Method for photocuring additive manufacturing of gradient-graded lithium disilicate glass ceramics
Through light-curing additive manufacturing technology, the 3Y-TZP content and colorant gradient changes are used, combined with flowing deionized water quenching and ion exchange reactions, to solve the problems of light transmittance and color gradient in the preparation of traditional lithium disilicate glass ceramics. Problem, the flexural strength and light transmittance gradient of the crown are realized, and the mechanical properties and aesthetic effects are improved.
Patent Information
- Application Number
- CN202410363038.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-03-28
AI Technical Summary
The traditional preparation method of lithium disilicate glass ceramics cannot effectively simulate the light transmittance and chroma gradient of natural teeth, resulting in poor bionic effect, and the translucency and flexural strength do not meet actual needs, and multiple sinterings lead to changes in the crystal structure Affects color and light transmittance.
Using light-curing additive manufacturing technology, by configuring basic glass powder and carrying out solvent wet mixing, ball milling, granulation, resin mixing, paste making, light-curing molding, degreasing and sintering, the 3Y-TZP content and colorant gradient changes are simulated Semipermeability and color changes, achieving gradual changes in flexural strength and light transmittance, and using flowing deionized water to quench and ion exchange reactions to improve mechanical properties.
It achieves the flexural strength, light transmittance and color gradient effect of the crown, improves the mechanical properties and aesthetic effects, meets individual needs, avoids the dependence on multiple heat treatments and hot pressing equipment, and enhances the bonding strength and Crystal interlocking structure.
Smart Images

Figure CN118270984B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium disilicate glass ceramic preparation, in particular to a method for photocuring additive manufacturing of gradient-graded lithium disilicate glass ceramic. Background Art
[0002] Lithium disilicate glass ceramics have been used clinically as dental restoration materials for many years. Dental restorations include crowns, abutments, inlays, onlays, veneers, facets, bridges and braces. Traditional lithium disilicate glass ceramic preparation methods mostly use a single ratio of raw materials to prepare the blank and then form it. The resulting products have consistent light transmittance and color. However, the light transmittance and color of natural teeth are different in different areas, so the bionic effect of traditional preparation methods is not good.
[0003] In response to this, some improved solutions for preparing lithium disilicate glass ceramics by sintering have emerged. However, there are also some disadvantages, including:
[0004] (1) Multicolor lithium silicate glass ceramics are prepared by introducing lithium silicate glass ceramic powders or suspensions of different colors. Although the color has a gradient effect, its translucency does not change, and the optical effect is not good;
[0005] (2) The closer to the root of a natural tooth, the higher the flexural strength, that is, the flexural strength decreases from the root to the top, and the closer to the top, the higher the translucency. The effect of gradual light transmission can be achieved by controlling the different contents of colorants and the different particle sizes of the powder. Although this method can achieve a gradual change in translucency, it will cause the flexural strength to increase from the root to the top, which is inconsistent with the actual mechanical properties. In addition, during preparation, the glass powders with gradual changes in color and translucency are molded in sequence and formed into blocks by dry pressing, resulting in insufficient bonding strength between layers. In addition, the thickness of each layer is fixed, and it is impossible to achieve a high simulation effect of color and translucency, and it is impossible to meet the personalized needs of color and translucency.
[0006] In addition, when the particles of lithium disilicate glass-ceramics are too large, spherical grains are easily generated during the sintering process, reducing the generation of rod-shaped grains. In this way, a microstructure of interlocking grains cannot be formed, thereby reducing the flexural strength and limiting its application range.
[0007] (3) There are multiple sintering treatments during the preparation process. After multiple sintering, the crystallinity of Li2Si2O5 increases, the needle-shaped lithium disilicate crystals become larger, and fuse into columnar crystals. The particles also become larger spherical crystals. At the same time, the glass phase transforms into the crystal phase, which affects the color and light transmittance of the restoration and reduces the fracture toughness. Summary of the invention
[0008] In view of the shortcomings of the prior art, the present invention provides a method for photocuring additive manufacturing gradient-graded lithium disilicate glass-ceramics, with the aim of making the flexural strength, translucency and color change characteristics of lithium disilicate glass-ceramics consistent with those of natural teeth, thereby enhancing the effect of bionic simulation.
