A TPEE composite material for automobile interior decoration, preparation method and application thereof

Through the combination of modified TPU resin and TPEE resin, the tensile strength and notched impact strength of TPEE composite materials for automotive interiors are improved, solving the problem of limited performance improvement of existing materials and achieving the dual goals of high performance and environmental protection.

CN118273133BActive Publication Date: 2024-10-22SUZHOU GREENTECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410605228.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-16
Publication Date
2024-10-22
Estimated Expiration
2044-05-16

AI Technical Summary

Technical Problem

Existing TPEE composite materials used in automotive interiors have limited improvements in tensile strength, making it difficult to meet the market's demand for higher performance.

Method used

Modified TPU resin is used, and the TPU resin is treated with maleic anhydride, glycidyl methacrylate and dendritic organic monomers to increase the number of active groups and branches, and is combined with TPEE resin for polymerization to improve the cross-linking of the TPEE skin layer. connection density and overall performance.

Benefits of technology

It significantly improves the peel strength, tensile strength and notched impact strength of TPEE composite materials, meeting the market demand for high performance, while reducing the amount of volatile organic compounds released, achieving the goals of low odor and simple processing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present application relates to the field of TPEE technology, and specifically discloses a TPEE composite material for automotive interior decoration, a preparation method and an application. The TPEE composite material includes a base fabric layer and a TPEE epidermis layer from bottom to top; the TPEE epidermis layer is mainly made of the following raw materials in parts by weight: 60-70 parts of TPEE resin, 10-20 parts of modified TPU resin, 2-5 parts of colorant, and 0.3-0.7 parts of antioxidant; the modified TPU resin is obtained by treating TPU resin with maleic anhydride, glycidyl methacrylate, and branched organic monomers. The TPEE composite material not only has the characteristics of low odor and simple processing technology, but also has the advantages of high peel strength, high tensile strength, and high notched impact strength, and has broad market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of artificial leather, and more specifically, to a TPEE composite material for automobile interior decoration, a preparation method and an application thereof. Background Art

[0002] With the continuous progress and development of society, the demand of OEMs for automotive interior materials must meet both mechanical performance requirements and environmental protection concepts. Among them, thermoplastic polyester elastomers have been accepted and recognized by the market due to their advantages of high compression bending modulus, excellent wear resistance, good high and low temperature stability, and good chemical stability, and are widely used in automotive interior materials. The TPEE composite material for automotive interior in the related technology includes a base fabric layer and a TPEE skin layer from bottom to top. The TPEE skin layer is a thermoplastic polyurethane skin layer, and its raw material is mainly TPEE resin. With the use of colorants, the TPEE skin layer has low odor and beautiful color. In order to make the TPEE skin layer have higher tensile strength and flexibility, some researchers directly add TPU resin to TPEE resin. Although it can enhance the tensile strength, the improvement of tensile strength is limited and needs to be further improved. Summary of the invention

[0003] In order to improve the tensile strength of TPEE composite materials, the present application provides a TPEE composite material for automotive interior, a preparation method and an application thereof.

[0004] In the first aspect, the present application provides a TPEE composite material for automotive interior, which adopts the following technical solution:

[0005] A TPEE composite material for automobile interior decoration, comprising a base fabric layer and a TPEE skin layer from bottom to top; the TPEE skin layer is mainly made of the following raw materials in parts by weight: 60-70 parts of TPEE resin, 10-20 parts of modified TPU resin, 2-5 parts of colorant, and 0.3-0.7 parts of antioxidant; the modified TPU resin is obtained by treating TPU resin with maleic anhydride, glycidyl methacrylate, and a branched organic monomer.

[0006] The TPEE composite material of this application has a total volatile organic compound emission of <100 μg / m 3 , with low volatile organic compound emission, meeting the requirements of safety and low odor. Moreover, peel strength>70N / 3cm, tensile strength>55MPa, -30℃ notched impact strength>100KJ / m 2 , it has the advantages of high peel strength, high tensile strength and high notched impact strength, meeting market demand.

