A gradient titanium-based material and preparation method thereof
By stacking gradient titanium-based composite material layers on the surface of titanium alloy materials and using reinforcing phases such as TiB, Y2O3 and Ti5Si3 to control the microstructure, the deficiencies of titanium alloy materials in terms of high impact and wear resistance are solved, and high strength, toughness, and wear resistance are achieved. Improved wear and impact resistance improves the reliability and service performance of parts.
Patent Information
- Application Number
- CN202410711997.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-04
AI Technical Summary
Traditional titanium alloy materials cannot meet the structural and functional requirements of wear resistance, heat resistance, and corrosion resistance under conditions of high impact, alternating bending, and contact stress. Moreover, surface strengthening treatment is costly and unreliable, and the coating and substrate are not firmly bonded, resulting in Parts are prone to friction, wear and peeling during service.
Gradient titanium-based materials are used. By stacking multiple titanium-based composite material layers on the surface of the titanium alloy substrate, the volume fraction of the reinforcing phase is distributed in a step gradient. The interface structure of the metallurgical bonding is designed, and the reinforcing phases such as TiB, Y2O3 and Ti5Si3 are used for microscopic analysis. Tissue regulation to achieve high strength, toughness, wear resistance and impact resistance.
It achieves a comprehensive improvement in the high modulus, high hardness, wear resistance and impact resistance of titanium-based materials, reduces the risk of friction, wear and peeling of parts, and improves the reliability and service performance of components.
Smart Images

Figure CN118308669B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material science and technology processing and manufacturing, and specifically relates to a gradient titanium-based material and a preparation method thereof. Background Art
[0002] Lightweight, high-performance materials can not only achieve the mission requirements of full-area mobility and target execution of equipment in the field of national defense, but also lightweight components are an effective way to achieve energy conservation, emission reduction and efficiency improvement in the field of civil transportation. Although traditional single homogeneous lightweight metal structural materials have the characteristics of high strength and high toughness, in actual application scenarios, when high strength and toughness are required while meeting the requirements of structural functional integration such as wear resistance, heat resistance and corrosion resistance, they are often achieved through coating technology and surface strengthening treatment. On the one hand, the technical requirements for the combination brought about by the matching of the physical and chemical properties of the external coating and the substrate are relatively high; on the other hand, the cost of the surface strengthening process is high, and the single detection technology cannot comprehensively reflect the reliability of the material or component during use.
[0003] Titanium alloy has become a lightweight alloy material with great potential to replace traditional metals due to its low density, high specific strength, good high temperature resistance and corrosion resistance. However, with the increasingly stringent requirements for vehicle service performance, titanium alloy is still difficult to be competent in components serving under high impact, alternating bending and contact stress conditions due to its low elastic modulus and wear resistance. For example, the balance elbow component of the military tracked vehicle motion system is a key component connecting the motion and suspension devices. There are two cylindrical surfaces on the axis of the balance elbow body as the rotating friction surface between the components, and there are problems of friction and wear in long-term service; in addition, the titanium-based composite armor of armored vehicles can obtain different protective effects through different combinations of materials, thicknesses, connection methods, fine structures and shapes of each layer. Among civilian automotive parts, gears are important parts with a large usage, and often have problems of tooth breakage, tooth surface peeling and excessive wear. At present, for the above-mentioned titanium alloy wear-resistant parts, laser cladding, surface nitriding, vapor deposition and other surface strengthening treatment processes have been adopted, but there are problems such as shallow wear-resistant coating depth, weak bonding between coating and substrate, hard and brittle wear-resistant coating, and difficult machining. For titanium alloy composite armor, adhesives are often used for bonding, and the bonding strength is low. Therefore, developing a preparation method in which the functional layer is strongly metallurgically bonded to the titanium alloy substrate and the functional layer design is controllable is an effective way to solve the problem of structural and functional integration of such parts. Summary of the invention
[0004] The present invention aims to at least partially overcome the above-mentioned technical problems and / or other potential problems existing in the prior art: by regulating the microstructure and properties of the gradient titanium-based material, a gradient titanium-based material and a preparation method thereof are provided that meet the requirements of high strength, toughness, wear resistance and impact resistance. The design of the step gradient interface of the present invention can avoid the step mutation of elements / thermal parameters / phase type / phase content / stress concentration in the transition zone. In addition, the metallurgical bonding of the interface gives the titanium-based materials and components with step gradient transition comprehensive performance advantages. At the same time, the preparation method of the gradient titanium-based material of the present invention has a short process flow, high reliability and strong versatility.
