A post-forging heat treatment process for SUP13Cr / 1 material
By combining annealing, continuous tempering, and high-temperature tempering heat treatment processes, the problems of uneven internal structure and grain size of SUP13Cr/1 material forging billets were solved, achieving high-quality production of forgings and improving delivery rate.
Patent Information
- Application Number
- CN202410436695.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-11
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-04-11
AI Technical Summary
The existing post-forging heat treatment process for SUP13Cr/1 material is difficult to achieve uniform microstructure and refined grain size, resulting in uneven internal microstructure of the forging billet, easy cracking, affecting quality and delivery rate, especially for large-size forgings.
A combined heat treatment process of annealing, continuous tempering and high-temperature tempering is adopted. By controlling the temperature of the heating furnace and the cooling rate, uniform cooling and heat preservation of the forging billet at different stages are ensured, structural stress is eliminated, and the formation of white spots and network structure is avoided.
This process achieves uniformity of internal structure and refinement of grain size in the forging billet, eliminates structural stress, prevents forging billet cracking, and improves the quality and delivery rate of forgings.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of heat treatment technology for metallic materials, and specifically relates to a post-forging heat treatment process for SUP13Cr / 1 material that not only improves the internal structure of forging billets and ensures uniform quality, but also increases the delivery rate of forging billets. Background Technology
[0002] SUP13Cr / 1 is a martensitic stainless steel, offering superior mechanical properties and corrosion resistance compared to 13Cr. It is particularly suitable for use in harsh environments and is primarily applied in offshore oil projects, OTG pipelines, shell systems, and downhole projects. This material contains 12.0%–13.0% Cr and 0.15% Si. The SUP13Cr / 1 material has a high alloy content, with Mn content between 0.30% and 0.50%, Ni content between 5.0% and 5.5%, Mo content between 1.8% and 2.0%, and V content between 0.06% and 0.09%. Due to this high alloy content, improper control of the post-forging heat treatment process during production can easily lead to network structures, uneven microstructure, uneven grain size, and cracking caused by internal stress processes in the forging billet. This affects product quality and makes delivery impossible, especially for diameters in the φ200~φ400mm range and lengths greater than 2... The impact is more pronounced on large-diameter SUP13Cr / 1 forgings with an outer diameter of φ200~φ400mm. Production using the conventional annealing heat treatment process of martensitic steel (φ200~φ400mm) makes it difficult to achieve uniform microstructure and refine grain size. Excessive microstructure stress can easily cause forging cracks and produce scrap. Furthermore, the excessively high surface hardness after annealing makes rough machining difficult, affecting delivery schedules and sales revenue. Therefore, for SUP13Cr / 1 forgings with an outer diameter in the range of φ200~φ400mm, there is an urgent need for a heat treatment process that can effectively improve the network microstructure, refine the grain size, and enhance the overall quality of the forgings. Summary of the Invention
[0003] The purpose of this invention is to overcome the shortcomings of the prior art and provide a post-forging heat treatment process for SUP13Cr / 1 material, which effectively improves the internal structure of the forging billet, ensures uniform quality, and increases the delivery rate of the forging billet.
[0004] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: a post-forging heat treatment process for SUP13Cr / 1 material, the specific heat treatment process being as follows: Step 1) Annealing: When loading the furnace, the furnace temperature is controlled at 600℃~700℃ for waiting. Then, the temperature is increased to 880℃~910℃ at a rate of 10℃ / h~100℃ / h and held for 5h~30h. After holding, the billet is removed from the furnace and air-cooled until the surface temperature of the forging billet is 100℃~150℃. The temperature measurement point is based on the highest temperature. During air cooling, the billet is rotated 180 degrees every half hour to ensure uniform air cooling. Then, the forging billet is loaded into the heating furnace. After completing Step 1), continuous tempering is prepared. Step 2) Continuous tempering: The forging billet is placed in a heating furnace at a temperature of 100℃~150℃ and held for 2h~10h. Then, the temperature is increased to 660℃~700℃ at a heating rate of 5℃ / h~80℃ / h and held for a holding time of (7~10)*R / 100h, where R is the diameter of the forging billet. Then, the temperature is decreased at a cooling rate of 5℃ / h~30℃ / h and cooled in the furnace to a heating furnace temperature of 280℃~300℃. Then, the billet is removed from the furnace and air-cooled to room temperature. The forging billet is then placed back into the heating furnace. After completing Step 2), high-temperature tempering is to be performed. Step 3) High-temperature tempering: The forging billet is placed in a heating furnace with a furnace temperature ≤450℃, and then heated to 620℃~660℃ at a heating rate of 5℃ / h~80℃ / h. The holding time is (5~8)*R / 100h, where R is the diameter of the forging billet. Then, the billet is removed from the furnace and air-cooled until the surface temperature of the forging billet reaches 100℃~400℃ for hot straightening. After hot straightening, it is air-cooled to room temperature.
