Intragranular precipitation reinforced heterostructure titanium-based composite material and preparation method thereof

Magneto-controlled sputtering and ball milling technology form a heterostructure strengthened intra-crystal nanophase precipitation and strengthening, which solves the problem of insufficient strength and plastic matching of Ti-6Al-4V alloy materials, and achieves high strength and excellent uniform elongation and post-break extension Rate.

CN119061281APending Publication Date: 2024-12-03NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411264388.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The grain size of traditional Ti-6Al-4V alloy materials is large, resulting in low plasticity and toughness of the material, and low composition uniformity. Mechanical properties and plasticity matching need to be improved. Existing improved methods such as alloy element addition and surface treatment There are limitations and it is difficult to achieve comprehensive optimization of material properties.

Method used

Magnetic sputtering is used to coat the surface of the titanium-based prealloy powder with uniform and dense metal film layer, and mixed with the unmodified titanium-based prealloy powder ball mill, and then quickly densified sintering and thermal deformation processing to form an intra-crystal nanophase. Precipitate the reinforced heterostructure to improve the strength and elongation of the material.

Benefits of technology

The strength and plastic matching of titanium-based composite materials are significantly improved, and the in-crystal precipitation reinforced heterostructure with high uniform elongation and post-break elongation is obtained, which solves the problem of low material strength and low uniform elongation, and achieves excellent strength. Plastic matching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061281A_ABST
    Figure CN119061281A_ABST
Patent Text Reader

Abstract

The invention discloses an intragranular precipitation strengthened heterostructure titanium-based composite material and a preparation method thereof, and the method comprises the following steps: step 1, plating a uniform and compact metal film layer on the surface of titanium-based pre-alloy powder by adopting a magnetron sputtering method for modification, carrying out ball milling and uniform mixing on the modified titanium-based pre-alloy powder and unmodified titanium-based pre-alloy powder to obtain heterogeneous composite powder; and secondly, the heterogeneous composite powder is subjected to densification sintering, an intragranular precipitation strengthened titanium alloy blank is obtained, and then the titanium-based composite material with the intragranular precipitation strengthened heterostructure is obtained through deformation machining. In the sintering process, metal film layer elements are rapidly diffused inwards to form a precipitated phase, the volume fraction of a beta phase is increased, the plasticity of a titanium matrix is improved, the rapid eutectoid reaction is beneficial for refining the alpha / beta lamellar size and improving the strength and plasticity, and the structure characteristics of an intragranular precipitation strengthened heterostructure are obtained; the high-strength and high-uniform-elongation titanium-based composite material can be suitable for the fields of spaceflight, wear resistance, corrosion resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal material strengthening and toughening design, and specifically relates to an intracrystalline precipitation strengthened heterogeneous structure titanium-based composite material and a preparation method thereof. Background Art

[0002] Ti-6Al-4V (TC4) alloy has excellent mechanical properties, corrosion resistance and high temperature stability, and is widely used in aerospace, automobile manufacturing and medical equipment. However, there are some problems with the traditional TC4 material prepared by simple smelting. First, due to its large grain size, the plasticity and toughness of the material are low. Secondly, due to the low composition uniformity of TC4 material, the mechanical properties and plastic matching of the material need to be improved. Therefore, researchers have been committed to finding ways to improve the mechanical properties and plastic matching of TC4 materials.

[0003] A common method is to improve the properties of TC4 materials by adding trace amounts of alloying elements. For example, by adding elements such as vanadium (V) and iron (Fe), the strength and plasticity of TC4 materials can be improved. However, this method has some disadvantages, such as the limited amount of alloying elements added, making it difficult to further optimize material properties.

[0004] Another method is to improve the performance of TC4 materials through surface treatment. For example, by forming a copper layer on the surface of TC4 materials, the strength and plasticity of the material can be improved. The copper layer can provide a good bonding interface, refine the grains of TC4 materials, and thus improve the plasticity and toughness of the material. However, there are some problems with traditional surface treatment methods, such as the low uniformity of the copper layer, which makes it difficult to achieve comprehensive improvement of the material.