[0009] The technical solution adopted by the present invention is as follows:
[0010] A method for photocuring additive manufacturing of gradient-graded lithium disilicate glass ceramics, comprising:
[0011] S1. Prepare basic glass powder, which includes the following components by mass fraction: 59% to 70% SiO2, 14% to 20% Li2O, 3% to 5% K2O, 1-5% P2O5, 1-3% ZnO and other components, wherein the other components include Al2O3, Na2O, Tb4O7, La2O3, MgO and CaO;
[0012] S2, wet-mixing the basic glass powder with a solvent, ball-milling it uniformly, drying it, heat-treating it into a molten state, and quenching it to form primary particles, wherein the D50 particle size of the primary particles is 0.8 microns;
[0013] Granulating the original particles to obtain lithium disilicate ceramic particles, which include coarse powder and fine powder;
[0014] S3, mixing the photosensitive resin premix, dispersant, and photoinitiator to obtain a resin mixture;
[0015] S4, taking n groups of lithium disilicate ceramic particles and preparing pastes respectively to obtain n groups of pastes, including: adding 3Y-TZP powder, colorant, and the coarse powder to the resin mixture, mixing evenly, then adding the fine powder and mixing evenly, then rolling, and then adding nano-fumed silica to obtain a paste, and vacuum degassing the paste; the particle size of the 3Y-TZP powder is 20-80 nanometers;
[0016] The color and translucency gradient of the n groups of pastes is achieved by using the gradient change of the 3Y-TZP content in the n groups of pastes to simulate the translucency change and the gradient change of the colorant content to simulate the color change, wherein n is greater than 4;
[0017] S5, placing the n groups of pastes in the order of color and translucency gradient into the additive manufacturing device for light-curing forming to obtain a green body, including: using the first group of pastes to solidify to form a first layer, using the second group of pastes to solidify to form a second layer, and so on, until the nth group of pastes is solidified to form an nth layer, and the thickness of each layer is executed according to a preset value;
[0018] S6, washing the green body with flowing liquid, and then drying;
[0019] S7, degreasing and sintering the cleaned and dried green body, including: controlling the oxygen content at 5%-8%, degreasing at 400°C-600°C, obtaining a degreasing sample after a predetermined time, placing the degreasing sample in a 21%-24% lithium polysilicate solution for vacuum impregnation, heating to 500°C in air after a predetermined time, and then evacuating, with the vacuum degree controlled below 10mbar, continuing to heat to 630°C, keeping the temperature for 2 hours, and then heating to 750°C-900°C for sintering, and cooling to room temperature after the predetermined time to obtain a sintered sample;
[0020] S8. Place the sintered sample in a high-pressure vacuum furnace in a nitrate in a flowing state under the action of a stirring device, and heat it to 300-600°C under vacuum conditions, so that the sintered sample is immersed in the molten nitrate to undergo an ion exchange reaction with the molten nitrate. The reaction time is 0.5-2 hours to finally obtain a product; the nitrate is a mixture of sodium nitrate and rubidium nitrate in a mass ratio of 1:1.
[0021] Further technical solutions are:
[0022] When n=6, the mass content of 3Y-TZP in the first to sixth groups of pastes are 15-13%, 13-10%, 10-8%, 8-6%, 6-4%, and 4-2%, respectively, and the mass content of colorant is 0.12%, 0.1%, 0.08%, 0.07%, 0.06%, and 0.04%, respectively.
[0023] The solid contents of the n groups of pastes are consistent.
[0024] In S2, the temperature of the heat treatment is 1400-1600°C;
[0025] The quenching is performed using flowing deionized water, the temperature of the deionized water is 20-25° C., and the flow rate is 1.5-2.5 m / s.
[0026] After granulation, the coarse powder D50 particle size = 20 microns, and the fine powder D50 particle size = 5 microns.
[0027] In the above S7, the degreasing time is 1 to 2 hours, and the sintering time is 2 hours.
[0028] The colorant is CeO2, Fe2O3, Pr6O 11 One or more of the .
[0029] In S3, the photosensitive resin premix includes a monofunctional photosensitive resin monomer, a bifunctional photosensitive resin monomer and a multifunctional photosensitive resin monomer in a mass ratio of 1:1:1 to 1:2:3;
[0030] The monofunctional photosensitive resin monomer includes one or more of hydroxyethyl methacrylate, lauryl acrylate, isobornyl acrylate, phenoxyethyl acrylate, and lauric acid methacrylate;
[0031] The bifunctional photosensitive resin monomer includes one or more of 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, and dipropylene glycol diacrylate;
[0032] The trifunctional photosensitive resin monomer includes propoxylated glycerol triacrylate or ethoxylated trimethylolpropane triacrylate.