[0007] Among the raw materials of the TPEE skin layer, TPEE resin is the main component, and the modified TPU resin is used to not only give TPEE excellent performance, but also reduce the surface treatment process and simplify the process. TPU resin is treated with maleic anhydride, glycidyl methacrylate, and branched organic monomers, and a large number of active groups are introduced on the surface of TPU resin, and the number of branches is increased, which can not only react with the unsaturated groups of TPEE resin, but also can polymerize with each other, increase the crosslinking density and integrity of the TPEE skin layer, improve the peel strength, tensile strength and notched impact strength, and make the TPEE composite material show better comprehensive performance.

[0008] Optionally, the modified TPU resin is prepared by the following method:

[0009] T1. Add maleic anhydride to the organic solvent under constant stirring, and then dropwise add the diethylenetriamine dilution. The diethylenetriamine dilution is added for 0.5-1.5 hours. After the addition is complete, continue stirring for 3-5 hours, and perform vacuum distillation to obtain an organic monomer.

[0010] T2. Add pentamethylenediamine to water at a temperature of 80-90° C. and stir continuously, then add organic monomer for the first time and stir for 5-7 hours, add organic monomer for the second time and stir for 5-7 hours, add organic monomer for the third time and stir for 5-7 hours, add organic monomer for the fourth time and stir for 5-7 hours, and perform reduced pressure distillation to obtain branched organic monomer;

[0011] T3. Mix TPU resin, maleic anhydride, glycidyl methacrylate and branched organic monomer, then melt and granulate to obtain modified TPU resin.

[0012] By adopting the above technical scheme, maleic anhydride contains anhydride groups and carbon-carbon double bonds, and diethylenetriamine contains one secondary amine group and two primary amine groups. When the two are mixed, the anhydride groups react with the secondary amine groups first. At this time, an excess of maleic anhydride is added, and the diethylenetriamine is diluted to obtain a diethylenetriamine dilution liquid, and the diethylenetriamine dilution liquid is added dropwise to make the anhydride groups react only with the primary amine groups to obtain an organic monomer. The organic monomer contains a carbon-carbon double bond and also has a branched chain, one chain end is a carboxyl group, and the remaining two chain ends are both primary amine groups.

[0013] The first organic monomer is added to pentamethylenediamine. Pentamethylenediamine contains two primary amine groups, which can react with the carboxyl groups in the two organic monomers respectively. Pentamethylenediamine is used as the core to increase the amount of branches and carbon-carbon double bonds, and introduce primary amine groups. Then, the organic monomer is added for the second time, the third time, and the fourth time, and the organic monomer is added continuously to react and form a branched organic monomer. The branched organic monomer contains more carbon-carbon double bonds and branches.

[0014] TPU resin, maleic anhydride, glycidyl methacrylate and branched organic monomers are mixed to achieve grafting of TPU resin. At the same time, polymerization reaction can be promoted between maleic anhydride, glycidyl methacrylate and branched organic monomers at high temperature to increase the amount of branches and compatibility, improve the use effect of modified TPU resin, increase the crosslinking density and integrity of the TPEE epidermis, and show better peel strength, tensile strength and notched impact strength.

[0015] Optionally, the weight ratio of the organic solvent, maleic anhydride, and diethylenetriamine diluent is (20-30):(4-5):(19-23); the diethylenetriamine diluent is a mixture of diethylenetriamine and 1,4-dioxane, and the weight ratio of diethylenetriamine and 1,4-dioxane is (3-4):(15-20); the weight ratio of pentamethylenediamine, the first organic monomer added, the second organic monomer added, the third organic monomer added, and the fourth organic monomer added is (0.5-1.5):(2-6):(5-10):(10-20):(20-40).

[0016] By adopting the above technical solution, the weight ratio of maleic anhydride and diethylenetriamine diluent is optimized, the addition amount of maleic anhydride and diethylenetriamine is controlled, and the maleic anhydride is excessive, which is convenient for the preparation and control of organic monomers. The weight ratio of pentamethylenediamine, the first addition of organic monomers, the second addition of organic monomers, the third addition of organic monomers, and the fourth addition of organic monomers is also optimized. With pentamethylenediamine as the core, the reaction is gradually carried out in steps to increase the amount of branches, which is convenient for the preparation and control of branched organic monomers.

[0017] Optionally, the weight ratio of the TPU resin, maleic anhydride, glycidyl methacrylate and branched organic monomer is (90-110):(9-11):(9-11):(1-3).