[0005] The technical solution of the present invention is as follows: a gradient titanium-based material, in which multiple titanium-based composite material layers are stacked on the surface of a titanium alloy substrate, and the titanium-based composite material layers include a matrix phase and a reinforcement phase; the composition of the matrix phase is the same as that of the titanium alloy substrate; the volume fraction of the reinforcement phase in each titanium-based composite material layer is distributed in a step gradient, and the volume fraction of the reinforcement phase in the nth titanium-based composite material layer is 0.5n%-5n%, n≥1, and n is an integer.
[0006] When n=1, it represents the first layer adjacent to the titanium alloy substrate, and when n=2, it represents the second layer adjacent to the first layer, and so on.
[0007] Preferably, the thickness of the titanium-based composite material layer is 0.2-10 mm; and the number of titanium-based composite material layers stacked on the surface of the titanium alloy substrate is at most 10 layers.
[0008] As an optimization, the reinforcement phase is TiB whiskers with a size of 5-20 μm, Y2O3 with a grain size of 50-100 nm, and Ti5Si3 reinforcement phases, wherein the volume fraction ratio of TiB, Y2O3 and Ti5Si3 is (2-5): (0.2-1): (0.2-1).
[0009] The present invention also provides a method for preparing a gradient titanium-based material, comprising the following steps:
[0010] 1) Designing a mold to surround the titanium alloy substrate and fill the powder raw materials of multiple layers of titanium-based composite materials; preforming the blank by cold pressing or cold isostatic pressing preforming method;
[0011] 2) The prefabricated blank is subjected to vacuum hot pressing sintering or hot isostatic pressing densification forming, and then subjected to rolling, extrusion or forging forming processing, and finally subjected to heat treatment to obtain a gradient titanium-based material.
[0012] As an optimization, in step 1), the powder raw material of the titanium-based composite material layer includes a matrix phase raw material and a reinforcement phase raw material; the reinforcement phase raw material is a mixture of multiple powders of Si, Y2O3 and TiB2, wherein the average particle size of Si and TiB2 is 1-10μm, and the average particle size of Y2O3 is 50-100nm; the matrix phase raw material is a titanium alloy powder with the same composition as the titanium alloy substrate, with an average particle size of 13-250μm, and the powder morphology is spherical or irregular.
[0013] As an optimization, in step 1), the temperature of the cold pressing or cold isostatic pressing preforming is room temperature, the pressure is 60-600 MPa, and the holding time is 0.5-15 min.
[0014] As an optimization, in step 2), the heating temperature of the vacuum hot pressing sintering or hot isostatic pressing densification molding is 1000-1300°C, the holding time is 1.5-6h, the hot isostatic pressing pressure is 100-240MPa, and the vacuum hot pressing sintering pressure is 20-40MPa.
[0015] As an optimization, in step 2), the heating temperature of the rolling, extrusion or forging forming process is 820-1050°C, the temperature is kept for 3-6 hours, the deformation temperature is 820-1050°C, and the surface is sprayed with glass lubricant for anti-oxidation treatment before heating and deformation.
[0016] As an optimization, in step 2), the heat treatment process is as follows: the solution temperature is 740-950°C and the solution time is 1-6h; then, the solution is heated to 500-650°C, kept at this temperature for 2-6h, and air-cooled.