[0033] In S3, the mass of the photoinitiator accounts for 0.5% to 2% of the mass of the photosensitive resin premix;
[0034] The photoinitiator includes one or two of diphenyl 2,4,6-trimethylbenzoylphosphine oxide and 1-hydroxycyclohexyl phenyl ketone;
[0035] The mass ratio of diphenyl 2,4,6-trimethylbenzoylphosphine oxide to 1-hydroxycyclohexyl phenyl ketone is 1:1;
[0036] The dispersant includes gamma-methacryloxypropyltrimethoxysilane and gamma-glycidyloxypropyltrimethoxysilane in a mass ratio of 1:1.
[0037] A dental crown prepared according to the method of light-curing additive manufacturing gradient lithium disilicate glass-ceramics, wherein the root flexural strength of the dental crown is 700MPa, the top flexural strength is 350MPa, and the linear transmittance of the top is more than 50%; the flexural strength of the dental crown gradually increases from the top to the root, the transmittance gradually decreases, and the color changes gradually.
[0038] The beneficial effects of the present invention are as follows:
[0039] The method of the present invention utilizes the gradient change of 3Y-TZP content to simulate the change of semi-permeability, and utilizes the gradient change of colorant content to simulate the color change to set multiple groups of lithium disilicate glass ceramic powders with gradual changes in color and semi-permeability, thereby obtaining multiple groups of pastes, wherein the gradient change of 3Y-TZP content is simultaneously used to adjust the flexural strength; and utilizing the characteristics of light-curing additive manufacturing layered molding, different layers are cured and molded using corresponding pastes, and the prepared crown has a decreasing content of 3Y-TZP from the bottom (root) to the top, a decreasing flexural strength, and an increasing semi-permeability, thereby achieving the effect of flexural strength, light transmittance, and chromaticity gradient of the crown, and the optimal flexural strength of the obtained single crown from the root to the top is a gradient of 350MPa to 700MPa. The present invention can be used for the preparation of various dental restorations, is easy to operate, and improves mechanical properties and aesthetic effects.
[0040] The present invention adopts additive manufacturing technology and is formed by stacking layers, so a layered microstructure is naturally formed between the inner surface layers of the crown, which greatly improves the bonding strength of lithium disilicate glass ceramics. In addition, the layer thickness and other parameters are flexibly set, that is, the thickness of each layer is not fixed, and can be adjusted in time according to actual needs, truly achieving the effect of bionic simulation, and fully meeting the personalized needs of color and translucency. In addition, since the solid content of each layer of paste is consistent, the shrinkage rate can be guaranteed to be consistent during the forming process, eliminating the internal stress between the gradient material layers.
[0041] The present invention first prepares the basic glass powder, and then adds 3Y-TZP and colorant when the paste is prepared later. Compared with the traditional method of adding 3Y-TZP when preparing glass powder, the advantages include: adding 3Y-TZP when preparing glass powder. If the amount added is too much, the viscosity of the glass in the molten state will increase, thereby preventing the formation of lithium disilicate and lithium metasilicate. Therefore, the amount of 3Y-TZP added is limited, and the present application adds in subsequent steps so that the amount of 3Y-TZP added is not limited. On the basis of the preparation of the basic powder, 3Y-TZP and colorant can be added as needed according to the number of layers and gradient design to meet personalized customization needs, with high flexibility, avoiding the preparation of glass powder with gradual strength and translucency from the beginning, and the need to reconfigure when replacing and optimizing the design causes waste of raw materials.
[0042] The present invention uses the improvement of the degreasing and sintering process by quenching with flowing deionized water. On the one hand, the heat of the molten mixture is quickly taken away by the flowing water in a short time, which prevents the accumulation of particles formed by quenching, reduces the generation of large particles, and obtains small-sized particles, thereby effectively reducing the particle size after quenching and improving the uniformity of particles, which not only shortens the subsequent ball milling time, but also facilitates the formation of more rod-shaped crystals during subsequent sintering. On the other hand, different temperature rise stages are set to regulate the corresponding degreasing and sintering atmospheres and parameters, avoid cracks and carbon residues, and further promote the generation of rod-shaped crystals. The interlocking structure formed by the rod-shaped grains greatly improves the mechanical properties.