[0018] By adopting the above technical scheme, the weight ratio of TPU resin, maleic anhydride, glycidyl methacrylate and branched organic monomer is optimized, which is convenient for the grafting and polymerization reaction of maleic anhydride, glycidyl methacrylate and branched organic monomer. When it is within the above range, the modified TPU resin can have a good use effect, enhance the peel strength, tensile strength and notched impact strength, and make the TPEE composite material show better performance.

[0019] Optionally, the organic solvent is one or more of 1,4-dioxane, carbon tetrachloride, NN-dimethylformamide, and xylene.

[0020] By adopting the above technical solution, the organic solvent is optimized, which is convenient for the selection of the organic solvent. Moreover, the organic solvent can make maleic anhydride and diethylenetriamine contact and react, which is convenient for the preparation of the organic monomer.

[0021] Optionally, in step T3, the melting temperature is 160-180°C.

[0022] By adopting the above technical solution, the melting temperature is limited, the TPU resin is fully melted, and the TPU resin, maleic anhydride, glycidyl methacrylate, and branched organic monomer are fully contacted to achieve grafting, which is convenient for the preparation of modified TPU resin and also ensures the quality and use effect of the modified TPU resin. In multiple embodiments, in step T3, the melting temperature is 180°C, and the temperature can also be set to 160°C, 165°C, 170°C, 175°C, etc. as needed.

[0023] Optionally, the hardness of the TPEE resin is 40-70D; the hardness of the TPU resin is 70-90D.

[0024] By adopting the above technical solution, TPEE resin and TPU resin are optimized, which not only facilitates the selection of TPEE resin and TPU resin, but also ensures the performance of TPEE composite materials, so that it can show better use effect. In multiple embodiments, the hardness of TPEE resin is 55D, and the hardness can also be set to 40D, 45D, 50D, 60D, 65D, 70D, etc. as needed. In multiple embodiments, the hardness of TPU resin is 80D, and the hardness can also be set to 70D, 75D, 85D, 90D, etc. as needed.

[0025] Optionally, the antioxidant is one or more of antioxidant 1010, antioxidant 2246, antioxidant T501, antioxidant BHT, and antioxidant TNPP.

[0026] By adopting the above technical solution, the antioxidant is optimized, which facilitates the selection of the antioxidant. Moreover, the antioxidant can effectively reduce the aging of the TPEE composite material due to oxidation during processing and use, improve durability and extend service life. Further, the antioxidant is an antioxidant 1010 and an antioxidant TNPP, and the weight ratio of the antioxidant 1010 and the antioxidant TNPP is (1-3): (1-3). In multiple embodiments, the weight ratio of the antioxidant 1010 and the antioxidant TNPP is 3:1, and the weight ratio can also be set to 1:1, 1:2, 1:3, 2:1, 2:3, 3:2, etc. as needed.

[0027] Further, the thickness of the TPEE skin layer is 0.2-1 mm. Preferably, the thickness of the TPEE skin layer is 0.4-0.5 mm. In multiple embodiments, the thickness of the TPEE skin layer is 0.45 mm, and the thickness can also be set to 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, etc. as needed.

[0028] Furthermore, the colorant is a masterbatch, and the masterbatch is one or more of TPU masterbatch and TPEE masterbatch. The color of the masterbatch is one of black, gray, yellow, orange, brown, red, dark red, green, cyan, blue, purple, and white.

[0029] Furthermore, the base fabric layer is a polyethylene terephthalate synthetic fiber fabric. The weight of the base fabric layer is 200-300 g / m 2 , thickness is 0.6-1mm. Preferably, the weight of the base fabric layer is 230-280g / m 2 , thickness is 0.7-0.8mm. More preferably, the weight of the base fabric layer is 250g / m 2 , thickness is 0.75mm.

[0030] In the second aspect, the present application provides a method for preparing the TPEE composite material for automotive interior, which adopts the following technical solution:

[0031] A method for preparing the TPEE composite material for automobile interior comprises the following steps:

[0032] S1, mixing TPEE resin, modified TPU resin, colorant and antioxidant to obtain a mixture;

[0033] S2, melting the mixture at a temperature of 170-200° C. to obtain a molten mixture;

[0034] S3. Coat the molten mixture on the surface of the release paper, then place the base fabric layer, and at a pressure of 0.4-1MPa, make the base fabric layer and the molten mixture fit together to form a three-layer structure. Cool down, and the molten mixture solidifies to form a TPEE skin layer. Tear off the release paper to obtain a TPEE composite material.