[0017] Specifically, the present invention provides a method for preparing a balanced elbow component using the gradient titanium-based material, comprising the following steps:
[0018] 1) According to the technical requirements of the balancing elbow component, select TC18 titanium alloy bars that meet the performance requirements and have qualified chemical composition, calculate the specifications of the TC18 titanium alloy bars according to the size of the balancing elbow component, and perform cutting and end chamfering;
[0019] 2) Design the number of titanium-based composite material layers and the composition of each layer for the step-gradient transition on the surface of TC18 titanium alloy rod: the titanium-based composite material layer adjacent to the titanium alloy rod is the first layer, and 4 layers of step-gradient transition layers are designed, each with a thickness of 2 mm. The compositions of the 1st to 4th layers of titanium-based composite materials are: 1 vol.% (TiB+Y2O3+Ti5Si3) / TC18, 2 vol.% (TiB+Y2O3+Ti5Si3) / TC18, 3 vol.% (TiB+Y2O3+Ti5Si3) / TC18 and 4vol.% (TiB+Y2O3+Ti5Si3) / TC18, the raw material powder is selected according to the designed titanium-based composite material layer composition; the raw material powder of the reinforcing phase is Si, Y2O3 and TiB2, wherein the average particle size of Si and TiB2 is 3μm, the average particle size of Y2O3 is 100nm, the average particle size of TC18 titanium alloy powder is 70μm, and the raw material ratio of the reinforcing phase (TiB+Y2O3+Ti5Si3) is prepared according to the volume fraction TiB:Y2O3:Ti5Si3=3:0.5:0.5;
[0020] 3) Design a 4-layer gradient titanium-based rod powder filling mold: the structure is that a steel chassis with partition slots is placed at the bottom of the rubber sleeve, and the slots are distributed in concentric circles, with a total of 3 concentric circle slots; 0.2mm thick aluminum foil is rolled into a cylinder and inserted into the chassis slot for fixation; the surface of the TC18 titanium alloy rod is polished and placed in the center of the powder filling mold, and accordingly, titanium-based powder is filled in each interlayer step by step. After powder filling, the sleeve is sealed; then cold isostatic pressing is performed for preforming. At room temperature, liquid is used as the pressure medium, the pressure is 400MPa, and the pressure holding time is 1min to obtain a gradient TC18 titanium-based material prefabricated blank;
[0021] 4) The aluminum foil separator in the prefabricated blank is removed, the blank is sealed with a steel sheath, and hot isostatic pressing is performed to densify the blank at a heating temperature of 1200°C, a holding time of 3 hours, a pressure of 140 MPa, and a vacuum environment; a gradient TC18 titanium-based rod is obtained, and the sheath is removed;
[0022] 5) The gradient TC18 titanium-based bar is die-forged at a heating temperature of 840°C, a holding time of 4 hours, and a forging temperature of 840°C to obtain a forging blank;
[0023] 6) The forging blank is subjected to double annealing treatment, with the first solution temperature being 840°C and the solution time being 3h. The second solution temperature is furnace cooled to 750°C, kept at this temperature for 3h, and air cooled. It is then heated to 650°C, kept at this temperature for 4h, and air cooled. It is then subjected to fine mechanical processing to obtain a TC18 titanium alloy balance elbow component.
[0024] The beneficial effects of the present invention are as follows: the gradient material is a material that selects two or more homogeneous materials with different properties, and gradually changes the composition and structure of these two (or more) materials so that the material properties change with the changes in the composition and structure of the materials, thereby forming a functional gradient material with performance change characteristics. The performance of the gradient material can change from one end of the material to the other end in a discontinuous or continuous manner, and the material properties can be presented in a step-like or gradual manner through different gradient designs. The titanium-based composite material is a composite material in which a high modulus, high strength, and high hardness reinforcing phase is added to a titanium or titanium alloy matrix. It combines the plastic toughness of the matrix with the high strength and high modulus of the reinforcing phase, so that the titanium-based composite material has higher strength, hardness, and wear resistance than the titanium alloy. Moreover, in the gradient titanium-based material, since the titanium-based composite material and the titanium alloy are homogeneous material matrices, there is a homogeneous interface structure transition between the two, and the bonding strength is high. By designing the gradient transition interface structure and optimizing the molding preparation method, a high-modulus wear-resistant and impact-resistant layer with metallurgical bonding and controllable thickness can be obtained. The use of gradient materials of titanium-based composite materials / titanium alloys can effectively solve the limitations of the performance limits of single homogeneous titanium alloy materials, further improve the service performance of components, and achieve comprehensive optimization of materials and performance at various positions within the components.
[0025] The traditional wear-resistant surface treatment method for titanium alloy components is to perform laser cladding, surface nitriding, vapor deposition, thermal spraying and other treatments after obtaining the forging blank. The wear-resistant coating is at most a hundred microns thick, and the coating is coated on the titanium alloy substrate, forming a heterogeneous interface bond, with weak bonding force, and is prone to peeling and failure during service. The titanium-based composite material layer of the present invention is metallurgically bonded to the titanium alloy substrate, and the titanium-based composite material layer has strong designability, and the thickness, composition, organization and performance are controllable. In addition, since the matrix phase of the titanium-based composite material layer is homogeneous with the titanium alloy substrate and the thermophysical parameters are similar, the forming process is similar. In the subsequent hot forming and heat treatment process of materials and components, the microstructure of the titanium-based composite material layer and the titanium alloy substrate can be coordinated and regulated to improve the interface bonding strength of each layer, which is conducive to the preparation of short-process, high-reliability structural and functional integrated titanium alloy materials and components.