[0043] The present invention obtains lithium disilicate ceramic particles including coarse powder and fine powder by granulating original particles. In the subsequent paste making process, the coarse powder is firstly mixed, and then the gaps between the coarse powders are filled by fine powder, thereby fully improving the density of the paste.
[0044] The method of the present invention has high manufacturing precision, does not require hot pressing, reduces dependence on hot pressing equipment, and avoids the precision loss caused by the lost wax method. It does not require multiple heat treatments, which avoids the reduction of product fracture toughness. The product can be directly obtained without grinding and glazing.
[0045] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 The present invention is a flow chart of the method of the present invention. DETAILED DESCRIPTION
[0047] The specific implementation of the present invention is described below with reference to the accompanying drawings.
[0048] Example 1
[0049] like Figure 1 As shown, a method for photocuring additive manufacturing gradient-graded lithium disilicate glass ceramics in this embodiment includes:
[0050] S1. Prepare basic glass powder, which includes the following components in mass fractions: 59% to 70% SiO2, 14% to 20% Li2O, 3% to 5% K2O, 1-5% P2O5, 1-3% ZnO and other components, wherein the other components include Al2O3, Na2O, Tb4O7, La2O3, MgO, and CaO.
[0051] S2, wet-mixing the basic glass powder with a solvent, ball-milling it uniformly, drying it, heat-treating it into a molten state, and quenching it to form original particles, wherein the D50 particle size of the original particles is 0.8 microns; granulating the original particles to obtain lithium disilicate ceramic particles, which include coarse powder and fine powder;
[0052] Specifically, the basic glass powder is wet-mixed with anhydrous ethanol, ball-milled and mixed uniformly, and then dried, and then heat-treated at 1400-1600° C. to obtain a molten mixture, and the molten mixture is dropped into deionized water with a stable flow state to quench, and original particles are formed in the deionized water, wherein the temperature of the deionized water is 20-25° C. and the flow rate is 1.5-2.5 m / s;
[0053] Specifically, the original particles are ball-milled and sieved to obtain powder with a particle size of D50=0.3-0.5 μm, and then granulated by spray drying. The coarse powder of lithium disilicate ceramic particles obtained by granulation has a particle size of D50=20 μm and the fine powder has a particle size of D50=5 μm.
[0054] S3, mixing the photosensitive resin premix, dispersant, and photoinitiator to obtain a resin mixture;
[0055] Specifically, the photosensitive resin premix includes a monofunctional photosensitive resin monomer, a bifunctional photosensitive resin monomer, and a multifunctional photosensitive resin monomer in a mass ratio of 1:1:1 to 1:2:3;
[0056] The monofunctional photosensitive resin monomer includes one or more of hydroxyethyl methacrylate, lauryl acrylate, isobornyl acrylate, phenoxyethyl acrylate, and lauric acid methacrylate;
[0057] The bifunctional photosensitive resin monomer includes one or more of 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, and dipropylene glycol diacrylate;
[0058] The trifunctional photosensitive resin monomer includes propoxylated glycerol triacrylate or ethoxylated trimethylolpropane triacrylate.
[0059] Specifically, the mass of the photoinitiator accounts for 0.5% to 2% of the mass of the photosensitive resin premix;
[0060] The photoinitiator includes one or both of diphenyl 2,4,6-trimethylbenzoylphosphine oxide and 1-hydroxycyclohexyl phenyl ketone;
[0061] The mass ratio of diphenyl 2,4,6-trimethylbenzoylphosphine oxide to 1-hydroxycyclohexyl phenyl ketone is 1:1.
[0062] Specifically, the dispersant includes γ-methacryloxypropyltrimethoxysilane and γ-glycidyloxypropyltrimethoxysilane in a mass ratio of 1:1.