[0035] By adopting the above technical scheme, the raw materials are mixed, and then melted to obtain a molten mixture, which is then coated on a release paper and attached to a base fabric layer to form a three-layer structure. The temperature is lowered to achieve bonding to obtain a TPEE composite material, which facilitates the preparation of a TP44 composite material.

[0036] In various embodiments, in step S2, the melting temperature is 200°C, and the melting temperature can also be set to 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, etc. as needed. In various embodiments, in step S3, the pressure is 0.5MPa, and the pressure can also be set to 0.4MPa, 0.6MPa, 0.7MPa, 0.8MPa, 0.9MPa, 1MPa, etc. as needed.

[0037] In a third aspect, the present application provides an automotive interior, which adopts the following technical solution:

[0038] An automobile interior is made by using the TPEE composite material for automobile interior.

[0039] In summary, this application has at least the following beneficial effects:

[0040] 1. The TPEE composite material of the present application not only has the characteristics of low odor and simple processing technology, but also has peel strength>70N / 3cm, tensile strength>55MPa, -30℃ notched impact strength>100KJ / m 2 It has the advantages of high peel strength, high tensile strength and high notch impact strength, and has broad market prospects.

[0041] 2. In the preparation method of the modified TPU resin of the present application, an organic monomer is first obtained by the reaction between maleic anhydride and diethylenetriamine. The organic monomer contains a carbon-carbon double bond and has a branched chain, one chain end is a carboxyl group, and the remaining two chain ends are primary amine groups. Then, with pentamethylenediamine as the core, the organic monomer is added step by step and reacted, the amount of branching and carbon-carbon double bonds is continuously increased, and a branched organic monomer is obtained. After that, the TPU resin is modified using maleic anhydride, glycidyl methacrylate, and branched organic monomers, which not only facilitates the preparation of the TPU resin, but also increases the use effect of the TPU resin, improves the peel strength, tensile strength, and notched impact strength, and makes the TPEE composite material show better performance. DETAILED DESCRIPTION

[0042] In order to make the present application easier to understand, the present application will be further described in detail below in conjunction with the examples, which are merely illustrative and are not intended to limit the scope of application of the present application. The raw materials or components used in the present application can be obtained through commercial routes or conventional methods unless otherwise specified.

[0043] Preparation Example

[0044] Preparation Example 1

[0045] A modified TPU resin is prepared by the following method:

[0046] T1. Add 90 g of maleic anhydride to 500 g of organic solvent at a rotation speed of 2000 r / min and stir for 2 min. Then add 420 g of diethylenetriamine dilution dropwise for 1 h. After the addition is complete, continue stirring for 4 h. Remove the organic solvent and excess maleic anhydride by vacuum distillation to obtain an organic monomer.

[0047] The organic solvent is 1,4-dioxane; the diethylenetriamine diluent is a mixed solution of diethylenetriamine and 1,4-dioxane, and the weight ratio of diethylenetriamine to 1,4-dioxane is 1:5.

[0048] T2. At a temperature of 85°C and a rotation speed of 1000r / min, add 1g of pentamethylenediamine to 1000g of water and stir for 2min. Then add 3.9g of organic monomer for the first time and stir for 6h. Add 7.9g of organic monomer for the second time and stir for 6h. Add 15.8g of organic monomer for the third time and stir for 6h. Add 31.5g of organic monomer for the fourth time and stir for 6h. Remove water by distillation under reduced pressure to obtain a branched organic monomer.

[0049] T3. Add 10 g of maleic anhydride, 10 g of glycidyl methacrylate and 2 g of branched organic monomer to 100 g of TPU resin, stir for 5 min, melt at 180° C., and granulate to obtain modified TPU resin.

[0050] The hardness of the TPU resin is 80D, and it is selected from TPU WHT-8280H of Yantai Wanhua.

[0051] Preparation Example 2

[0052] A modified TPU resin is prepared by the following method:

[0053] T1. Add 80 g of maleic anhydride to 400 g of organic solvent at a rotation speed of 2000 r / min and stir for 2 min. Then add 460 g of diethylenetriamine dilution dropwise for 1.5 h. After the addition is complete, continue stirring for 3 h. Remove the organic solvent and excess maleic anhydride by vacuum distillation to obtain an organic monomer.