[0026] The present invention starts with regulating the distribution gradient of the titanium-based composite material layer, changes the performance of the titanium-based composite material layer by adding a reinforcing phase, and realizes the performance change of the gradient material by adjusting the distribution of the reinforcing phase, gradually turning from a high-strength and high-toughness titanium alloy to a high-modulus, high-hardness, impact-resistant and wear-resistant titanium-based composite material. In terms of gradient material selection, the materials required at each end are screened according to the performance indicators required by each part of the target component in the actual service environment to ensure that the gradient material meets the performance requirements of each position in the target component. In terms of the structural design of the transition zone, in order to further weaken the step mutation of elements / thermal parameters / phase types / phase content during the transition of the gradient material, 0.5n%-5n% reinforcing phase components are used for step gradient transition to avoid stress concentration and mutation of material parameters. The "cut-and-cut" design of the above-mentioned material can achieve directional regulation of the microstructure by reasonably designing the powder filling mold tooling and the cold and hot isostatic pressing molding methods. This method can ensure a clean interface and avoid the generation of harmful products on the interface.
[0027] The wear-resistant mechanism of the titanium-based composite material layer is that during the high-temperature and high-pressure sintering, hot pressing and hot isostatic pressing processes of the titanium-based composite raw material powder, under the dual effects of powder plastic forming and solid phase diffusion, an in-situ autogenous reaction occurs in the titanium-based composite raw material powder to generate high-hardness and high-modulus TiB and Ti5Si3 ceramic wear-resistant phases, and the added nano-scale Y2O3 phase synergistically strengthens with them to form a high-strength and wear-resistant titanium-based composite material layer, and is metallurgically combined with the titanium alloy substrate. The titanium-based composite material layer and the titanium alloy matrix and each gradient interface all present a homogeneous interface structure transition. The titanium-based composite material layer adjacent to the titanium alloy substrate has the smallest volume fraction of the reinforcing phase and the best interface transition with the titanium alloy substrate, achieving stress buffering. Therefore, it has a very high interface bonding strength, giving the titanium alloy materials and components excellent wear resistance and impact resistance. Compared with the prior art, the added nano-scale Y2O3 particles of the present invention have the characteristics of high melting point and high hardness. Since they are evenly dispersed on the surface of titanium alloy particles, they can play the role of pinning "grain boundaries", limit the growth of titanium alloy grains, and refine the grains; the multi-scale and multi-scale synergistic reinforcement effect of nano-scale Y2O3 particles and micron-scale TiB and micro-nano-scale Ti5Si3 reinforcement phases can further improve the mechanical properties and high-temperature properties of titanium-based composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Schematic diagram of the gradient distribution of the gradient titanium-based rod composition along the longitudinal section in Example 1.
[0029] Figure 2 Schematic diagram of the titanium alloy balance elbow component in Example 1.
[0030] Figure 3 The hardness change of the gradient transition titanium-based rod component in Example 1.
[0031] Figure 4 This is the interface microstructure of the wear-resistant layer of the titanium-based composite material and the titanium alloy balance elbow in Example 1.
[0032] Figure 5 This is the gradient titanium-based gear component in Example 2.
[0033] Figure 6 This is the gradient titanium-based composite armor plate in Example 3, (a) the macroscopic morphology and dimensions of the armor plate, and (b) a schematic diagram of the cross-sectional morphology and dimensions of the armor plate. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below with specific examples, but the present invention is not limited to the following specific examples. Example
[0035] The preparation method of the gradient TC18 titanium-based bar balanced elbow component of this embodiment comprises the following steps:
[0036] Step 1: According to the technical requirements of the titanium-based bar balanced elbow component, select TC18 titanium alloy bars that meet the performance requirements and have qualified chemical composition. According to the size of the titanium-based bar balanced elbow component, calculate the specifications of the TC18 titanium alloy bars, and perform cutting and end chamfering.
