel space with waterproof material, and automatic repair of the inside of leak points.

[0034] 2. Compared with existing technologies, this invention uses perforated grouting to create a new waterproof layer on the water-facing side, thereby repairing the water ingress point and completely solving the building leakage problem.

[0035] 3. The present invention, through the synthesis and modification of siloxanes and subsequent preparation of silane-modified polyether sealant, not only provides a waterproof sealant but also has an anti-mildew effect, thereby extending its service life and enhancing its waterproof and sealing properties. Detailed Implementation

[0036] 6-Fluoro-3-(2-propenyl)-2(3H)-benzothiazolon-5-yl isocyanate, CAS No.: 112893-03-5.

[0037] Polyether diol, Mw = 12000.

[0038] Epoxy acrylate, model: RJ351, Guangzhou Lihou Trading Co., Ltd.

[0039] 5-Isocyanatopent-1-ene, CAS No.: 2487-98-1.

[0040] Compare with Example 1

[0041] A process for reconstructing a durable waterproof layer includes the following steps:

[0042] S1. Locate the leak and treat the cracks;

[0043] S2. Drill holes in the treated surface, penetrating the protective layer, and insert grouting needles. The number of grouting needles is 4 per m. 2 ;

[0044] S3. Inject epoxy acrylate through the grouting needle, with the injection volume based on the injection of this needle, and grout exiting from other pressure relief holes within the corresponding area;

[0045] S4. Inject waterproof and mildew-proof sealant through the grouting needle. The injection volume is based on the injection of this needle, and the grout comes out of other pressure relief holes in the corresponding area.

[0046] S5. Seal the grouting holes and restore the finish to complete the reconstruction of the waterproof layer.

[0047] The preparation method of the waterproof and mildew-proof sealant includes the following steps:

[0048] X1. Mix 120g of polyether diol and 10g of 3-mercaptopropyltriethoxysilane, heat to 80℃ and stir for 14h. After stirring, silane-modified polyether is obtained.

[0049] X2. After mixing light calcium carbonate and dioctyl phthalate, heat to dehydrate. Then add silane-modified polyether, (3-aminopropyl)trimethoxysilane, dibutyltin dilaurate, and vinyltris(2-methoxyethoxy)silane and stir for 40 minutes. The mass ratio of silane-modified polyether to light calcium carbonate, dioctyl phthalate, (3-aminopropyl)trimethoxysilane, dibutyltin dilaurate, and vinyltris(2-methoxyethoxy)silane is 10:10:3:0.3:0.02:0.1. After mixing evenly, discharge to obtain waterproof and mildew-proof sealant.

[0050] Compare with Example 2

[0051] A process for reconstructing a durable waterproof layer includes the following steps:

[0052] S1. Locate the leak and treat the cracks;

[0053] S2. Drill holes in the treated surface, penetrating the protective layer, and insert grouting needles. The number of grouting needles is 4 per m. 2 ;

[0054] S3. Inject epoxy acrylate through the grouting needle, with the injection volume based on the injection of this needle, and grout exiting from other pressure relief holes within the corresponding area;

[0055] S4. Inject waterproof and mildew-proof sealant through the grouting needle. The injection volume is based on the injection of this needle, and the grout comes out of other pressure relief holes in the corresponding area.

[0056] S5. Seal the grouting holes and restore the finish to complete the reconstruction of the waterproof layer.

[0057] The preparation method of the waterproof and mildew-proof sealant includes the following steps:

[0058] X1. Mix 120g of polyether diol and 10g of 3-mercaptotriethoxysilane, heat to 80℃ and stir for 14h. After stirring, silane-modified polyether is obtained.

[0059] X2. After mixing light calcium carbonate and dioctyl phthalate, heat to dehydrate. Then add silane-modified polyether, (3-aminopropyl)trimethoxysilane, dibutyltin dilaurate, vinyltris(2-methoxyethoxy)silane, and 1,2-benzisothiazolin-3-one and stir for 40 minutes. The mass ratio of silane-modified polyether to light calcium carbonate, dioctyl phthalate, (3-aminopropyl)trimethoxysilane, dibutyltin dilaurate, vinyltris(2-methoxyethoxy)silane, and 1,2-benzisothiazolin-3-one is 10:10:3:0.3:0.02:0.1:0.2. After mixing evenly, discharge to obtain waterproof and mildew-proof sealant.

[0060] Example 1

[0061] A process for reconstructing a durable waterproof layer includes the following steps:

[0062] S1. Locate the leak and treat the cracks;

[0063] S2. Drill holes in the treated surface, penetrating the protective layer, and insert grouting needles. The number of grouting needles is 4 per m. 2 ;

[0064] S3. Inject epoxy acrylate through the grouting needle, with the injection volume based on the injection of this needle, and grout exiting from other pressure relief holes within the corresponding area;

[0065] S4. Inject waterproof and mildew-proof sealant through the grouting needle. The injection volume is based on the injection of this needle, and the grout comes out of other pressure relief holes in the corresponding area.

[0066] S5. Seal the grouting holes and restore the finish to complete the reconstruction of the waterproof layer.