[0005] Therefore, a new method is needed to prepare TC4 materials with heterogeneous structures to further improve their mechanical properties and plastic matching. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing a titanium-based composite material with an intracrystalline precipitation-strengthened heterogeneous structure in view of the above-mentioned deficiencies of the prior art. The method uses magnetron sputtering to modify the surface of titanium-based pre-alloyed powder, and mixes it with unmodified titanium-based pre-alloyed powder by ball milling, and obtains a titanium-based composite material with an intracrystalline nanophase precipitation-strengthened heterogeneous structure through rapid densification sintering and thermal deformation processing, thereby improving the strength and elongation of the titanium-based composite material, and solving the problem that the titanium alloy material prepared by the prior art has low strength and low uniform elongation.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing an intracrystalline precipitation-strengthened heterogeneous structure titanium-based composite material, characterized in that the method comprises the following steps:

[0008] Step 1: Surface modification of titanium-based pre-alloyed powder and preparation of heterogeneous composite powder: a uniform and dense metal film layer is coated on the surface of the titanium-based pre-alloyed powder by magnetron sputtering to modify the powder, and then the modified titanium-based pre-alloyed powder and the unmodified titanium-based pre-alloyed powder are ball-milled and mixed to obtain a heterogeneous composite powder;

[0009] Step 2: Composite material forming: The heterogeneous composite powder obtained in step 1 is subjected to rapid densification sintering to obtain an intragranular precipitation-strengthened titanium alloy billet, which is then subjected to hot deformation processing to obtain an intragranular precipitation-strengthened heterogeneous structure titanium-based composite material.

[0010] The present invention firstly adopts a magnetron sputtering method to modify the surface of a titanium-based pre-alloyed powder, deposits a metal film layer with controllable thickness and uniform and dense on the surface of the titanium-based pre-alloyed powder, then uniformly mixes the modified titanium-based pre-alloyed powder with an unmodified titanium-based pre-alloyed powder by ball milling to obtain a heterogeneous composite powder, and then undergoes rapid densification sintering to obtain a heterogeneous structure titanium alloy blank having an original titanium alloy structure and an intracrystalline precipitation-strengthened titanium alloy structure. On the basis of maintaining the excellent properties of the titanium-based material, the mechanical properties and plastic matching of the material are improved, that is, the material has better high-strength and high-plastic properties. The precipitation phase size is further regulated by deformation processing to improve the mechanical properties, so that the material has better strength and plastic matching, and the intracrystalline precipitation-strengthened heterogeneous structure titanium-based composite material with high uniform elongation and elongation after fracture is obtained.

[0011] In the preparation process of the present invention, titanium-based pre-alloyed powder with high sphericity is usually selected, on the one hand, to ensure that all titanium-based pre-alloyed powders can be evenly plated during magnetron sputtering, and on the other hand, to ensure that a single titanium-based pre-alloyed powder is fully rotated to form a uniform and well-bonded metal film layer after plating, and the metal film layer will not fall off or adhere to the surface of the unmodified titanium-based pre-alloyed powder in the subsequent process. At the same time, the present invention usually adopts low-energy ball milling to mix the modified titanium-based pre-alloyed powder with the unmodified titanium-based pre-alloyed powder for a short time, on the one hand, to ensure the full mixing of the two powders, and on the other hand, the low-energy and short-time mixing ensures that the metal film layer on the surface of the modified titanium-based pre-alloyed powder will not be squeezed and deformed to cause unevenness, and also avoids the metal film layer adhering to the surface of the unmodified titanium-based pre-alloyed powder, so that the subsequent sintering structure cannot achieve a heterogeneous effect.

[0012] During the rapid densification sintering process, since the metal elements in the metal film layer do not have time to fully diffuse and homogenize between the grains, some of the metal elements on the surface of the modified titanium-based pre-alloyed powder diffuse inward during the sintering process and precipitate nanophases in the grains, which not only increases the volume fraction of the β phase, which is beneficial to improving the plasticity of the titanium matrix, but also its fast eutectoid reaction is beneficial to refining the size of the α / β sheet, while improving the strength and plasticity; at the same time, the structure of the unmodified titanium-based pre-alloyed powder in the heterogeneous composite powder after sintering is the Widmanstatten structure, which ensures that during plastic deformation, due to the different phases and grains in the heterogeneous structure, a variety of coordinated deformations are provided, thereby increasing the plasticity of the titanium-based composite material. On the other hand, a large number of geometrically necessary dislocations are generated near the soft phase region at the soft / hard interface in the heterogeneous structure composite material, thereby forming strain gradients and stress gradients, and producing a significant back stress strengthening effect; at the same time, the continuous accumulation of geometrically necessary dislocations at the soft and hard interface also increases the work hardening ability during the tensile process, so that the heterogeneous structure titanium-based composite material maintains high tensile plasticity.

