Durable anti-mildew coating for door panels and preparation method thereof

Through the use of modified hollow glass beads and inorganic composite flame retardants, the problems of insufficient mildew resistance, sound insulation and flame retardancy of coatings in humid environments are solved, and the durable mildew resistance, sound insulation and flame retardant properties are improved. , ensuring the long-term use of the door panel and human health and safety.

CN118307997BActive Publication Date: 2024-10-01GUANGDONG NATURE HOME FURNISHING TECH RES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410407903.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-07
Publication Date
2024-10-01
Estimated Expiration
2044-04-07

AI Technical Summary

Technical Problem

Existing coatings have poor mildew resistance, sound insulation and flame retardancy in humid environments, making it difficult to meet the high functional requirements of modern industry.

Method used

Modified hollow glass beads and inorganic composite flame retardants are used as functional additives and flame retardants. Through plasma treatment and organic modification, the anti-mildew, sound insulation and flame retardant properties of the coating are enhanced.

Benefits of technology

It significantly improves the antibacterial and mildew-proof performance, sound insulation effect and flame retardant performance of the coating, extends the service life of the door panel, and ensures human health and building safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118307997B_ABST
    Figure CN118307997B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, and discloses a durable mildew-proof coating for door panels and a preparation method thereof. The coating comprises the following raw materials: acrylic emulsion, filler, functional additive, inorganic composite flame retardant, antioxidant, water, film-forming aid, leveling agent, and defoamer; wherein the functional additive is prepared by grafting ε-polylysine onto the surface of hollow glass microspheres; the inorganic composite flame retardant is tourmaline powder modified by nitrogen-phosphorus organic modification, and the advantages of the functional additive and the inorganic composite flame retardant are utilized to improve the mildew-proof performance, sound insulation performance and flame retardant performance of the coating, which is beneficial to prolonging the service life of the coating, creating a more beautiful, safe and comfortable environment for people, and having greater practical promotion value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a durable anti-mildew coating for door panels and a preparation method thereof. Background Art

[0002] Door panels are prone to mold in a humid environment, especially during the rainy season in the south. This is particularly serious for basements or houses on low floors. Mold not only reproduces on door panels, but its shed spores are also easily dispersed into the air. Once inhaled by the human body, it may cause adverse effects on health. In addition, the presence of mold will seriously affect the aesthetics of door panels and destroy the cleanliness and comfort of the indoor environment. In order to protect door panels and extend their service life, the most common method is to coat them with anti-mold paint to form an anti-mold coating, thereby enhancing the anti-mold ability of door panels. In order to make the paint have anti-mold properties, adding additives with anti-mold properties during paint production has become a hot research topic in the current paint field.

[0003] With the development of modern industry, higher requirements are placed on the functionality of coatings. Compared with ordinary coatings, coatings used for door panels need to have sound insulation effects, because in daily life, there are a lot of noises around us, such as the sound of vehicles driving, the sound of construction sites, the sound of square dancing, etc., which will cause serious noise pollution and affect people's sleep and life. In addition, door panels are an important part of buildings, and their flame retardant properties are directly related to the safety of other objects inside the building. The use of flame retardant coatings can reduce the degree of damage to other objects caused by fire and reduce property losses. Therefore, it is extremely important to develop a durable, mildew-proof coating that has sound insulation and flame retardant properties.

[0004] The patent with publication number CN114921163B discloses a nano-silver antibacterial and mildew-proof water-based polyurethane coating and its preparation method. The invention improves the mildew-proof performance of the coating by adding a specific nano-silver ion antibacterial agent into the matrix. Even in an environment with a humidity greater than 70%, its antibacterial and mildew-proof properties are still good. However, nano-silver is easily oxidized and can easily cause changes in the overall performance of the coating. Summary of the invention

[0005] The purpose of the present invention is to provide a durable anti-mildew coating for door panels and a preparation method thereof, which solves the following technical problems:

[0006] (1) It solves the problem of poor mildew resistance of ordinary coatings;

[0007] (2) It solves the problem of poor sound insulation of ordinary coatings;

[0008] (3) It solves the problem of poor flame retardancy of ordinary coatings.