[0054] The organic solvent is 1,4-dioxane; the diethylenetriamine diluent is a mixture of diethylenetriamine and 1,4-dioxane, and the weight ratio of diethylenetriamine to 1,4-dioxane is 3:20.

[0055] T2. At a temperature of 80°C and a rotation speed of 1000 r / min, add 0.5 g of pentamethylenediamine to 800 g of water and stir for 2 min. Then add 2 g of organic monomer for the first time and stir for 5 h. Add 10 g of organic monomer for the second time and stir for 7 h. Add 20 g of organic monomer for the third time and stir for 7 h. Add 20 g of organic monomer for the fourth time and stir for 5 h. Remove water by distillation under reduced pressure to obtain a branched organic monomer.

[0056] T3. Add 9g of maleic anhydride, 11g of glycidyl methacrylate and 1g of branched organic monomer to 90g of TPU resin, stir for 5min, melt at 180°C, and granulate to obtain modified TPU resin.

[0057] The hardness of the TPU resin is 80D, and it is selected from TPU WHT-8280H of Yantai Wanhua.

[0058] Preparation Example 3

[0059] A modified TPU resin is prepared by the following method:

[0060] T1. Add 100 g of maleic anhydride to 600 g of organic solvent at a rotation speed of 2000 r / min and stir for 2 min. Then add 380 g of diethylenetriamine dilution dropwise for 0.5 h. After the addition is complete, continue stirring for 5 h. Remove the organic solvent and excess maleic anhydride by vacuum distillation to obtain an organic monomer.

[0061] The organic solvent is 1,4-dioxane; the diethylenetriamine diluent is a mixed solution of diethylenetriamine and 1,4-dioxane, and the weight ratio of diethylenetriamine to 1,4-dioxane is 4:15.

[0062] T2. At a temperature of 90°C and a rotation speed of 1000r / min, add 1.5g of pentamethylenediamine to 1200g of water and stir for 2min. Then add 6g of organic monomer for the first time and stir for 7h. Add 5g of organic monomer for the second time and stir for 5h. Add 10g of organic monomer for the third time and stir for 5h. Add 40g of organic monomer for the fourth time and stir for 7h. Remove water by distillation under reduced pressure to obtain a branched organic monomer.

[0063] T3. Add 11 g of maleic anhydride, 9 g of glycidyl methacrylate and 3 g of branched organic monomer to 110 g of TPU resin, stir for 5 min, melt at 180° C., and granulate to obtain modified TPU resin.

[0064] The hardness of the TPU resin is 80D, and it is selected from TPU WHT-8280H of Yantai Wanhua. Example

[0065] Table 1 Raw material dosage of TPEE composite materials (unit: ×10g)

[0066]

[0067] Example 1

[0068] A TPEE composite material for automobile interior, comprising a base fabric layer and a TPEE skin layer from bottom to top. The base fabric layer is a polyethylene terephthalate synthetic fiber fabric, and the weight of the base fabric layer is 250g / m 2 The thickness is 0.75mm. The thickness of the TPEE skin layer is 0.45mm. The raw materials and raw material ratios of the TPEE skin layer are shown in Table 1.

[0069] Among them, the hardness of TPEE resin is 55D, and it is selected from TPEE 5526 of DuPont of the United States; the colorant is a masterbatch, the masterbatch is a black TPU masterbatch, and it is selected from Shenzhen Chenmei Pigment Colorant Co., Ltd.; the antioxidants are antioxidant 1010 and antioxidant TNPP, and the weight ratio of antioxidant 1010 and antioxidant TNPP is 3:1; the modified TPU resin is prepared by the method of Preparation Example 1.

[0070] A method for preparing a TPEE composite material for automobile interior, comprising the following steps:

[0071] S1. Add modified TPU resin, colorant and antioxidant into TPEE resin at a rotation speed of 500 r / min, stir for 3 min, and obtain a mixture.

[0072] S2. Melting the mixture at a temperature of 200° C. to obtain a molten mixture.

[0073] S3. Coat the molten mixture on the surface of the release paper, then place the base fabric layer, and at a pressure of 0.5 MPa, make the base fabric layer and the molten mixture fit together to form a three-layer structure. Cool down to 23°C, and the molten mixture solidifies to form a TPEE surface layer. Tear off the release paper to obtain a TPEE composite material.