[0013] The subsequent hot deformation processing in the present invention will further refine the intracrystalline α grain size, refine the matrix structure, and improve the material density. As the degree of deformation increases, the dislocation density in the material continues to rise, and when the dislocation moves, it is easy to form obstacles such as dislocation accumulation groups and steps, which hinder the further movement of the dislocation, cause an increase in deformation resistance, and improve the strength of the material. Under the action of multiple strengthening mechanisms, the present invention finally obtains a titanium-based composite material with high strength and high uniform elongation.

[0014] In summary, the present invention performs surface modification on titanium-based pre-alloyed powder by magnetron sputtering, and then mixes it with unmodified titanium-based pre-alloyed powder by ball milling, thereby improving the bonding strength between the two and improving the dispersion uniformity. After rapid densification sintering, the metal film layer elements on the surface of the modified titanium-based pre-alloyed powder are diffused and maintained within a grain, forming a heterogeneous structure in the titanium matrix to strengthen the material, increase the plasticity of the material, and combine hot deformation processing to regulate the microstructure and mechanical properties, further improve the mechanical properties of the material, and make it have an excellent level of strength-plasticity matching.

[0015] The method for preparing the above-mentioned intracrystalline precipitation strengthened heterogeneous structure titanium-based composite material is characterized in that the titanium-based pre-alloyed powder in step 1 is prepared by a plasma rotating electrode method, the powder has good sphericity, no planetary powder, the powder particle size is 15μm to 53μm, and the chemical composition conforms to GB / T3620.1-2007 "Titanium and Titanium Alloy Grades and Chemical Compositions". Preferably, the titanium-based pre-alloyed powder is selected from TC4 titanium alloy powder.

[0016] The method for preparing the above-mentioned intracrystalline precipitation-strengthened heterostructure titanium-based composite material is characterized in that the component of the metal film layer in step one is metallic copper. The present invention preferably uses β-stabilizing element copper. The soft phase metallic copper has good wettability with titanium, and is easy to be evenly coated on its surface. After sintering, a nano-precipitated phase is precipitated in the crystal, which plays a strengthening role. In this way, the introduction of unmodified titanium alloy can exert the soft-hard interface strengthening effect. Usually, the thickness of the metal film layer is at the micron level, preferably not more than 10μm, to avoid cracking. The size and amount of the precipitated phase are controlled by the metal film layer, and the performance of the titanium-based composite material is regulated.

[0017] The above-mentioned method for preparing the intracrystalline precipitation strengthened heterostructure titanium-based composite material is characterized in that the metal target material used in the magnetron sputtering method in step 1 has a mass purity of 99.995%.

[0018] The above-mentioned method for preparing the intracrystalline precipitation strengthened heterostructure titanium-based composite material is characterized in that the coating power used in the magnetron sputtering method in step 1 is 100W, the sputtering bias is 0V, and the vacuum degree is 6×10 -3 Pa, argon protective atmosphere is introduced, and the coating time is 2h to 4h. The thickness and uniformity of the metal film layer can be controlled by controlling the process parameters of magnetron sputtering coating.

[0019] The method for preparing the intracrystalline precipitation strengthened heterogeneous structure titanium-based composite material is characterized in that the ball milling speed in step 1 is 150 r / min to 250 r / min, the ball milling time is 1 h to 2 h, and the ball-to-material ratio is 5: 1. The ball milling conditions not only make the two powders mix evenly, but also ensure the spherical morphology of the two powders to the greatest extent.

[0020] The above-mentioned method for preparing the intracrystalline precipitation-strengthened heterogeneous structure titanium-based composite material is characterized in that the rapid densification sintering described in step 2 is plasma sintering, and the temperature of plasma sintering is 800°C to 1100°C, the heating rate is 100°C / min, the holding time is 5min to 10min, and the pressure is 30MPa to 60MPa. The preferred densification sintering method and process parameters of the present invention are conducive to the metal film layer elements on the surface of the modified titanium-based pre-alloyed powder not having time to homogenize and quickly diffuse into the crystal, reacting with the titanium matrix to generate nano-precipitation phase in situ, and further improving the density of the material, improving the sintered structure of the titanium matrix, and optimizing its mechanical properties. Generally, it is preferred to use SPS equipment to achieve rapid sintering at high temperature in a short time to improve production efficiency.