[0063] S4, taking 6 groups of lithium disilicate ceramic particles and preparing pastes respectively to obtain n groups of pastes, including: adding 3Y-TZP powder, colorant, and the coarse powder to the resin mixture, mixing evenly, then adding the fine powder and mixing evenly, then rolling, and then adding nano-fumed silica to obtain a paste, and vacuum degassing the paste; the particle size of the 3Y-TZP powder is 20-80 nanometers;
[0064] The color and translucency gradient of 6 groups of pastes are achieved by utilizing the gradient change of the 3Y-TZP content in the 6 groups of pastes to simulate the translucency change and the gradient change of the colorant content to simulate the color change. As a specific implementation manner, the content of 3Y-TZP in the first to sixth groups of pastes is 15-13%, 13-10%, 10-8%, 8-6%, 6-4%, and 4-2%, respectively, and the content of the colorant is 0.12%, 0.1%, 0.08%, 0.07%, 0.06%, and 0.04%, respectively.
[0065] Specifically, the coloring agent is CeO2, Fe2O3, Pr6O 11 One or more of the .
[0066] Specifically, coarse powder is added to the resin mixture, dispersed by ball milling, and then fine powder is added, mixed evenly in a homogenizer, and then rolled by a roller press.
[0067] Among them, the solid content of the six groups of pastes is consistent, that is, the proportion of lithium disilicate glass ceramics in each group of pastes is consistent. Specifically, in each group of pastes, the mass of lithium disilicate ceramic particles, 3Y-TZP and colorants accounts for 70% to 85% of the total mass of the paste. The mass of nano-fumed silica accounts for 0.1% to 0.5% of the paste, and the particle size of nano-fumed silica is 7 nanometers.
[0068] The solid content of each group of paste is consistent, which can ensure consistent sintering shrinkage and prevent cracks.
[0069] Among them, those skilled in the art will know that 3Y-TZP refers to a zirconium oxide (ZrO2) ceramic material stabilized by 3 mol% rare earth oxide (usually Y2O3). Compared with traditional zirconium oxide materials, 3Y-TZP has higher stability and toughness and can resist fracture under high stress environments.
[0070] S5, placing 6 groups of pastes in the order of color and translucency gradient into the additive manufacturing equipment for light-curing forming to obtain a green body, including: using the first group of pastes to solidify to form a first layer, using the second group of pastes to solidify to form a second layer, and so on, until the sixth group of pastes is solidified to form a sixth layer, and the thickness of each layer is executed according to a preset value;
[0071] Specifically, the first to sixth groups of pastes are arranged in order of decreasing 3Y-TZP content, and the first to sixth layers formed correspond to the bottom (root) to the top of the crown respectively, thereby ensuring that the flexural strength of the final product from the bottom (root) to the top gradually decreases and the semi-permeability gradually increases.
[0072] S6, washing the green body with flowing liquid and then drying with hot air;
[0073] Specifically, the flowing liquid is composed of resin monomer, polyethylene glycol 200 and isopropyl alcohol in a mass ratio of 1:1:1.
[0074] S7, degreasing and sintering the cleaned and dried green body, including: controlling the oxygen content at 5%-8%, degreasing at 400°C-600°C, obtaining a degreasing sample after a predetermined time, placing the degreasing sample in a 21%-24% lithium polysilicate solution for vacuum impregnation, heating to 500°C in air after a predetermined time, and then evacuating, with the vacuum degree controlled below 10mbar, continuing to heat to 630°C, keeping the temperature for 2 hours, and then heating to 750°C-900°C for sintering, and cooling to room temperature after the predetermined time to obtain a sintered sample;
[0075] Specifically, the degreasing time is 1 to 2 hours, and the sintering time is 2 hours.
[0076] S8. Place the sintered sample in a high-pressure vacuum furnace in a nitrate in a flowing state under the action of a stirring device, and heat it to 300-600°C under vacuum conditions, so that the sintered sample is immersed in the molten nitrate to undergo an ion exchange reaction with the molten nitrate. The reaction time is 0.5-2 hours, and finally a crown product is obtained; the nitrate is a mixture of sodium nitrate and rubidium nitrate in a mass ratio of 1:1.
[0077] Specifically, the sintered sample is placed in an alumina crucible, and then the whole is placed in nitrate in a high-pressure vacuum furnace for heating to obtain the product after the reaction.
[0078] Among them, the purpose of ion exchange is to use large-sized cations (sodium and rubidium ions) to replace small-sized ions (lithium ions) to form a packing effect. Residual compressive stress will be generated on the surface without changing the microstructure, thereby improving the mechanical properties and quality.