[0037] Step 2: Design the number of titanium-based composite wear-resistant layers with step gradient transition on the surface of TC18 titanium alloy rod and the composition of each layer. The titanium-based composite wear-resistant layer adjacent to the titanium alloy rod is the first layer. Design 4 layers of step gradient transition layers, each with a thickness of (2±0.5) mm. The composition of the 1st to 4th titanium-based composite wear-resistant layers, that is, the composition of the 1st to 4th titanium-based composite materials, are: 1 vol.% (TiB+Y2O3+Ti5Si3) / TC18, 2 vol.% (TiB+Y2O3+Ti5Si3) / TC18, 3 vol.% (TiB+Y2O3+Ti5Si3) / TC18 and 4 vol.% (TiB+Y2O3+Ti5Si3) / TC18. The schematic diagram of the gradient distribution of the gradient titanium-based rod composition along the longitudinal section is shown in Figure 1 As shown. According to the designed titanium-based composite material wear-resistant layer composition, the raw material powders of the reinforcement phase are selected as Si, Y2O3 and TiB2, among which the average particle size of Si and TiB2 is 3μm, the average particle size of Y2O3 is 100nm, the average particle size of TC18 titanium alloy powder is 70μm, and the raw material ratio of the reinforcement phase (TiB+Y2O3+Ti5Si3) is prepared according to the volume fraction TiB:Y2O3:Ti5Si3=3:0.5:0.5;
[0038] The mixed powders were milled in a planetary ball mill with a milling time of 4 h, a milling speed of 150 rpm, a ball-to-material ratio of 5:1, and argon atmosphere protection to obtain titanium-based powders with different compositions.
[0039] Step 3: Design a 4-layer gradient titanium-based rod powder filling mold and tooling, mainly a steel chassis with partition slots placed at the bottom of the rubber sleeve, the slots are distributed in concentric circles, and there are 3 concentric circle slots in total; roll the 0.2mm thick aluminum foil into a cylinder and insert it into the chassis slot for fixing. Polish the surface of the TC18 titanium alloy rod and put it in the center of the powder filling mold. Correspondingly, fill the titanium-based powder in each interlayer step by step. After filling the powder, seal the sleeve. Then perform cold isostatic preforming on the sealed sleeve. At room temperature, use liquid as the pressure medium, the pressure is 400MPa, and the holding time is 1min to obtain the gradient TC18 titanium-based material preform.
[0040] Step 4: Remove the aluminum foil separator from the prefabricated blank, seal the blank with a steel sheath, and perform hot isostatic pressing and densification molding on it at a heating temperature of 1200°C, a holding time of 3 hours, a pressure of 140 MPa, and a vacuum environment. Obtain the gradient TC18 titanium-based rod and remove the sheath.
[0041] Step 5: The gradient TC18 titanium-based bar is die forged, the heating temperature is 840°C, the holding time is 4h, the forging temperature is 840°C, free forging and three-fire die forging are performed to form a gradient titanium-based balanced elbow forging blank.
[0042] Step 6: Double annealing treatment is performed on the forging blank, the first solution temperature is 840℃, the solution time is 3h, the second solution temperature is cooled to 750℃ with the furnace, kept for 3h, and air-cooled; then heated to 650℃, kept for 4h, and air-cooled; then fine mechanical processing is performed to obtain a high-strength, impact-resistant and wear-resistant TC18 titanium alloy balance elbow component. The schematic diagram of the balance elbow component is shown in Figure 2 shown.
[0043] The mechanical properties of the gradient TC18 titanium-based bar balance elbow component are as follows: the core titanium alloy part: tensile strength R m The yield strength is 1210MPa and R p0.2 is 1130MPa, the elongation after fracture A5 is 17%, and the fracture toughness K IC 43 MPa·m 1 / 2 , impact toughness α KU :380 KJ / m 2 , hardness: 35HRC; the hardness of the outermost titanium-based composite material wear-resistant layer is 55HRC, and the hardness change diagram of the gradient TC18 titanium-based rod component is as follows Figure 3 The microstructure of the interface between the wear-resistant layer of the titanium-based composite material and the titanium alloy balance elbow is shown in Figure 4shown. Example
[0044] The method for preparing the gradient transition TC11 titanium-based gear component of this embodiment comprises the following steps:
[0045] Step 1: According to the technical requirements and shape and size characteristics of titanium alloy gears, select TC11 titanium alloy bars that meet the performance requirements and have qualified chemical composition. According to the gear size, calculate the specifications of TC11 titanium alloy bars, and perform cutting and end chamfering.