[0074] Example 2

[0075] A TPEE composite material for automobile interior, which differs from Example 1 in that the raw material ratio of the TPEE surface layer is different, and the raw material ratio is shown in Table 1.

[0076] Example 3

[0077] A TPEE composite material for automobile interior, which differs from Example 1 in that the raw material ratio of the TPEE surface layer is different, and the raw material ratio is shown in Table 1.

[0078] Example 4

[0079] A TPEE composite material for automobile interior, which differs from Example 1 in that the source of the modified TPU resin in the raw materials of the TPEE skin layer is different, and the modified TPU resin is prepared by the method of Preparation Example 2.

[0080] Example 5

[0081] A TPEE composite material for automobile interior, which differs from Example 1 in that the source of the modified TPU resin in the raw materials of the TPEE skin layer is different, and the modified TPU resin is prepared by the method of Preparation Example 3.

[0082] Comparative Example

[0083] Comparative Example 1

[0084] A TPEE composite material for automobile interior, which differs from Example 1 in that an equal amount of TPEE resin is used to replace the modified TPU resin in the raw material of the TPEE skin layer.

[0085] Comparative Example 2

[0086] A TPEE composite material for automobile interior, which differs from Example 1 in that an equal amount of TPU resin is used to replace the modified TPU resin in the raw material of the TPEE surface layer.

[0087] Comparative Example 3

[0088] A TPEE composite material for automobile interior, which differs from Example 1 in that, in the preparation method of the modified TPU resin of the TPEE skin layer, glycidyl methacrylate and branched organic monomer are replaced by an equal amount of maleic anhydride.

[0089] Comparative Example 4

[0090] A TPEE composite material for automobile interior decoration, which differs from Example 1 in that in the preparation method of the modified TPU resin of the TPEE skin layer, the maleic anhydride and the branched organic monomer are replaced by an equal amount of glycidyl methacrylate.

[0091] Comparative Example 5

[0092] A TPEE composite material for automobile interior decoration, which differs from Example 1 in that in the preparation method of the modified TPU resin of the TPEE skin layer, maleic anhydride and glycidyl methacrylate are replaced by an equal amount of branched organic monomers.

[0093] Performance Testing

[0094] The TPEE composite materials obtained in Examples 1-5 and Comparative Examples 1-5 were taken as samples, and the following performance tests were performed on the samples. The test results are shown in Table 2.

[0095] Among them, the peel strength of the sample was tested according to QB / T4194-2011; the tensile strength of the sample was tested according to ISO527-2; the notched impact strength of the sample was tested according to ISO179 / 1eA; the C 6 -C 16 The total volatile organic compound emission was tested.

[0096] Table 2

[0097]

[0098] As can be seen from Table 2, the TPEE composite material of the present application has a peel strength of 70.3-73.2N / 3cm, which is relatively high. Moreover, its tensile strength is 55.9-58.6MPa, and its -30℃ notched impact strength is 109.5-113.6KJ / m 2 It has the advantages of high tensile strength and high notched impact strength. At the same time, the total volatile organic compound emission is less than 100μg / m 3 , the emission of volatile organic compounds is low, meeting the needs of safety and low odor.

[0099] Comparing Comparative Example 1 with Comparative Example 2, the raw material of the TPEE skin layer of Comparative Example 1 uses TPEE resin, while the raw materials of the TPEE skin layer of Comparative Example 2 use TPEE resin and TPU resin. It can be seen that adding TPU resin to TPEE resin can improve peel strength, tensile strength and notched impact strength.

[0100] Comparing Example 1 with Comparative Examples 3-5, the raw material of the TPEE skin layer of Comparative Example 3 uses maleic anhydride to modify the TPU resin; the raw material of the TPEE skin layer of Comparative Example 4 uses glycidyl methacrylate to modify the TPU resin; the raw material of the TPEE skin layer of Comparative Example 5 uses a dendritic organic monomer to modify the TPU resin; the raw material of the TPEE skin layer of Example 1 uses maleic anhydride, glycidyl methacrylate, and dendritic organic monomer to modify the TPU resin. It can be seen that by modifying the TPU resin with maleic anhydride, glycidyl methacrylate, and dendritic organic monomers, active groups and branching amount are introduced on the surface of the TPU, the compatibility and integrity are increased, and the TPEE composite material exhibits better comprehensive performance.