[0079] In this embodiment, nitrate is used for ion exchange because it is relatively stable, easy to remove, and will not form insoluble precipitated compounds with the exchanged ions.
[0080] In this embodiment, ion exchange is performed under vacuum conditions, and gas molecules are extracted, thereby increasing the space and rate of ion exchange. This helps to accelerate the diffusion and penetration of ions, that is, increase the migration speed of ions inside the material, thereby shortening the time of ion exchange and improving the exchange efficiency. In addition, nitrate is in a flowing state, further increasing the exchange rate.
[0081] Compared with the time required for ion exchange in a static molten state of nitrate, which is more than 8 hours, the ion exchange under high pressure vacuum conditions in this embodiment can be completed in only 0.5-2 hours.
[0082] The crown produced by the method of this embodiment has a root flexural strength of 700 MPa, a top flexural strength of 350 MPa, and a top linear transmittance of more than 50%. The flexural strength of the crown decreases from the root to the top, the translucency increases, and the color changes gradually.
[0083] Example 2
[0084] The method for photocuring additive manufacturing of gradient-graded lithium disilicate glass ceramics in this embodiment is the same as that in embodiment 1 under the same other conditions and parameters, except that:
[0085] In step S4, 4 groups of lithium disilicate ceramic particles are taken to make pastes respectively to obtain 4 groups of pastes. The contents of 3Y-TZP in the first to fourth groups of pastes are 15-13%, 13-10%, 10-8% and 8-6% respectively, and the content of the colorant is set in a gradient according to actual needs.
[0086] The crown made by this embodiment has a root flexural strength of 700 MPa, a top flexural strength of 420 MPa, and a top light transmittance of 25%. The flexural strength of the crown decreases gradually from the root to the top, the translucency increases gradually, and the color changes gradually.
[0087] Example 3
[0088] The method for photocuring additive manufacturing of gradient-graded lithium disilicate glass ceramics in this embodiment is the same as that in embodiment 1 under the same other conditions and parameters, except that:
[0089] In step S4, three groups of lithium disilicate ceramic particles are taken to prepare pastes respectively to obtain four groups of pastes. The contents of 3Y-TZP in the first to third groups of pastes are 15-13%, 13-10%, and 10-8%, respectively. The content of the colorant is set in a gradient according to actual needs.
[0090] The root strength of the crown made by this embodiment is 700MPa, the top flexural strength is 460MPa, and the top light transmittance is 20%. The flexural strength of the crown decreases from the root to the top, the translucency increases, and the color changes gradually.
[0091] In summary, six layers of bionic simulation effect is better, and six layers are preferred in this application.
[0092] Those skilled in the art can understand that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions recorded in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for photocuring additive manufacturing of gradient-graded lithium disilicate glass ceramics, characterized in that: include: S1. Prepare basic glass powder, which includes the following components by mass fraction: 59% to 70% SiO2, 14% to 20% Li2O, 3% to 5% K2O, 1-5% P2O5, 1-3% ZnO and other components, wherein the other components include Al2O3, Na2O, Tb4O7, La2O3, MgO, and CaO; S2, wet-mixing the basic glass powder with a solvent, ball-milling it uniformly, drying it, heat-treating it into a molten state, and quenching it to form primary particles, wherein the D50 particle size of the primary particles is 0.8 microns; Granulating the original particles to obtain lithium disilicate ceramic particles, which include coarse powder and fine powder; S3, mixing the photosensitive resin premix, dispersant, and photoinitiator to obtain a resin mixture; S4, taking n groups of lithium disilicate ceramic particles and preparing pastes respectively to obtain n groups of pastes, including: adding 3Y-TZP powder, colorant, and the coarse powder to the resin mixture, mixing evenly, then adding the fine powder and mixing evenly, then rolling, and then adding nano-fumed silica to obtain a paste, and vacuum degassing the paste; the particle size of the 3Y-TZP powder is 20-80 nanometers; The color and translucency gradient of the n groups of pastes is achieved by using the gradient change of the 3Y-TZP content in the n groups of pastes to simulate the translucency change and the gradient change of the colorant content to simulate the color change, wherein n is greater than 4; S5, placing the n groups of pastes