[0021] The above-mentioned method for preparing the intracrystalline precipitation strengthened heterostructure titanium-based composite material is characterized in that the thermal deformation processing in step 2 is rolling, and the rolling temperature is 800°C to 1000°C, the insulation time is 10min to 30min, and the total rolling deformation is 50% to 90%.

[0022] At the same time, the invention also discloses an intracrystalline precipitation-reinforced heterogeneous structure titanium-based composite material prepared by the above method.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] 1. Compared with the method of introducing metal particles or nanolayers on the surface of titanium-based pre-alloyed powder by ball milling or chemical plating, the present invention adopts a magnetron sputtering method to introduce a metal film layer, which not only realizes the controllable thickness, density and uniformity of the metal film layer, but also significantly improves the interface bonding strength between the metal film layer and the titanium-based pre-alloyed powder through the layer-by-layer accumulation and physical deposition of metal atoms in the sputtering layer, thereby avoiding the undesirable phenomena such as the metal film layer falling off or the metal film layer adhering to the surface of the unmodified titanium-based pre-alloyed powder during the subsequent ball milling process.

[0025] 2. The present invention ball-mills and mixes the modified titanium-based pre-alloyed powder coated with a metal film layer with the unmodified titanium-based pre-alloyed powder, and then densifies and sinters them, so that the elements of the metal film layer diffuse rapidly inward to form a precipitated phase, which not only increases the volume fraction of the β phase and is beneficial to improving the plasticity of the titanium matrix, but also its fast eutectoid reaction is beneficial to refining the size of the α / β lamellae, improving the strength and plasticity. The unmodified titanium-based pre-alloyed powder forms a coarse Widmanstätten lamellae structure after sintering, thereby obtaining the organizational characteristics of the intracrystalline precipitation-strengthened heterogeneous structure, and obtaining a titanium-based composite material with high strength and high uniform elongation.

[0026] 3. The present invention performs hot deformation processing on a titanium alloy billet having an intragranular precipitation strengthened heterogeneous structure, further regulates the microstructure and mechanical properties, exerts a variety of strengthening factors, and utilizes different phases and grains in the heterogeneous structure to provide a variety of coordinated deformations, thereby improving the strength and plasticity of the titanium-based composite material.

[0027] 4. In the heterogeneous structure composite material of the present invention, a large number of geometric dislocations are accumulated near the soft phase at the soft / hard interface, thereby forming strain gradients and stress gradients, producing a significant back stress strengthening effect; at the same time, the continuous accumulation of geometric dislocations at the soft and hard interface also increases the work hardening ability during the stretching process, so that the heterogeneous structure titanium-based composite material maintains high tensile plasticity.

[0028] 5. The present invention combines the precipitation strengthening of metal materials with the configuration design ideas of metal-based composite materials, thereby achieving an improvement in the strength and plasticity of titanium-based composite materials and a good match between the two. The process is simple, efficient and controllable, and has good application prospects.

[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a SEM image of the TC4 alloy powder with a surface coated with a copper film prepared in Example 1 of the present invention.

[0031] Figure 2 This is a distribution diagram of Cu elements at the interface of the TC4 alloy powder with a surface-coated copper film prepared in Example 1 of the present invention.

[0032] Figure 3 This is a SEM image of the titanium-based composite material prepared in Example 1 of the present invention.

[0033] Figure 4 This is a performance comparison chart of the titanium-based composite materials prepared in Examples 3 to 5 of the present invention and the titanium alloy materials prepared in Comparative Examples 1 to 2. DETAILED DESCRIPTION

[0034] Example 1

[0035] This embodiment includes the following steps:

[0036] Step 1, surface modification of titanium-based pre-alloyed powder and preparation of heterogeneous composite powder: 60 g of TC4 titanium alloy powder was placed in an ion plating machine, and a magnetron sputtering method was used for plating for 4 hours, and a uniform and dense copper film was plated on the surface of the TC4 titanium alloy powder for modification, and then the modified TC4 titanium alloy powder and 60 g of unmodified TC4 titanium alloy powder were placed in a ball mill together, and ball milled for 1 hour at a rotation speed of 150 r / min and a ball-to-material ratio of 5:1 to obtain a heterogeneous composite powder;

[0037] The TC4 titanium alloy powder is prepared by a plasma rotating electrode method, has good powder sphericity, no planetary powder, a powder particle size of 15 μm to 53 μm, and a chemical composition that complies with GB / T 3620.1-2007 "Titanium and Titanium Alloy Grades and Chemical Compositions";