[0009] The purpose of the present invention can be achieved by the following technical solutions:

[0010] A durable anti-mildew paint for door panels comprises the following raw materials in parts by weight: 50-70 parts of acrylic emulsion, 10-15 parts of filler, 6-8 parts of functional additives, 4-6 parts of inorganic composite flame retardant, 1-2 parts of antioxidant, 20-40 parts of water, 1-2 parts of film-forming aid, 1-3 parts of leveling agent and 2-3 parts of defoaming agent.

[0011] Furthermore, the preparation method of the functional additive comprises the following steps:

[0012] S1: placing the hollow glass microspheres in a plasma treatment apparatus, evacuating the cavity to 8-10 Pa, then injecting air to clean the hollow glass microspheres, and after the cleaning process, maintaining the vacuum degree of the cavity at 8-10 Pa, and then injecting oxygen to activate the hollow glass microspheres to obtain pretreated hollow glass microspheres;

[0013] S2: adding the pretreated hollow glass microspheres to dimethyl sulfoxide, ultrasonically dispersing for 10 to 30 minutes, passing nitrogen protection, then adding glyoxylic acid and a catalyst, mixing, stirring at a temperature of 90 to 110° C. for 4 to 8 hours, cooling the material, filtering, washing, and drying to obtain modified hollow glass microspheres;

[0014] S3: Place the modified hollow glass microspheres in ionized water, and ultrasonically disperse them to form a uniform dispersion. Continue to add ε-polylysine to the dispersion, and then begin to drop sodium hydroxide solution, adjust the pH value of the system to 7.5-8.5, increase the temperature to 45-55°C, stir the reaction for 6-10 hours, and discharge the material to obtain a functional additive.

[0015] Furthermore, in step S1, the average particle size of the hollow glass microspheres is 5 μm.

[0016] Furthermore, in step S2, the catalyst is any one of trifluoromethanesulfonic acid, p-toluenesulfonic acid or aminosulfonic acid.

[0017] Furthermore, in step S3, the mass fraction of the sodium hydroxide solution is 10% to 40%.

[0018] Through the above technical scheme, the hollow glass microspheres are subjected to plasma treatment, and hydroxyl groups are introduced on the surface of the hollow glass microspheres. Under the action of a catalyst, the carboxyl groups in the glyoxylic acid structure can react with the hydroxyl groups on the surface of the hollow glass microspheres, thereby grafting the glyoxylic acid onto the surface of the hollow glass microspheres to obtain modified hollow glass microspheres. Then, based on the principle that the active amino functional groups in the ε-polylysine structure can react with the aldehyde functional groups on the surface of the modified hollow glass microspheres to undergo a Schiff base reaction, the ε-polylysine is further grafted onto the surface of the hollow glass microspheres to obtain a functional additive.

[0019] Furthermore, the preparation method of the inorganic composite flame retardant comprises the following steps:

[0020] SS1: Tourmaline powder and tetrahydrofuran are added to the reactor in sequence, and after being mixed evenly, 6-chloronicotinoyl chloride is added to the reactor under stirring conditions. After the addition is complete, the mixture is stirred at room temperature for 5 to 7 hours. The obtained product is washed with anhydrous ethanol for 2 to 4 times, and then dried to obtain modified tourmaline powder;

[0021] SS2: Disperse the modified tourmaline powder in N,N-dimethylformamide to form a stable dispersion, then add 2,6,7-trioxa-1-phosphabicyclo (2.2.2) octane-4-methanol-1-oxide and a promoter, introduce nitrogen to exhaust the air, turn on the heating, wait for the temperature to rise to 70-80°C, stir and react for 5-9 hours. After the reaction is completed, centrifuge the solid material, wash and vacuum dry it to obtain an inorganic composite flame retardant.

[0022] Furthermore, in step SS1, the particle size of the tourmaline powder is 3 to 10 μm.