in the order of color and translucency gradient into the additive manufacturing device for light-curing forming to obtain a green body, including: using the first group of pastes to solidify to form a first layer, using the second group of pastes to solidify to form a second layer, and so on, until the nth group of pastes is solidified to form an nth layer, and the thickness of each layer is executed according to a preset value; S6, washing the green body with flowing liquid, and then drying; S7, degreasing and sintering the cleaned and dried green body, including: controlling the oxygen content at 5%-8%, degreasing at 400°C-600°C for 1-2 hours, obtaining a degreasing sample, placing the degreasing sample in a 21%-24% lithium polysilicate solution for vacuum impregnation, heating to 500°C in air, and then evacuating, with the vacuum degree controlled below 10 mbar, continuing to heat to 630°C, keeping the temperature for 2 hours, and then heating to 750°C-900°C for sintering, with the sintering time being 2 hours, and then cooling to room temperature to obtain a sintered sample; S8, placing the sintered sample in a high-pressure vacuum furnace in a nitrate in a flowing state under the action of a stirring device, heating to 300-600° C. under vacuum conditions, immersing the sintered sample in the molten nitrate to undergo an ion exchange reaction with the molten nitrate, the reaction time being 0.5-2 hours, and finally obtaining a product; the nitrate is a mixture of sodium nitrate and rubidium nitrate in a mass ratio of 1:1; Among the n groups of pastes, when n=6, the mass contents of 3Y-TZP in the first to sixth groups of pastes were 15-13%, 13-10%, 10-8%, 8-6%, 6-4%, and 4-2%, respectively, and the mass contents of colorants were 0.12%, 0.1%, 0.08%, 0.07%, 0.06%, and 0.04%, respectively.
2. The method for photocuring additive manufacturing gradient-graded lithium disilicate glass ceramics according to claim 1, characterized in that: The solid contents of the n groups of pastes are consistent.
3. The method for photocuring additive manufacturing gradient-graded lithium disilicate glass ceramics according to claim 1, characterized in that: In S2, the temperature of the heat treatment is 1400-1600°C; The quenching is performed using flowing deionized water, the temperature of the deionized water is 20-25° C., and the flow rate is 1.5-2.5 m / s.
4. The method for photocuring additive manufacturing gradient-graded lithium disilicate glass ceramics according to claim 1, characterized in that: After granulation, the coarse powder D50 particle size = 20 microns, and the fine powder D50 particle size = 5 microns.
5. The method for photocuring additive manufacturing gradient-graded lithium disilicate glass ceramics according to claim 1, characterized in that: The colorant is CeO2, Fe2O3, Pr6O 11 One or more of the .
6. The method for photocuring additive manufacturing gradient-graded lithium disilicate glass ceramics according to claim 1, characterized in that: In S3, the photosensitive resin premix includes a monofunctional photosensitive resin monomer, a bifunctional photosensitive resin monomer, and a trifunctional photosensitive resin monomer in a mass ratio of 1:1:1 to 1:2:3; The monofunctional photosensitive resin monomer includes one or more of hydroxyethyl methacrylate, lauryl acrylate, isobornyl acrylate, phenoxyethyl acrylate, and lauric acid methacrylate; The bifunctional photosensitive resin monomer includes one or more of 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, and dipropylene glycol diacrylate; The trifunctional photosensitive resin monomer includes propoxylated glycerol triacrylate or ethoxylated trimethylolpropane triacrylate.
7. The method for photocuring additive manufacturing gradient-graded lithium disilicate glass ceramics according to claim 1, characterized in that: In S3, the mass of the photoinitiator accounts for 0.5% to 2% of the mass of the photosensitive resin premix; The photoinitiator includes one or two of diphenyl 2,4,6-trimethylbenzoylphosphine oxide and 1-hydroxycyclohexyl phenyl ketone; The mass ratio of diphenyl 2,4,6-trimethylbenzoylphosphine oxide to 1-hydroxycyclohexyl phenyl ketone is 1:1; The dispersant includes gamma-methacryloxypropyltrimethoxysilane and gamma-glycidyloxypropyltrimethoxysilane in a mass ratio of 1:
1.
8. A dental crown prepared by the method for light-curing additive manufacturing of gradient-graded lithium disilicate glass ceramics according to any one of claims 1 to 7, characterized in that: The root flexural strength of the crown is 700MPa, the top flexural strength is 350MPa, and the linear transmittance of the top is more than 50%; the flexural strength of the crown increases gradually from the top to the root, the transmittance decreases gradually, and the color changes gradually.