[0067] The preparation method of the waterproof and mildew-proof sealant includes the following steps:

[0068] X1. 6.6 g of 6-fluoro-3-(2-propenyl)-2(3H)-benzothiazoline-5-isocyanate and 7 g of 3-mercaptopropyltriethoxysilane were added to 80 mL of anhydrous ethanol, followed by the addition of 0.1 g of azobisisobutyronitrile. The mixture was heated to 80 °C and stirred for 4 h. After stirring, the mixture was cooled to room temperature and concentrated to dryness under reduced pressure to obtain the modified siloxane.

[0069] X2. Mix 120g of polyether diol and 10g of modified siloxane, heat to 80℃ and stir for 14h. After stirring, silane-modified polyether is obtained.

[0070] X3. Mix light calcium carbonate with dioctyl phthalate and heat to 120°C to dehydrate. Then add silane-modified polyether, (3-aminopropyl)trimethoxysilane, dibutyltin dilaurate, and vinyltris(2-methoxyethoxy)silane and stir for 40 minutes. The mass ratio of silane-modified polyether to light calcium carbonate, dioctyl phthalate, (3-aminopropyl)trimethoxysilane, dibutyltin dilaurate, and vinyltris(2-methoxyethoxy)silane is 10:10:3:0.3:0.02:0.1. After mixing evenly, discharge to obtain waterproof and mildew-proof sealant.

[0071] Example 2

[0072] A process for reconstructing a durable waterproof layer includes the following steps:

[0073] S1. Locate the leak and treat the cracks;

[0074] S2. Drill holes in the treated surface, penetrating the protective layer, and insert grouting needles. The number of grouting needles is 4 per m. 2 ;

[0075] S3. Inject epoxy acrylate through the grouting needle, with the injection volume based on the injection of this needle, and grout exiting from other pressure relief holes within the corresponding area;

[0076] S4. Inject waterproof and mildew-proof sealant through the grouting needle. The injection volume is based on the injection of this needle, and the grout comes out of other pressure relief holes in the corresponding area.

[0077] S5. Seal the grouting holes and restore the finish to complete the reconstruction of the waterproof layer.

[0078] The preparation method of the waterproof and mildew-proof sealant includes the following steps:

[0079] X1. Add 3g of 5-pentene isocyanate and 7g of 3-mercaptopropyltriethoxysilane to 80mL of anhydrous ethanol, then add 0.1g of azobisisobutyronitrile, heat to 80℃ and stir for 4h. After stirring, cool to room temperature and concentrate under reduced pressure to dryness to obtain modified siloxane.

[0080] X2. Mix 120g of polyether diol and 7g of modified siloxane, heat to 80℃ and stir for 14h. After stirring, silane-modified polyether is obtained.

[0081] X3. Mix light calcium carbonate with dioctyl phthalate and heat to 120°C to dehydrate. Then add silane-modified polyether, (3-aminopropyl)trimethoxysilane, dibutyltin dilaurate, and vinyltris(2-methoxyethoxy)silane and stir for 40 minutes. The mass ratio of silane-modified polyether to light calcium carbonate, dioctyl phthalate, (3-aminopropyl)trimethoxysilane, dibutyltin dilaurate, and vinyltris(2-methoxyethoxy)silane is 10:10:3:0.3:0.02:0.1. After mixing evenly, discharge to obtain waterproof and mildew-proof sealant.

[0082] Example 3

[0083] Same as Example 1, except that the mass ratio of silane-modified polyether to light calcium carbonate, dioctyl phthalate, (3-aminopropyl)trimethoxysilane, dibutyltin dilaurate, and vinyltris(2-methoxyethoxy)silane is 10:10:5:0.3:0.02:0.1.

[0084] Example 4

[0085] Same as Example 1, except that the mass ratio of silane-modified polyether to light calcium carbonate, dioctyl phthalate, (3-aminopropyl)trimethoxysilane, dibutyltin dilaurate, and vinyltris(2-methoxyethoxy)silane is 10:10:3:0.5:0.02:0.1.

[0086] Example 5

[0087] Same as Example 1, except that the mass ratio of silane-modified polyether to light calcium carbonate, dioctyl phthalate, (3-aminopropyl)trimethoxysilane, dibutyltin dilaurate, and vinyltris(2-methoxyethoxy)silane is 10:10:3:0.3:0.02:0.2.

[0088] Test Example 1

[0089] The waterproof and mildew-proof sealants prepared in the control example and the embodiment were tested. The water permeability test was conducted under a water pressure of 0.3 MPa for 60 minutes. The peel strength test was performed according to GB / T 7122-1996 "Determination of peel strength of high-strength adhesives - floating roller method".

[0090] Table 1 Performance Test of Waterproof and Mildew-proof Sealants

[0091] Experimental protocol Water resistance Peel strength / N / 10 mm Compare with Example 1 impermeable 17.66 Compare with Example 2 impermeable 17.42 Example 1 impermeable 18.12 Example 2 impermeable 17.56

[0092] The test results show that the sealant prepared in this invention has good adhesive strength and water resistance. This is due to the unique molecular structure of silane-modified polyether, which combines the characteristics of silicone and polyurethane polymers, resulting in excellent mechanical and adhesive properties. Furthermore, its low pollution and environmentally friendly nature, making it harmless to human health, gives it a wider range of applications than other types of sealants.