[0038] The copper target material used in the magnetron sputtering method has a mass purity of 99.995%; the coating power used in the magnetron sputtering method is 100W, the sputtering bias voltage is 0V, and the vacuum degree is 6×10 -3 Pa, argon protective atmosphere is introduced;

[0039] Step 2, composite material forming: plasma sintering the heterogeneous composite powder obtained in step 1 to obtain an intracrystalline precipitation-strengthened titanium alloy billet, and then hot deformation processing to obtain an intracrystalline precipitation-strengthened heterogeneous structure titanium-based composite material; the plasma sintering temperature is 1000°C, the heating rate is 100°C / min, the holding time is 5min, and the pressure is 40MPa; the hot deformation processing is rolling, and the rolling temperature is 900°C, the holding time is 20min, and the total rolling deformation is 75%.

[0040] Figure 1 is a SEM image of the TC4 alloy powder with a copper film plated on the surface prepared in this embodiment, Figure 2 The Cu element distribution diagram of the interface of the TC4 alloy powder with copper film on the surface prepared in this embodiment is shown in FIG. Figure 1 and Figure 2 It can be seen that the surface of the TC4 alloy powder is covered with a micron-sized copper film layer with uniform thickness, and the copper film layer has a high density.

[0041] Figure 3 This is the SEM image of the titanium-based composite material prepared in this embodiment. Figure 3 It can be seen that the titanium-based composite material has an obvious heterogeneous structure.

[0042] Example 2

[0043] This embodiment includes the following steps:

[0044] Step 1, surface modification of titanium-based pre-alloyed powder and preparation of heterogeneous composite powder: 60 g of TC4 titanium alloy powder was placed in an ion plating machine, and a magnetron sputtering method was used for plating for 4 hours, and a uniform and dense copper film was plated on the surface of the TC4 titanium alloy powder for modification, and then 12 g of the modified TC4 titanium alloy powder and 108 g of the unmodified TC4 titanium alloy powder were placed in a ball mill together, and ball milled for 1 hour at a rotation speed of 200 r / min and a ball-to-material ratio of 5:1 to obtain a heterogeneous composite powder;

[0045] The TC4 titanium alloy powder is prepared by a plasma rotating electrode method, has good powder sphericity, no planetary powder, a powder particle size of 15 μm to 53 μm, and a chemical composition that complies with GB / T 3620.1-2007 "Titanium and Titanium Alloy Grades and Chemical Compositions";

[0046] The copper target material used in the magnetron sputtering method has a mass purity of 99.995%; the coating power used in the magnetron sputtering method is 100W, the sputtering bias voltage is 0V, and the vacuum degree is 6×10 -3 Pa, argon protective atmosphere is introduced;

[0047] Step 2, composite material forming: plasma sintering the heterogeneous composite powder obtained in step 1 to obtain an intracrystalline precipitation-strengthened titanium alloy billet, and then hot deformation processing to obtain an intracrystalline precipitation-strengthened heterogeneous structure titanium-based composite material; the plasma sintering temperature is 1000°C, the heating rate is 100°C / min, the holding time is 5min, and the pressure is 40MPa; the hot deformation processing is rolling, and the rolling temperature is 900°C, the holding time is 20min, and the total rolling deformation is 75%.

[0048] Example 3

[0049] This embodiment includes the following steps:

[0050] Step 1, surface modification of titanium-based pre-alloyed powder and preparation of heterogeneous composite powder: 60 g of TC4 titanium alloy powder was placed in an ion plating machine, and a magnetron sputtering method was used for plating for 4 hours, and a uniform and dense copper film was plated on the surface of the TC4 titanium alloy powder for modification, and then 20 g of the modified TC4 titanium alloy powder and 96 g of the unmodified TC4 titanium alloy powder were placed in a ball mill together, and ball milled for 1 hour at a rotation speed of 200 r / min and a ball-to-material ratio of 5:1 to obtain a heterogeneous composite powder;

[0051] The TC4 titanium alloy powder is prepared by a plasma rotating electrode method, has good powder sphericity, no planetary powder, a powder particle size of 15 μm to 53 μm, and a chemical composition that complies with GB / T 3620.1-2007 "Titanium and Titanium Alloy Grades and Chemical Compositions";

[0052] The copper target material used in the magnetron sputtering method has a mass purity of 99.995%; the coating power used in the magnetron sputtering method is 100W, the sputtering bias voltage is 0V, and the vacuum degree is 6×10 -3 Pa, argon protective atmosphere is introduced;

[0053] Step 2, composite material forming: plasma sintering the heterogeneous composite powder obtained in step 1 to obtain an intracrystalline precipitation-strengthened titanium alloy billet, and then hot deformation processing to obtain an intracrystalline precipitation-strengthened heterogeneous structure titanium-based composite material; the plasma sintering temperature is 1000°C, the heating rate is 100°C / min, the holding time is 5min, and the pressure is 40MPa; the hot deformation processing is rolling, and the rolling temperature is 900°C, the holding time is 20min, and the total rolling deformation is 75%.