[0005] Compared with the prior art, the process of this invention has the following advantages: 1. Annealing followed by continuous tempering can not only refine the grain size and make the microstructure more uniform, but also eliminate the microstructure stress generated during the annealing process.
[0006] 2. SUP13Cr / 1 material has a high Ni content, so it is highly sensitive to white spots. This invention can remove hydrogen to a certain extent and avoid the formation of white spots.
[0007] 3. It can avoid the formation of bainitic structure that is prone to grain inheritance, and effectively solve the problems of uneven grain size and the formation of network structure.
[0008] 4. It can effectively soften the microstructure and reduce the surface hardness of the forging billet, which is beneficial for rough machining. The SUP13Cr / 1 material forgings produced according to this invention not only improves the internal microstructure of the forging billet and ensures uniform quality, but also increases the forging billet delivery rate. Detailed Implementation
[0009] Example 1: A heat treatment process after forging of SUP13Cr / 1 material; steel grade: SUP13Cr / 1; chemical composition: C=0.022%, Si=0.23%, Mn=0.47%, Cr=12.55%, Ni=5.47%, S=0.001%, P=0.019%, Mo=1.93%, V=0.07%; specifications: Φ335mm*7820mm; heat treatment process is as follows: Step 1) Annealing: When loading the furnace, the furnace temperature is controlled at 630℃~660℃ for waiting. Then, the temperature is increased to 890℃ at a rate of 80℃ / h and held for 10 hours. After holding, the billet is removed from the furnace and air-cooled until the surface temperature of the forging billet is 138℃. The temperature measurement point is based on the highest temperature. During air cooling, the billet is rotated 180 degrees every half hour to ensure uniform air cooling. Then, the forging billet is loaded into the heating furnace. Step 2) After Step 1) is completed, perform continuous tempering: put the forging billet into a heating furnace with a furnace temperature of 100℃~150℃ and hold it for 5 hours. Then, raise the temperature to 680℃ at a heating rate of 50℃ / h and hold it for 30 hours. Then, cool it with the furnace at a cooling rate of 20℃ / h until the furnace temperature is 285℃. Remove it from the furnace and air cool it to room temperature. Then put the forging billet into the heating furnace. Step 3) After step 2) is completed, perform high-temperature tempering: put the forging billet into a heating furnace with a furnace temperature of 310℃, and then heat it to 650℃ at a heating rate of 50℃ / h, hold it at that temperature for 20h, and then take it out of the furnace and air cool it until the surface temperature of the forging billet reaches 370℃ for hot straightening. After hot straightening, air cool it to room temperature.
[0010] The test results after production according to the above-mentioned post-forging heat treatment process are shown in Table 1: Table 1 Test Results Technical Requirements Grain size ≥ 4 Reticulate structures are not allowed. Actual testing Level 7.5 Areticular tissue After production using the post-forging heat treatment process of SUP13Cr / 1 material according to the present invention, the grain size and network structure of the forged billet meet the requirements.