[0046] Step 2: Design the composition of each layer of the titanium-based composite wear-resistant layer with a step-gradient transition on the surface of the TC11 titanium alloy rod. The titanium-based composite wear-resistant layer adjacent to the titanium alloy rod is the first layer. Design three layers of step-gradient transition layers, each with a thickness of (1±0.2) mm. The compositions of the 1st to 3rd titanium-based composite wear-resistant layers are: 2 vol.% (TiB+Y2O3+Ti5Si3) / TC11, 4 vol.% (TiB+Y2O3+Ti5Si3) / TC11, and 6 vol.% (TiB+Y2O3+Ti5Si3) / TC11. According to the designed titanium-based composite material wear-resistant layer composition, the raw material powders of the reinforcing phase are selected as Si, Y2O3 and TiB2, wherein the average particle size of Si and TiB2 is 5μm, the average particle size of Y2O3 is 100nm, the average particle size of TC11 titanium alloy powder is 150μm, and the raw material ratio of the reinforcing phase (TiB+Y2O3+Ti5Si3) is prepared according to the volume fraction TiB:Y2O3:Ti5Si3=2:0.2:0.2;
[0047] The mixed powders were milled in a planetary ball mill with a milling time of 6 h, a milling speed of 200 rpm, a ball-to-material ratio of 6:1, and argon atmosphere protection to obtain titanium-based powders with different compositions.
[0048] Step 3: Design a three-layer gradient titanium-based rod powder filling mold and tooling, mainly a steel chassis with a separation slot placed at the bottom of the rubber sleeve, the slots are distributed in concentric circles, and there are 2 concentric circle slots in total; roll a 0.5mm thick aluminum foil into a cylinder and insert it into the chassis slot for fixing. Polish the surface of the TC11 titanium alloy rod and put it in the center of the powder filling mold. Correspondingly, fill each interlayer with wear-resistant titanium-based powder in steps. After filling the powder, seal the sleeve. Then perform cold isostatic preforming on the sealed sleeve. At room temperature, use liquid as the pressure medium, the pressure is 430MPa, and the holding time is 1.5min to obtain a gradient TC11 titanium-based rod preform.
[0049] Step 4: Remove the aluminum foil separator from the prefabricated blank, seal the blank with a steel sheath, and perform vacuum hot pressing sintering at a heating temperature of 1150°C, a holding time of 4 hours, a pressure of 30 MPa, and a vacuum environment. Obtain a step-gradient TC11 titanium-based bar and remove the sheath.
[0050] Step 5: The gradient TC11 titanium-based rod is extruded, the heating temperature is 980°C, the holding time is 4 hours, the extrusion temperature is 980°C, and the gradient TC11 titanium-based extruded rod is obtained.
[0051] Step 6: Heat treat the extruded blank with a solution temperature of 950°C, a solution time of 2 hours, and air cooling; then heat to 530°C, keep warm for 6 hours, and air cool; then perform fine mechanical processing to obtain high-strength, tough, and wear-resistant TC11 titanium alloy gear parts, such as Figure 5 shown.
[0052] The mechanical properties of the gradient TC11 titanium-based gear parts are as follows: the core titanium alloy part: tensile strength R m 1100MPa, yield strength R p0.2 990MPa, elongation after fracture A5 is 15%, fracture toughness K IC 83 MPa·m 1 / 2 , impact toughness α KU :430 KJ / m 2 , hardness: 34HRC; the hardness of the outermost titanium-based composite material wear-resistant layer is 58HRC. Example
[0053] The preparation method of the gradient TC4 titanium-based composite armor of this embodiment comprises the following steps:
[0054] Step 1: According to the technical requirements and shape and size characteristics of titanium-based composite armor, select TC4 titanium alloy plates that meet the performance requirements and have qualified chemical composition. According to the size of the composite armor, calculate the specifications of the TC4 titanium alloy plates, and perform cutting and end chamfering.
[0055] Step 2: Design the composition of each layer of the titanium-based composite material layer with a step-gradient transition on the surface of the TC4 titanium alloy plate. The titanium-based composite material layer adjacent to the titanium alloy plate is the first layer. Design two layers of step-gradient transition layers, each with a thickness of (5±0.2) mm. The compositions of the first and second layers of titanium-based composite materials are 3 vol.% (TiB+Y2O3+Ti5Si3) / TC4 and 6 vol.% (TiB+Y2O3+Ti5Si3) / TC4, respectively.