[0054] Example 4

[0055] This embodiment includes the following steps:

[0056] Step 1, surface modification of titanium-based pre-alloyed powder and preparation of heterogeneous composite powder: 60 g of TC4 titanium alloy powder was placed in an ion plating machine, and a magnetron sputtering method was used for plating for 4 hours, and a uniform and dense copper film was plated on the surface of the TC4 titanium alloy powder for modification, and then 36 g of the modified TC4 titanium alloy powder and 84 g of the unmodified TC4 titanium alloy powder were placed in a ball mill together, and ball milled for 1 hour at a rotation speed of 200 r / min and a ball-to-material ratio of 5:1 to obtain a heterogeneous composite powder;

[0057] The TC4 titanium alloy powder is prepared by a plasma rotating electrode method, has good powder sphericity, no planetary powder, a powder particle size of 15 μm to 53 μm, and a chemical composition that complies with GB / T 3620.1-2007 "Titanium and Titanium Alloy Grades and Chemical Compositions";

[0058] The copper target material used in the magnetron sputtering method has a mass purity of 99.995%; the coating power used in the magnetron sputtering method is 100W, the sputtering bias voltage is 0V, and the vacuum degree is 6×10 -3 Pa, argon protective atmosphere is introduced;

[0059] Step 2, composite material forming: plasma sintering the heterogeneous composite powder obtained in step 1 to obtain an intracrystalline precipitation-strengthened titanium alloy billet, and then hot deformation processing to obtain an intracrystalline precipitation-strengthened heterogeneous structure titanium-based composite material; the plasma sintering temperature is 1000°C, the heating rate is 100°C / min, the holding time is 5min, and the pressure is 40MPa; the hot deformation processing is rolling, and the rolling temperature is 900°C, the holding time is 20min, and the total rolling deformation is 75%.

[0060] Example 5

[0061] This embodiment includes the following steps:

[0062] Step 1, surface modification of titanium-based pre-alloyed powder and preparation of heterogeneous composite powder: 60 g of TC4 titanium alloy powder was placed in an ion plating machine, and a magnetron sputtering method was used for plating for 4 hours, and a uniform and dense copper film was plated on the surface of the TC4 titanium alloy powder for modification, and then 48 g of the modified TC4 titanium alloy powder and 72 g of the unmodified TC4 titanium alloy powder were placed in a ball mill together, and ball milled for 1 hour at a rotation speed of 200 r / min and a ball-to-material ratio of 5:1 to obtain a heterogeneous composite powder;

[0063] The TC4 titanium alloy powder is prepared by a plasma rotating electrode method, has good powder sphericity, no planetary powder, a powder particle size of 15 μm to 53 μm, and a chemical composition that complies with GB / T 3620.1-2007 "Titanium and Titanium Alloy Grades and Chemical Compositions";

[0064] The copper target material used in the magnetron sputtering method has a mass purity of 99.995%; the coating power used in the magnetron sputtering method is 100W, the sputtering bias voltage is 0V, and the vacuum degree is 6×10 -3 Pa, argon protective atmosphere is introduced;

[0065] Step 2, composite material forming: plasma sintering the heterogeneous composite powder obtained in step 1 to obtain an intracrystalline precipitation-strengthened titanium alloy billet, and then hot deformation processing to obtain an intracrystalline precipitation-strengthened heterogeneous structure titanium-based composite material; the plasma sintering temperature is 1000°C, the heating rate is 100°C / min, the holding time is 5min, and the pressure is 40MPa; the hot deformation processing is rolling, and the rolling temperature is 900°C, the holding time is 20min, and the total rolling deformation is 75%.