[0093] Test Example 2

[0094] The antifungal properties of sealants were tested using the accelerated four-week agar plate method, a standard test method for determining the resistance of paint films and related coatings to fungal abrasion, in accordance with ASTM D5590-2010.

[0095] Table 2. Mold Resistance Test of Sealants

[0096] Experimental protocol Anti-mildew grade Compare with Example 1 Level 2 Compare with Example 2 Level 1 Example 1 Level 0 Example 2 Level 2

[0097] By comparing Comparative Examples 1 and 2 with Example 1, it can be found that the addition of anti-mold components has a crucial impact on the anti-mold properties of the sealant. In Comparative Example 1, no modification was made to the siloxane, while in Comparative Example 2, a commercially available anti-mold agent, 1,2-benzisothiazolin-3-one, was added. Therefore, the anti-mold properties of Comparative Example 2 were better than those of Comparative Example 1. However, adding a commercially available anti-mold agent alone can easily cause the component to become ineffective, so the anti-mold performance was ultimately not as good as that of Example 1. In Example 1, a modified siloxane was obtained by mixing 6-fluoro-3-(2-propenyl)-2(3H)-benzothiazoline-5-isocyanate with 3-mercaptopropyltriethoxysilane. This modified siloxane was then reacted with a polyether polyol to obtain a silane-modified polyether sealant. The benzothiazoline heterocycle in the modified siloxane exhibits excellent antibacterial activity, as it can interact with various bacterial targets, thereby inactivating the bacteria. Furthermore, the strong electron-withdrawing groups and halogen atoms on 6-fluoro-3-(2-propenyl)-2(3H)-benzothiazoline-5-isocyanate further enhance the antibacterial activity. Mixing this modified siloxane with 3-mercaptopropyltriethoxysilane to obtain a silane-modified polyether sealant not only provides a waterproof sealant but also offers anti-mildew properties, thus extending its service life and strengthening its waterproof sealing effect. The comparison between Example 1 and Example 2 effectively demonstrates that the anti-mold property mainly comes from the benzothiazole heterocyclic structure. Although the siloxane was also modified in Example 2, the anti-mold effect was significantly worse than that in Example 1.

[0098] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.

Claims

1. A process for reconstructing a durable waterproof layer, characterized in that, Includes the following steps: S1. Locate the leak and treat the cracks; S2. Drill holes in the treated surface to penetrate the protective layer and insert grouting needles; S3. Inject back filler through the grouting needle, with the injection volume based on the injection of this needle, and grout exiting from other pressure relief holes within the corresponding area; S4. Inject waterproof and mildew-proof sealant through the grouting needle. The injection volume is based on the injection of this needle, and the grout comes out of other pressure relief holes in the corresponding area. S5. Seal the grouting holes and restore the finish, thus completing the reconstruction of the waterproof layer; The preparation method of the waterproof and mildew-proof sealant includes the following steps: X1. Add 4-8 parts by weight of 6-fluoro-3-(2-propenyl)-2(3H)-benzothiazoline-5-isocyanate and 4-10 parts by weight of 3-mercaptopropyltriethoxysilane to 50-100 parts by weight of anhydrous ethanol, then add 0.01-0.2 parts by weight of azobisisobutyronitrile, heat to 70-90℃ and stir for 2-5 hours. After stirring, cool to room temperature and concentrate under reduced pressure to dryness to obtain modified siloxane. X2. Mix 100-150 parts by weight of polyether diol and 9-15 parts by weight of modified siloxane, heat to 80-90℃ and stir for 12-16 hours. After stirring, silane-modified polyether is obtained. X3. After mixing the filler and plasticizer, heat to 110~130℃ to dehydrate. Then add silane-modified polyether, silane coupling agent, catalyst, and dehydrating agent and mix for 30~60 minutes. The mass ratio of silane-modified polyether to filler, plasticizer, silane coupling agent, catalyst, and dehydrating agent is 5~15:5~16:1~5:0.1~0.5:0.01~0.04:0.1~0.

2. After mixing evenly, discharge to obtain waterproof and mildew-proof sealant.

2. The process for reconstructing a durable waterproof layer as described in claim 1, characterized in that, The filler is one of light calcium carbonate, nano zinc oxide, or kaolin.

3. The process for reconstructing a durable waterproof layer as described in claim 1, characterized in that, The plasticizer is dioctyl phthalate, the silane coupling agent is (3-aminopropyl)trimethoxysilane, and the catalyst is dibutyltin dilaurate.

4. The process for reconstructing a durable waterproof layer as described in claim 1, characterized in that, The dehydrating agent is vinyltris(2-methoxyethoxy)silane.

Citation Information

Patent Citations

  • Basement structure bottom plate leakage plugging and repairing method

    CN114293602A

  • Composite mildew-proof silane modified polyether sealant and preparation method and application thereof

    CN112480852A

  • Method for reconstructing waterproof layer through minimally invasive technology

    CN112878727A