[0023] Furthermore, in step SS1, the mass ratio of the tourmaline powder to 6-chloronicotinoyl chloride is 1:0.1-0.6.

[0024] Furthermore, in step SS2, the promoter is any one of triethylamine or pyridine.

[0025] Through the above technical scheme, the acyl chloride group in the structure of 6-chloronicotinoyl chloride is highly active and can react with the hydroxyl group on the surface of tourmaline powder to introduce the halogen group into the surface of the tourmaline powder to obtain modified tourmaline powder. Then, through the halogen substitution reaction, 2,6,7-trioxa-1-phosphabicyclo (2.2.2) octane-4-methanol-1-oxide is grafted onto the surface of the tourmaline powder to obtain an inorganic composite flame retardant.

[0026] A method for preparing a durable anti-mildew coating for door panels comprises the following steps:

[0027] Ⅰ: Add acrylic emulsion, filler, functional additive, inorganic composite flame retardant, antioxidant and deionized water into a mixer, set the stirring speed of the mixer to 400-600 r / min, stir and mix for 30-50 min to obtain a premix;

[0028] II: Pour the film-forming aid, leveling agent and defoamer into the premix obtained in step I, continue stirring for 30 to 50 minutes, and obtain the coating after natural defoaming.

[0029] Beneficial effects of the present invention:

[0030] (1) The present invention prepares hollow glass microspheres with surface modified ε-polylysine as a functional additive and mixes them with a matrix material. After the hollow glass microspheres are organically modified, they can achieve good compatibility with the matrix material, so that the hollow glass microspheres are evenly and stably dispersed in the matrix material. On the one hand, the hollow glass microspheres have a special spherical structure, which can enhance the absorption and reflection of sound waves, effectively extend the propagation path of sound waves in the matrix, and enhance the attenuation performance of sound waves. At the same time, since the microspheres are spherical particles with uniform particles, they are arranged tightly and orderly, and can be evenly distributed in the material, thereby forming a tight sound insulation layer, which can further block the propagation of sound, thereby achieving a sound insulation effect. On the other hand, the anti-mildew and antibacterial properties of ε-polylysine can be used to effectively improve the anti-mildew and antibacterial properties of the coating, thereby avoiding the problem of damage to door panels due to the generation of a large number of bacteria and molds in a humid environment, which affects human health.

[0031] (2) The present invention prepares an inorganic composite flame retardant, which is a tourmaline powder modified by nitrogen-phosphorus organic modification. After modification, the binding force between the tourmaline powder and the matrix material is greatly enhanced, which helps to evenly and stably disperse the tourmaline powder in the matrix material. The tourmaline powder can release negative ions, thereby inhibiting the growth and reproduction of mold, further improving the mildew resistance of the coating. In addition, the nitrogen-phosphorus flame retardant element contained in the inorganic composite flame retardant can form a dense barrier layer on its surface when burning, effectively isolating oxygen and heat, thereby inhibiting the combustion reaction and improving the flame retardant performance of the coating.

[0032] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0034] Figure 1 This is a scanning electron microscope image of the hollow glass microspheres and functional additives prepared in Example 1 of the present invention.

[0035] Figure 2 This is an infrared spectrum test chart of the modified tourmaline powder and the inorganic composite flame retardant prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] 1. Preparation of functional additives

[0039] S1: 5g of hollow glass microspheres with an average particle size of 5μm are placed in a plasma treatment instrument with a power of 50W, the cavity is evacuated to 9Pa, and then air is injected to clean the hollow glass microspheres for 80s. After the cleaning process is completed, the vacuum degree of the cavity is maintained at 9Pa, and then oxygen is injected. When the oxygen flow rate is stabilized to 0.5L / min, the high-frequency power supply is turned on to activate the hollow glass microspheres for 100s to obtain pretreated hollow glass microspheres;

[0040] S2: 5 g of pretreated hollow glass microspheres were added to dimethyl sulfoxide, and ultrasonically dispersed for 20 min under nitrogen protection, and then 2.1 g of glyoxylic acid and 0.1 g of trifluoromethanesulfonic acid were added, mixed, and stirred at a temperature of 100° C. for 6 h. After the material was cooled, filtered, washed, and dried, the modified hollow glass microspheres were obtained;