[0066] Example 6

[0067] This embodiment includes the following steps:

[0068] Step 1, surface modification of titanium-based pre-alloyed powder and preparation of heterogeneous composite powder: 30 g of TC4 titanium alloy powder was placed in an ion plating machine, and a magnetron sputtering method was used for plating for 2 hours, and a uniform and dense copper film was plated on the surface of the TC4 titanium alloy powder for modification, and then the modified TC4 titanium alloy powder and 70 g of unmodified TC4 titanium alloy powder were placed in a ball mill together, and ball milled for 2 hours at a rotation speed of 250 r / min and a ball-to-material ratio of 5:1 to obtain a heterogeneous composite powder;

[0069] The TC4 titanium alloy powder is prepared by a plasma rotating electrode method, has good powder sphericity, no planetary powder, a powder particle size of 15 μm to 53 μm, and a chemical composition that complies with GB / T 3620.1-2007 "Titanium and Titanium Alloy Grades and Chemical Compositions";

[0070] The copper target material used in the magnetron sputtering method has a mass purity of 99.995%; the coating power used in the magnetron sputtering method is 100W, the sputtering bias voltage is 0V, and the vacuum degree is 6×10 -3 Pa, argon protective atmosphere is introduced;

[0071] Step 2, composite material forming: plasma sintering the heterogeneous composite powder obtained in step 1 to obtain an intracrystalline precipitation-strengthened titanium alloy billet, and then hot deformation processing to obtain an intracrystalline precipitation-strengthened heterogeneous structure titanium-based composite material; the plasma sintering temperature is 1100°C, the heating rate is 100°C / min, the holding time is 10min, and the pressure is 30MPa; the hot deformation processing is rolling, and the rolling temperature is 800°C, the holding time is 30min, and the total rolling deformation is 50%.

[0072] Example 7

[0073] This embodiment includes the following steps:

[0074] Step 1, surface modification of titanium-based pre-alloyed powder and preparation of heterogeneous composite powder: 50 g of TC4 titanium alloy powder was placed in an ion plating machine, and a magnetron sputtering method was used for plating for 4 hours, and a uniform and dense copper film was plated on the surface of the TC4 titanium alloy powder for modification, and then the modified TC4 titanium alloy powder and 50 g of unmodified TC4 titanium alloy powder were placed in a ball mill together, and ball milled for 1 hour at a rotation speed of 200 r / min and a ball-to-material ratio of 5:1 to obtain a heterogeneous composite powder;

[0075] The TC4 titanium alloy powder is prepared by a plasma rotating electrode method, has good powder sphericity, no planetary powder, a powder particle size of 15 μm to 53 μm, and a chemical composition that complies with GB / T 3620.1-2007 "Titanium and Titanium Alloy Grades and Chemical Compositions";

[0076] The copper target material used in the magnetron sputtering method has a mass purity of 99.995%; the coating power used in the magnetron sputtering method is 100W, the sputtering bias voltage is 0V, and the vacuum degree is 6×10 -3 Pa, argon protective atmosphere is introduced;

[0077] Step 2, composite material forming: plasma sintering the heterogeneous composite powder obtained in step 1 to obtain an intracrystalline precipitation-strengthened titanium alloy billet, and then hot deformation processing to obtain an intracrystalline precipitation-strengthened heterogeneous structure titanium-based composite material; the plasma sintering temperature is 800°C, the heating rate is 100°C / min, the holding time is 10min, and the pressure is 60MPa; the hot deformation processing is rolling, and the rolling temperature is 1000°C, the holding time is 10min, and the total rolling deformation is 90%.

[0078] Comparative Example 1

[0079] The specific process of this comparative example is: 120g of spherical TC4 titanium alloy powder with a particle size of 15μm to 53μm is put into a ball mill, ball milled for 1h at a rotation speed of 200r / min and a ball-to-material ratio of 5:1, then plasma sintered, and then subjected to hot deformation processing to obtain a titanium alloy material; the plasma sintering temperature is 1000℃, the heating rate is 100℃ / min, the insulation time is 5min, and the pressure is 40MPa; the hot deformation processing is rolling, and the rolling temperature is 900℃, the insulation time is 20min, and the total rolling deformation is 75%.

[0080] Comparative Example 2

[0081] The specific process of this comparative example is: 60g of TC4 titanium alloy powder is put into an ion plating machine, and a magnetron sputtering method is used for plating for 4h, and a uniform and dense copper film is plated on the surface of the TC4 titanium alloy powder for modification, which is repeated twice, and the obtained 120g of modified TC4 titanium alloy powder is put into a ball mill, and ball milled for 1h at a rotation speed of 200r / min and a ball-to-material ratio of 5:1, and then plasma sintered, and then subjected to hot deformation processing to obtain a titanium alloy material; the plasma sintering temperature is 1000°C, the heating rate is 100°C / min, the holding time is 5min, and the pressure is 40MPa; the hot deformation processing is rolling, and the rolling temperature is 900°C, the holding time is 20min, and the total rolling deformation is 75%.