[0056] According to the designed titanium-based composite material layer composition, the raw material powders of the reinforcement phase are selected as Si, Y2O3 and TiB2, wherein the average particle size of Si and TiB2 is 3μm, the average particle size of Y2O3 is 100nm, the average particle size of TC11 titanium alloy powder is 200μm, and the raw material ratio of the reinforcement phase (TiB+Y2O3+Ti5Si3) is prepared according to the volume fraction TiB:Y2O3:Ti5Si3=5:1:1;
[0057] The mixed powders were milled in a planetary ball mill with a milling time of 5 h, a milling speed of 150 rpm, a ball-to-material ratio of 5:1, and argon atmosphere protection to obtain titanium-based powders with different compositions.
[0058] Step 3: Design a two-layer gradient titanium-based sheet powder filling mold and tooling, make a steel rectangular mold according to the size of the titanium-based composite armor, place the titanium alloy sheet at the bottom, spread the first layer of titanium-based powder on the titanium alloy sheet, and then place a 1mm thick titanium foil as a partition layer, spread the second layer of titanium-based powder, and finally fix it with a 10mm thick steel plate; use a hydraulic press to cold press it with a pressure of 60MPa and a holding time of 5min to obtain a gradient TC4 titanium-based sheet prefabricated blank.
[0059] Step 4: The prefabricated blank is sealed with a steel sheath and hot isostatically pressed at a heating temperature of 1200°C, a holding time of 4 hours, a pressure of 130 MPa, and a vacuum environment. The step-gradient TC4 titanium-based sheet is obtained, and the sheath and steel sheet layer are removed.
[0060] Step 5: The gradient TC4 titanium-based sheet is rolled into shape, with a heating temperature of 940°C, a heat preservation time of 3 hours, and a rolling temperature of 940°C to obtain a gradient TC4 titanium-based sheet.
[0061] Step 6: Heat treatment of the gradient titanium-based plate, solution temperature of 920°C, solution time of 2h, water quenching; then heating to 580°C, keeping temperature for 4h, air cooling; and then mechanical fine processing to obtain impact-resistant gradient TC4 titanium-based composite armor plate, such as Figure 6 shown.
[0062] The mechanical properties of the gradient TC4 titanium-based composite armor plate are as follows: the tensile strength of the titanium alloy layer R m 950MPa, yield strength R p0.2 The hardness of the outermost titanium-based composite material impact-resistant layer is 57HRC.
[0063] The above are only examples of the features of the present invention and do not constitute any limitation on the protection scope of the present invention. Any technical solution formed by equivalent exchange or equivalent replacement falls within the protection scope of the present invention.
Claims
1. A gradient titanium-based material, characterized in that: A plurality of titanium-based composite material layers are stacked on the surface of a titanium alloy substrate, wherein the titanium-based composite material layers include a matrix phase and a reinforcement phase; the composition of the matrix phase is the same as that of the titanium alloy substrate; the volume fraction of the reinforcement phase in each titanium-based composite material layer is distributed in a step gradient, and the volume fraction of the reinforcement phase in the nth titanium-based composite material layer is 0.5n%-5n%, n≥1, and n is an integer; When n=1, it represents the first layer adjacent to the titanium alloy substrate, and when n=2, it represents the second layer adjacent to the first layer; and so on; The thickness of the titanium-based composite material layer is 0.2-10 mm; The reinforcement phase is TiB whiskers with a size of 5-20 μm, Y2O3 with a grain size of 50-100 nm, and Ti5Si3 reinforcement phases, wherein the volume fraction ratio of TiB, Y2O3 and Ti5Si3 is (2-5): (0.2-1): (0.2-1).
2. A method for preparing the gradient titanium-based material according to claim 1, characterized in that: The following steps are involved: 1) designing a mold to surround the titanium alloy substrate and fill the powder raw materials of the multi-layer titanium-based composite material layer; and using a cold pressing preforming method to complete the prefabrication of the blank; 2) The prefabricated blank is subjected to vacuum hot pressing sintering or hot isostatic pressing densification forming, and then subjected to rolling, extrusion or forging forming processing, and finally subjected to heat treatment to obtain a gradient titanium-based material.
3. The method for preparing a gradient titanium-based material according to claim 2, characterized in that: In step 1), the powder raw materials of the titanium-based composite material layer include a matrix phase raw material and a reinforcement phase raw material; the reinforcement phase raw material is a mixture of multiple powders of Si, Y2O3 and TiB2, wherein the average particle size of Si and TiB2 is 1-10μm, and the average particle size of Y2O3 is 50-100nm; the matrix phase raw material is a titanium alloy powder with the same composition as the titanium alloy substrate, with an average particle size of 13-250μm, and the powder morphology is spherical or irregular.