[0041] S3: Place 5 g of modified hollow glass microspheres in ionized water and ultrasonically disperse them to form a uniform dispersion. Continue to add 3.2 g of ε-polylysine to the dispersion, then start to drop a 20% mass fraction of sodium hydroxide solution, adjust the pH value of the system to 8, increase the temperature to 50°C, stir the reaction for 8 hours, discharge the material, and obtain a functional additive.

[0042] The morphology of hollow glass microspheres and functional additives was analyzed using an EVO 18 scanning electron microscope. The test results are shown in Figure 1, where A is hollow glass microspheres and B is functional additives. As can be seen from the figure, the hollow glass microspheres have a spherical structure with a smooth surface, while the surface morphology of the functional additives changes significantly and becomes rough. This is because ε-polylysine is grafted onto the surface of the hollow glass microspheres.

[0043] 2. Preparation of Inorganic Composite Flame Retardant

[0044] SS1: 3 g of tourmaline powder with an average particle size of 3 μm and tetrahydrofuran were added to the reactor in sequence. After mixing evenly, 1.4 g of 6-chloronicotinoyl chloride was added to the reactor under stirring. After the addition was completed, the mixture was stirred at room temperature for 6 h. The obtained product was washed 3 times with anhydrous ethanol and dried to obtain modified tourmaline powder.

[0045] SS2: Disperse 3 g of modified tourmaline powder in N,N-dimethylformamide to form a stable dispersion, then add 1.5 g of 2,6,7-trioxa-1-phosphabicyclo (2.2.2) octane-4-methanol-1-oxide and 0.08 g of triethylamine, introduce nitrogen to exhaust the air, turn on the heating, wait for the temperature to rise to 75°C, stir and react for 7 hours. After the reaction is completed, centrifuge the solid material, wash and vacuum dry it to obtain an inorganic composite flame retardant.

[0046] The infrared spectrometer Spectrum 100 was used to conduct infrared tests on modified tourmaline powder and inorganic composite flame retardant. Figure 2 As shown in the figure, the analysis shows that in the infrared spectrum of modified tourmaline powder, 1275cm -1 The characteristic absorption peak of BO appears at 1025cm -1 The characteristic absorption peak of Si-O appears at 1722cm -1 The characteristic absorption peak of the ester group C=O appears at 713 cm -1 The characteristic absorption peak of CCl appears at 1606cm -1 The characteristic absorption peak of C=N appears at 1408cm -1 The characteristic absorption peak of CN appears at 1745cm. This is because the hydroxyl groups on the surface of tourmaline powder can react with the acyl chloride groups in the structure of 6-chloronicotinoyl chloride to obtain modified tourmaline powder. In the infrared spectrum of the inorganic composite flame retardant, 1745cm -1 The characteristic absorption peak of the ester group C=O appears at 1075cm -1 The characteristic absorption peak of ether bond COC appears at 1611 cm -1 The characteristic absorption peak of C=N appears at 1421cm -1 The characteristic absorption peak of CN appears at 1252cm -1A characteristic absorption peak of P=O appears at the surface of the modified tourmaline powder. This is because the halogen on the surface of the modified tourmaline powder can undergo a substitution reaction with the hydroxyl group in the structure of 2,6,7-trioxa-1-phosphabicyclo (2.2.2) octane-4-methanol-1-oxide to obtain an inorganic composite flame retardant.

[0047] 3. Preparation of coating

[0048] Ⅰ: Add 50 g acrylic emulsion, 10 g talcum powder, 6 g functional additive, 4 g inorganic composite flame retardant, 1 g antioxidant 1098, and 20 g deionized water into a blender, set the blender stirring speed to 400 r / min, and stir and mix for 30 min to obtain a premix;

[0049] II: Pour 1 g of propylene glycol methyl ether, 1 g of polybutyl acrylate and 2 g of fatty alcohol polyoxyethylene ether into the premix obtained in step I, continue stirring for 30 min, and obtain the coating after natural defoaming.