[0101] It should be noted that the embodiments described above are only used to explain the present application and do not constitute any limitation to the present application. The present application is described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present application may be modified as specified within the scope of the claims of the present application, and the present invention may be revised without departing from the scope and spirit of the present application. Although the present application described therein relates to specific methods, materials and embodiments, it does not mean that the present application is limited to the specific examples disclosed therein. On the contrary, the present application can be extended to all other methods and applications with the same functions.

Claims

1. A TPEE composite material for automotive interior, characterized in that: It includes a base fabric layer and a TPEE skin layer from bottom to top; the TPEE skin layer is mainly made of the following raw materials in parts by weight: 60-70 parts of TPEE resin, 10-20 parts of modified TPU resin, 2-5 parts of colorant, and 0.3-0.7 parts of antioxidant; the modified TPU resin is obtained by treating TPU resin with maleic anhydride, glycidyl methacrylate, and branched organic monomers; The modified TPU resin is prepared by the following method: T1. Add maleic anhydride to the organic solvent under constant stirring, and then dropwise add the diethylenetriamine dilution. The diethylenetriamine dilution is added for 0.5-1.5 hours. After the addition is complete, continue stirring for 3-5 hours, and perform vacuum distillation to obtain an organic monomer. T2. Add pentamethylenediamine to water at a temperature of 80-90° C. and stir continuously, then add organic monomer for the first time and stir for 5-7 hours, add organic monomer for the second time and stir for 5-7 hours, add organic monomer for the third time and stir for 5-7 hours, add organic monomer for the fourth time and stir for 5-7 hours, and perform reduced pressure distillation to obtain branched organic monomer; T3, mixing TPU resin, maleic anhydride, glycidyl methacrylate, and branched organic monomer, and then melting and granulating to obtain modified TPU resin; The weight ratio of the organic solvent, maleic anhydride, and diethylenetriamine diluent is (20-30):(4-5):(19-23); the diethylenetriamine diluent is a mixed solution of diethylenetriamine and 1,4-dioxane, and the weight ratio of diethylenetriamine and 1,4-dioxane is (3-4):(15-20); the weight ratio of pentamethylenediamine, the first organic monomer, the second organic monomer, the third organic monomer, and the fourth organic monomer is (0.5-1.5):(2-6):(5-10):(10-20):(20-40); The weight ratio of the TPU resin, maleic anhydride, glycidyl methacrylate and branched organic monomer is (90-110):(9-11):(9-11):(1-3).

2. The TPEE composite material for automotive interior according to claim 1, characterized in that: The organic solvent is one or more of 1,4-dioxane, carbon tetrachloride, NN-dimethylamide and xylene.

3. The TPEE composite material for automobile interior according to claim 1, characterized in that: In step T3, the melting temperature is 160-180°C.

4. The TPEE composite material for automobile interior according to claim 1, characterized in that: The hardness of the TPEE resin is 40-70D; the hardness of the TPU resin is 70-90D.

5. The TPEE composite material for automobile interior according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1010, antioxidant 2246, antioxidant T501, antioxidant BHT, and antioxidant TNPP.

6. A method for preparing a TPEE composite material for automotive interior according to any one of claims 1 to 5, characterized in that: The steps include: S1, mixing TPEE resin, modified TPU resin, colorant and antioxidant to obtain a mixture; S2, melting the mixture at a temperature of 170-200° C. to obtain a molten mixture; S3. Coat the molten mixture on the surface of the release paper, then place the base fabric layer, and at a pressure of 0.4-1MPa, make the base fabric layer and the molten mixture fit together to form a three-layer structure. Cool down, and the molten mixture solidifies to form a TPEE skin layer. Tear off the release paper to obtain a TPEE composite material.

7. An automobile interior, characterized in that: The invention is made of the TPEE composite material for automobile interior decoration as claimed in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Branched polyacrylamide and preparation method thereof

    CN102675535A

  • Water-based polyurethane coating and graphene oxide composite coating interface hyperbranched polyamide adhering method

    CN108727962A

  • Automobile lightweight interior material and preparation method thereof

    CN117048160A

  • Thermoplastic polyurethane elastomer composition and laminate using same composition

    JP2004331899A

  • Oligomer or polymer, composition, use of the oligomer or polymer and intermediate

    US20220340717A1