4. The method for preparing a gradient titanium-based material according to claim 3, characterized in that: In step 1), the temperature of the cold pressing preforming is room temperature, the pressure is 60-600 MPa, and the holding time is 0.5-15 min.
5. The method for preparing a gradient titanium-based material according to claim 4, characterized in that: In step 2), the heating temperature of the vacuum hot pressing sintering or hot isostatic pressing densification molding is 1000-1300°C, the holding time is 1.5-6h, the hot isostatic pressing pressure is 100-240MPa, and the vacuum hot pressing sintering pressure is 20-40MPa.
6. The method for preparing a gradient titanium-based material according to claim 2, characterized in that: In step 2), the heating temperature of the rolling, extrusion or forging forming process is 820-1050°C, the insulation time is 3-6h, the deformation temperature is 820-1050°C, and the surface is sprayed with glass lubricant for anti-oxidation treatment before heating and deformation; in step 2), the heat treatment process is a solution temperature of 740-950°C and a solution time of 1-6h; then heated to 500-650°C, kept for 2-6h, and air cooled.
7. A method for preparing a balanced elbow component using the gradient titanium-based material according to claim 1, characterized in that: The steps include: 1) According to the technical requirements of the balancing elbow component, select TC18 titanium alloy bars that meet the performance requirements and have qualified chemical composition, calculate the specifications of the TC18 titanium alloy bars according to the size of the balancing elbow component, and perform cutting and end chamfering; 2) Design the number of titanium-based composite material layers and the composition of each layer for the step-gradient transition on the surface of TC18 titanium alloy rod: the titanium-based composite material layer adjacent to the titanium alloy rod is the first layer, and 4 layers of step-gradient transition layers are designed, each with a thickness of 2 mm. The compositions of the 1st to 4th layers of titanium-based composite materials are: 1 vol.% (TiB+Y2O3+Ti5Si3) / TC18, 2 vol.% (TiB+Y2O3+Ti5Si3) / TC18, 3 vol.% (TiB+Y2O3+Ti5Si3) / TC18 and 4vol.% (TiB+Y2O3+Ti5Si3) / TC18, raw material powders are selected according to the designed titanium-based composite material layer composition; the raw material powders of the reinforcing phase are Si, Y2O3 and TiB2, wherein the average particle size of Si and TiB2 is 3μm, the average particle size of Y2O3 is 100nm, the average particle size of TC18 titanium alloy powder is 70μm, and the raw material ratio of the reinforcing phase (TiB+Y2O3+Ti5Si3) is prepared according to the volume fraction TiB:Y2O3:Ti5Si3=3:0.5:0.5; 3) Design a 4-layer gradient titanium-based rod powder filling mold: the structure is that a steel chassis with partition slots is placed at the bottom of the rubber sleeve, and the slots are distributed in concentric circles, with a total of 3 concentric circle slots; 0.2mm thick aluminum foil is rolled into a cylinder and inserted into the chassis slot for fixation; the surface of the TC18 titanium alloy rod is polished and placed in the center of the powder filling mold, and accordingly, titanium-based powder is filled in each interlayer step by step. After filling the powder, the sleeve is sealed; then cold isostatic pressing is performed for preforming, at room temperature, with liquid as the pressure medium, the pressure is 400MPa, and the pressure holding time is 1min to obtain a gradient TC18 titanium-based material prefabricated blank; 4) taking out the aluminum foil separator from the prefabricated blank, sealing the blank with a steel sheath, and performing hot isostatic pressing densification molding on the blank at a heating temperature of 1200° C., a holding time of 3 h, a pressure of 140 MPa, and a vacuum environment; obtaining a gradient TC18 titanium-based rod, and removing the sheath; 5) The gradient TC18 titanium-based bar is die-forged at a heating temperature of 840° C., a holding time of 4 h, and a forging temperature of 840° C. to obtain a forging blank; 6) The forging blank is subjected to double annealing treatment, with the first solution temperature being 840°C and the solution time being 3h. The second solution temperature is furnace cooled to 750°C, kept at this temperature for 3h, and air cooled. It is then heated to 650°C, kept at this temperature for 4h, and air cooled. It is then subjected to mechanical fine processing to obtain a TC18 titanium alloy balance elbow component.