[0050] Example 2

[0051] Coating preparation

[0052] Ⅰ: Add 60g acrylic emulsion, 12g talcum powder, 7g functional additive, 5g inorganic composite flame retardant, 1.5g antioxidant 1098, and 30g deionized water into a blender, set the blender stirring speed to 500r / min, and stir and mix for 40min to obtain a premix;

[0053] II: Pour 1.5 g of propylene glycol methyl ether, 2 g of polybutyl acrylate and 2.5 g of fatty alcohol polyoxyethylene ether into the premix obtained in step I, continue stirring for 40 min, and obtain the coating after natural defoaming.

[0054] The preparation method of the functional additive and the inorganic composite flame retardant is the same as that in Example 1.

[0055] Example 3

[0056] Coating preparation

[0057] Ⅰ: Add 70g acrylic emulsion, 15g talcum powder, 8g functional additive, 6g inorganic composite flame retardant, 2g antioxidant 1098, and 40g deionized water into a blender, set the blender stirring speed to 600r / min, and stir and mix for 50min to obtain a premix;

[0058] II: Pour 2g of propylene glycol methyl ether, 3g of polybutyl acrylate and 3g of fatty alcohol polyoxyethylene ether into the premix obtained in step I, continue stirring for 50 minutes, and obtain the coating after natural defoaming.

[0059] The preparation method of the functional additive and the inorganic composite flame retardant is the same as that in Example 1.

[0060] Comparative Example 1

[0061] Coating preparation

[0062] Ⅰ: Add 60g acrylic emulsion, 12g talcum powder, 7g functional additive, 1.5g antioxidant 1098 and 30g deionized water into a blender, set the blender stirring speed to 500r / min, and stir and mix for 40min to obtain a premix;

[0063] II: Pour 1.5 g of propylene glycol methyl ether, 2 g of polybutyl acrylate and 2.5 g of fatty alcohol polyoxyethylene ether into the premix obtained in step I, continue stirring for 40 min, and obtain the coating after natural defoaming.

[0064] The preparation method of the functional additive is the same as that in Example 1.

[0065] Comparative Example 2

[0066] Coating preparation

[0067] Ⅰ: Add 60g acrylic emulsion, 12g talcum powder, 5g inorganic composite flame retardant, 1.5g antioxidant 1098, and 30g deionized water into a blender, set the blender stirring speed to 500r / min, and stir and mix for 40min to obtain a premix;

[0068] II: Pour 1.5 g of propylene glycol methyl ether, 2 g of polybutyl acrylate and 2.5 g of fatty alcohol polyoxyethylene ether into the premix obtained in step I, continue stirring for 40 min, and obtain the coating after natural defoaming.

[0069] The preparation method of the inorganic composite flame retardant is the same as that in Example 1.

[0070] Comparative Example 3

[0071] Coating preparation

[0072] Ⅰ: Add 60g acrylic emulsion, 12g talcum powder, 7g functional additive, 5g tourmaline powder, 1.5g antioxidant 1098 and 30g deionized water into a blender, set the blender stirring speed to 500r / min, stir and mix for 40min to obtain a premix;

[0073] II: Pour 1.5 g of propylene glycol methyl ether, 2 g of polybutyl acrylate and 2.5 g of fatty alcohol polyoxyethylene ether into the premix obtained in step I, continue stirring for 40 min, and obtain the coating after natural defoaming.

[0074] The preparation method of the functional additive is the same as that in Example 1.

[0075] Comparative Example 4

[0076] Coating preparation

[0077] Ⅰ: Add 60g acrylic emulsion, 12g talc, 3g hollow glass microspheres, 4g ε-polylysine, 5g inorganic composite flame retardant, 1.5g antioxidant 1098, and 30g deionized water into a blender, set the blender stirring speed to 500r / min, and stir and mix for 40min to obtain a premix;

[0078] II: Pour 1.5 g of propylene glycol methyl ether, 2 g of polybutyl acrylate and 2.5 g of fatty alcohol polyoxyethylene ether into the premix obtained in step I, continue stirring for 40 min, and obtain the coating after natural defoaming.