[0011] Example 2: A post-forging heat treatment process for SUP13Cr / 1 material; Steel grade: SUP13Cr / 1; Chemical composition: C=0.021%, Si=0.22%, Mn=0.43%, Cr=12.55%, Ni=5.50%, S=0.003%, P=0.018%, Mo=1.97%, V=0.06%; Specifications: Φ335mm*7820mm; Heat treatment process is as follows: Step 1) Annealing: When loading the furnace, the furnace temperature is controlled at 630℃~660℃ for waiting. Then, the temperature is increased to 890℃ at a rate of 80℃ / h and held for 10 hours. After holding, the billet is removed from the furnace and air-cooled until the surface temperature of the forging billet is 135℃. The temperature measurement point is based on the highest temperature. During air cooling, the billet is rotated 180 degrees every half hour to ensure uniform air cooling. Then, the forging billet is loaded into the heating furnace. Step 2) After Step 1) is completed, perform continuous tempering: put the forging billet into a heating furnace with a furnace temperature of 100℃~150℃ and hold it for 5 hours. Then, raise the temperature to 680℃ at a heating rate of 50℃ / h and hold it for 30 hours. Then, cool it with the furnace at a cooling rate of 20℃ / h until the furnace temperature is 288℃. Remove it from the furnace and air cool it to room temperature. Then put the forging billet into the heating furnace. Step 3) After step 2) is completed, perform high-temperature tempering: put the forging billet into a heating furnace with a furnace temperature of 303℃, and then heat it to 650℃ at a heating rate of 50℃ / h, hold it at that temperature for 20h, and then take it out of the furnace and air cool it until the surface temperature of the forging billet reaches 350℃ for hot straightening. After hot straightening, air cool it to room temperature.
[0012] The test results after production according to the above-mentioned post-forging heat treatment process are shown in Table 2: Table 2 Test Results Technical Requirements Grain size ≥ 4 Reticulate structures are not allowed. Actual testing Levels 7-6.5 Areticular tissue After production using the post-forging heat treatment process of SUP13Cr / 1 material according to the present invention, the grain size and network structure of the forged billet meet the requirements.
Claims
1. A post-forging heat treatment process for SUP13Cr / 1 material, characterized in that: The SUP13Cr / 1 material has a Cr content between 12.0% and 13.0%, a Si content between 0.15% and 0.40%, a Mn content between 0.30% and 0.50%, a Ni content between 5.0% and 5.5%, a Mo content between 1.8% and 2.0%, and a V content between 0.06% and 0.09%. Its heat treatment process is as follows: Step 1) Annealing: When loading the furnace, the furnace temperature is controlled at 600℃~700℃ for waiting. Then, the temperature is increased to 880℃~910℃ at a rate of 10℃ / h~100℃ / h and held for 5h~30h. After holding, the billet is removed from the furnace and air-cooled until the surface temperature of the forging billet is 100℃~150℃. The temperature measurement point is based on the highest temperature. During air cooling, the billet is rotated 180 degrees every half hour to ensure uniform air cooling. Then, the forging billet is loaded into the heating furnace to prepare for continuous tempering. Step 2) Continuous tempering: The forging billet is placed in a heating furnace at a temperature of 100℃~150℃ and held for 2h~10h. Then, the temperature is increased to 660℃~700℃ at a heating rate of 5℃ / h~80℃ / h and held for a holding time of (7~10)*R / 100h, where R is the diameter of the forging billet. Then, the forging billet is cooled in the furnace at a cooling rate of 5℃ / h~30℃ / h until the furnace temperature is 280℃~300℃. Then, the forging billet is removed from the furnace and air-cooled to room temperature. Finally, the forging billet is placed in the heating furnace to prepare for high-temperature tempering. Step 3) High-temperature tempering: The forging billet is placed in a heating furnace with a furnace temperature ≤450℃, and then heated to 620℃~660℃ at a heating rate of 5℃ / h~80℃ / h. The holding time is (5~8)*R / 100h, where R is the diameter of the forging billet. Then, the billet is removed from the furnace and air-cooled until the surface temperature of the forging billet reaches 100℃~400℃ for hot straightening. After hot straightening, it is air-cooled to room temperature.
Citation Information
Patent Citations
Post-forging heat treatment process and forging process of G102Cr18Mo stainless steel forge piece
CN115125376A
125Ksi high-toughness SUP13Cr oil well pipe for shale gas and hot continuous rolling process manufacturing method
CN116607068A