[0082] Figure 4 The performance comparison diagram of the titanium-based composite materials prepared in Examples 3 to 5 of the present invention and the titanium alloy materials prepared in Comparative Examples 1 to 2 is shown in FIG. Figure 4 It can be seen that compared with the titanium alloy material prepared by directly sintering TC4 titanium alloy powder in Comparative Example 1, and the titanium alloy material prepared by sintering all modified TC4 titanium alloy powders in Comparative Example 2, the titanium-based composite materials prepared in Examples 3 to 5 of the present invention have high strength and excellent uniform elongation, and the maximum strength is as high as 1300 MPa, and the elongation after fracture is greater than 10%, indicating that the method of the present invention improves the strength and plasticity of the composite material based on the synergistic effect of intracrystalline nano-precipitation strengthening and heterogeneous interface strengthening, and achieves excellent strength-plasticity matching.

[0083] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing an intracrystalline precipitation-strengthened heterogeneous structure titanium-based composite material, characterized in that: The method comprises the following steps: Step 1: Surface modification of titanium-based pre-alloyed powder and preparation of heterogeneous composite powder: a uniform and dense metal film layer is coated on the surface of the titanium-based pre-alloyed powder by magnetron sputtering to modify the powder, and then the modified titanium-based pre-alloyed powder and the unmodified titanium-based pre-alloyed powder are ball-milled and mixed to obtain a heterogeneous composite powder; Step 2: Composite material forming: The heterogeneous composite powder obtained in step 1 is subjected to rapid densification sintering to obtain an intragranular precipitation-strengthened titanium alloy billet, which is then subjected to hot deformation processing to obtain an intragranular precipitation-strengthened heterogeneous structure titanium-based composite material.

2. The method for preparing the intracrystalline precipitation strengthened heterogeneous structure titanium-based composite material according to claim 1, characterized in that: The titanium-based pre-alloyed powder described in step 1 is prepared by a plasma rotating electrode method, the powder has good sphericity, no planetary powder, a powder particle size of 15 μm to 53 μm, and a chemical composition that complies with GB / T 3620.1-2007 "Titanium and Titanium Alloy Grades and Chemical Compositions".

3. The method for preparing the intracrystalline precipitation strengthened heterostructure titanium-based composite material according to claim 1, characterized in that: The component of the metal film layer in step 1 is metallic copper.

4. The method for preparing the intracrystalline precipitation strengthened heterogeneous structure titanium-based composite material according to claim 1, characterized in that: The metal target material used in the magnetron sputtering method in step 1 has a purity of 99.995%.

5. The method for preparing the intracrystalline precipitation strengthened heterogeneous structure titanium-based composite material according to claim 1, characterized in that: The magnetron sputtering method in step 1 uses a coating power of 100 W, a sputtering bias of 0 V, and a vacuum degree of 6 × 10 - 3 Pa, introduce argon protective atmosphere, and the plating time is 2h~4h.

6. The method for preparing the intracrystalline precipitation strengthened heterogeneous structure titanium-based composite material according to claim 1, characterized in that: The rotation speed of the ball mill in step 1 is 150r / min to 250r / min, the ball milling time is 1h to 2h, and the ball-to-material ratio is 5:

1.

7. The method for preparing the intracrystalline precipitation strengthened heterogeneous structure titanium-based composite material according to claim 1, characterized in that: The rapid densification sintering in step 2 is plasma sintering, and the temperature of the plasma sintering is 800° C. to 1100° C., the heating rate is 100° C. / min, the insulation time is 5 min to 10 min, and the pressure is 30 MPa to 60 MPa.

8. The method for preparing the intracrystalline precipitation strengthened heterogeneous structure titanium-based composite material according to claim 1, characterized in that: The thermal deformation process in step 2 is rolling, and the rolling temperature is 800° C. to 1000° C., the holding time is 10 min to 30 min, and the total rolling deformation is 50% to 90%.

9. An intracrystalline precipitation strengthened heterogeneous structure titanium-based composite material prepared by the method according to any one of claims 1 to 8.

Citation Information

Cited By

  • Tungsten material with dual-scale heterogeneous layered structure and preparation method thereof

    CN120715211A