[0079] The preparation method of the inorganic composite flame retardant is the same as that in Example 1.

[0080] Comparative Example 5

[0081] Coating preparation

[0082] Ⅰ: Add 60g acrylic emulsion, 12g talcum powder, 1.5g antioxidant 1098 and 30g deionized water into a mixer, set the stirring rate of the mixer to 500r / min, stir and mix for 40min to obtain a premix;

[0083] II: Pour 1.5 g of propylene glycol methyl ether, 2 g of polybutyl acrylate and 2.5 g of fatty alcohol polyoxyethylene ether into the premix obtained in step I, continue stirring for 40 min, and obtain the coating after natural defoaming.

[0084] The acrylic emulsion used in the above Examples 1 to 3 and Comparative Examples 1 to 5 was purchased from Shanghai Zhenlishi Network Technology Co., Ltd., and the model number was PRI MAL TR-407.

[0085] Performance Testing

[0086] ① The coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were uniformly coated on the surface of a clean wooden board to prepare samples that met the specifications. After being thoroughly dried, performance tests were performed. The samples were tested for mildew resistance and antibacterial properties according to HG / T 3950-2007; according to the UL-94 flame retardant grade standard, vertical combustion tests were performed on the samples to determine the flame retardant properties of the samples. The specific test results are shown in the following table:

[0087]

[0088] From the test results in the above table, it can be seen that the samples prepared in Examples 1 to 3 all have excellent durable mildew resistance, antibacterial and flame retardancy; the sample prepared in Comparative Example 1 added a functional additive, and the mildew resistance and antibacterial performance of the sample was good, and it had mildew resistance durability, but no inorganic composite flame retardant was added, and the flame retardancy of the sample was poor compared with the examples; the sample prepared in Comparative Example 2 added an inorganic composite flame retardant, and the flame retardancy of the sample was good, but no functional additive was added, and the mildew resistance and antibacterial performance of the sample were average compared with the examples; the sample prepared in Comparative Example 3 added a functional additive The samples prepared by adding inorganic composite flame retardant, hollow glass microspheres and ε-polylysine showed good mildew resistance, antibacterial and flame retardancy. The samples prepared by adding neither functional additives nor inorganic composite flame retardants showed poor mildew resistance, antibacterial and flame retardancy. However, the flame retardancy of the samples was average, which may be because the surface of the tourmaline powder was not organically modified, and the tourmaline powder agglomerated in the matrix, resulting in a decrease in the flame retardancy of the samples. In the samples prepared by comparative example 4, inorganic composite flame retardant, hollow glass microspheres and ε-polylysine were added, and the samples showed good durable mildew resistance, antibacterial and flame retardancy. In the samples prepared by comparative example 5, neither functional additives nor inorganic composite flame retardants were added, and the mildew resistance, antibacterial and flame retardancy of the samples were poor.

[0089] ② According to GB / T 50121-2005, the normalized impact sound pressure levels of the coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 5 at different impact frequencies of 100 Hz, 400 Hz and 1600 Hz were measured, and the sound insulation performance of the coatings was evaluated by the improvement in the impact sound pressure levels. The specific test results are shown in the following table:

[0090]

[0091] From the test results in the above table, it can be seen that the coatings prepared in Examples 1 to 3 and Comparative Examples 1 and 3 have good sound insulation effects; unmodified hollow glass microspheres are added to the coating prepared in Comparative Example 4, and the sound insulation effect of the coating is average, which may be because the unmodified hollow glass microspheres are agglomerated in the matrix and are unevenly dispersed in the matrix, resulting in average sound insulation effect of the coating; since hollow glass microspheres are not added to the coatings prepared in Comparative Examples 2 and 5, the sound insulation effect of the coatings is poor.

[0092] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A durable anti-mildew coating for door panels, characterized in that: The invention comprises the following raw materials in parts by weight: 50-70 parts of acrylic emulsion, 10-15 parts of filler, 6-8 parts of functional additive, 4-6 parts of inorganic composite flame retardant, 1-2 parts of antioxidant, 20-40 parts of water, 1-2 parts of film-forming aid, 1-3 parts of leveling agent, and 2-3 parts of defoaming agent; The preparation method of the functional additive comprises the following steps: S1: placing the hollow glass microspheres in a plasma treatment apparatus, evacuating the cavity to 8-10 Pa, then injecting air to clean the hollow glass microspheres, and after the cleaning process, maintaining the vacuum degree of the cavity at 8-10 Pa, and then injecting oxygen to activate the hollow glass microspheres to obtain pretreated hollow glass microspheres; S2: adding the pretreated hollow glass microspheres to dimethyl sulfoxide, ultrasonically dispersing for 10 to 30 minutes, passing nitrogen protection, then adding glyoxylic acid and a catalyst, mixing, stirring at a temperature of 90 to 110° C. for 4 to 8 hours, cooling the material, filtering, washing, and drying to obtain modified hollow glass microspheres; S3: Place the modified hollow glass microspheres in deionized water, and ultrasonically disperse them to form a uniform dispersion, continue to add ε-polylysine to the dispersion, and then begin to drop sodium hydroxide solution, adjust the pH value of the system to 7.5-8.5, increase the temperature to 45-55° C., stir the reaction for 6-10 hours, and discharge the material to obtain a functional additive; The preparation method of the inorganic composite flame retardant comprises the following steps: SS1: Tourmaline powder and tetrahydrofuran are added to the reactor in sequence, and after being mixed evenly, 6-chloronicotinoyl chloride is added to the reactor under stirring conditions. After the addition is complete, the mixture is stirred at room temperature for 5 to 7 hours. The obtained product is washed with anhydrous ethanol for 2 to 4 times, and then dried to obtain modified tourmaline powder; SS2: Disperse the modified tourmaline powder in N,N-dimethylformamide to form a stable dispersion, then add 2,6,7-trioxa-1-phosphabicyclo (2.2.2) octane-4-methanol-1-oxide and a promoter, introduce nitrogen to exhaust the air, turn on the heating, wait for the temperature to rise to 70-80°C, stir and react for 5-9 hours. After the reaction is completed, centrifuge the solid material, wash and vacuum dry it to obtain an inorganic composite flame retardant.

2. The durable anti-mildew paint for door panels according to claim 1, characterized in that: In step S1, the average particle size of the hollow glass microspheres is 5 μm.

3. The durable anti-mildew paint for door panels according to claim 1, characterized in that: In step S2, the catalyst is any one of trifluoromethanesulfonic acid, p-toluenesulfonic acid or aminosulfonic acid.

4. The durable anti-mildew paint for door panels according to claim 1, characterized in that: In step S3, the mass fraction of the sodium hydroxide solution is 10% to 40%.

5. The durable anti-mildew paint for door panels according to claim 1, characterized in that: In step SS1, the particle size of the tourmaline powder is 3 to 10 μm.

6. The durable anti-mildew paint for door panels according to claim 1, characterized in that: In step SS1, the mass ratio of the tourmaline powder to 6-chloronicotinoyl chloride is 1:0.1-0.

6.

7. The durable anti-mildew paint for door panels according to claim 1, characterized in that: In step SS2, the promoter is any one of triethylamine or pyridine.

8. A method for preparing the durable anti-mildew paint for door panels as claimed in claim 1, characterized in that: The preparation method comprises the following steps: Ⅰ: Add acrylic emulsion, filler, functional additive, inorganic composite flame retardant, antioxidant and deionized water into a mixer, set the stirring speed of the mixer to 400-600 r / min, stir and mix for 30-50 min to obtain a premix; II: Pour the film-forming aid, leveling agent and defoamer into the premix obtained in step I, continue stirring for 30 to 50 minutes, and obtain the coating after natural defoaming.