Discontinuum reinforced titanium-based composite material sintering-rolling short-process ring piece forming method and product

Through the sintering-rolling short process method, the problem of high difficulty in forming titanium-based composite materials at high temperatures is solved, the high density and excellent performance of the ring are achieved, the process steps are simplified, and the production efficiency is improved.

CN118788965APending Publication Date: 2024-10-18HUAZHONG UNIV OF SCI & TECH

Patent Information

Application Number
CN202410808769.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In the existing technology, when titanium-based composite materials are formed at high temperatures, there are problems such as narrow hot processing range, high forming difficulty, uneven deformation, and poor material fluidity, resulting in discontinuous-reinforced titanium-based composite rings during large-deformation ring rolling. It is easy to crack during forming, and the traditional process has many steps and low efficiency, making it difficult to process high-performance ring parts.

Method used

Using the sintering-rolling short process method, titanium alloy matrix powder and reinforced phase powder are mixed through ball milling, and hot isostatic pressing is performed to obtain a ring-shaped blank. The ring-shaped blank is then modified and modified during the ring rolling process, and the mold structure is optimized to control the amount of deformation. , reduce defects and achieve short-cycle forming of rings with complex cross-sections.

Benefits of technology

It improves the structural uniformity and performance of the ring, reduces the oxygen content and impurity content, achieves high density and excellent mechanical properties, simplifies the process steps, improves the production efficiency and forming quality, and solves the forming failure in the traditional process. and low efficiency issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788965A_ABST
    Figure CN118788965A_ABST
Patent Text Reader

Abstract

The invention belongs to the related technical field of metal material forming, and discloses a non-continuum reinforced titanium-based composite material sintering-rolling short-process ring piece forming method and a product. The annular blank can be prepared through a sintering process, the section shape of the annular blank can be freely designed, sintering defects are reduced and the structure is homogenized through shape correction and modification in subsequent rolling forming, and it is ensured that the mechanical property of the annular piece is optimal. The sintering-rolling short-process ring piece forming method specifically comprises the steps of sintering process formulation, annular blank sintering and ring piece rolling forming, and aims at obtaining the discontinuous body reinforced titanium-based composite material ring piece which is uniform in target shape and size and structure and excellent in performance. By means of the sintering-rolling short-process ring piece forming method, the problems that in traditional ring piece rolling forming, due to the fact that the number of passes is large, the working procedure is long, temperature drop and the accumulated deformation amount are large, plasticity is poor, forming is difficult, and a composite material ring blank is prone to cracking, and forming fails can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field related to metal material forming, and more specifically, relates to a discontinuous body reinforced titanium-based composite material sintering-rolling short-process ring forming method and product. Background Art

[0002] Titanium alloys have the characteristics of low density, high specific strength, non-magnetic and non-toxic, and excellent corrosion resistance. They are widely used in key parts in the fields of aerospace, weapons and equipment, automobiles, ships, etc. However, titanium alloys are currently limited by thermal barrier temperatures during their application. When the service temperature is above 600°C, the high-temperature strength, creep resistance, and high-temperature oxidation resistance of titanium alloys drop sharply, causing the material to fail and the parts to fail to meet performance requirements. High-temperature section parts of high-pressure compressors (such as rings, blades, etc.) working in the range of 400°C to 700°C currently still use nickel-based high-temperature alloys with a density of about 1.83 times that of titanium alloys. Excessive use of nickel-based high-temperature alloy materials will significantly increase engine weight and energy consumption, restricting the improvement of engine thrust-to-weight ratio. With the rapid development of the aerospace field, higher requirements are placed on lightweight, high-strength, and high-temperature resistant materials.

[0003] The combination of high modulus and high strength reinforcements and titanium alloy matrix with good plasticity and toughness makes titanium matrix composites (TMCs) have better performance. Compared with the matrix titanium alloy, titanium matrix composites have higher specific modulus, specific strength, high temperature creep resistance, oxidation resistance and wear resistance, which can increase the service temperature of the matrix titanium alloy by nearly 200℃. Compared with continuous fiber reinforced titanium matrix composites, discontinuous reinforced titanium matrix composites (DRTMCs) with particles or whiskers as reinforcements have isotropy, simple preparation process, low production cost, and most importantly, can be processed by secondary deformation, and have better high temperature performance, which meets the high temperature service requirements of high-performance aircraft engine high-pressure compressor parts. It is considered to be a structural material with great application prospects in the aerospace field, which can replace nickel-based high-temperature alloy structural parts in compressors to reduce weight and improve the thrust-to-weight ratio of engines. In addition, the introduction of high elastic modulus reinforcements makes TMCs have a high specific modulus, which can reduce the deformation of parts during operation, thereby ensuring the stiffness of parts. However, due to the introduction of reinforcements with different physical and chemical properties from the matrix titanium alloy, TMCs face the following difficulties in thermoplastic processing: TMCs have a narrow hot working range and are difficult to form; the difference in structure between the reinforcement and the matrix causes uneven deformation, resulting in poor material fluidity; large deformation can easily cause TMCs to crack and make forming difficult, making the manufacturing and forming of DRTMCs parts quite difficult.

[0004] Rings are important load-bearing parts in aircraft engines, such as compressor casings, turbine casings, connecting rings, sealing rings, etc. Due to the high operating temperature, high-density nickel-based high-temperature alloy materials are still mostly used. Selecting DRTMCs with good performance to replace nickel-based high-temperature alloys as the material for forming rings can reduce the weight of aircraft engines and improve thrust-to-weight ratio. However, due to the large diameter and thin wall thickness of the rings in aircraft engine compressors, and the large deformation resistance and poor fluidity of DRTMCs materials. The traditional ring rolling process first requires the casting to be forged, upset, pre-punched, and punched at high temperature to form a ring blank, and then radial and axial rolling is used to form the ring, such as Figure 2 As shown in the figure, it has the characteristics of many passes, long process, large temperature drop and cumulative deformation. Therefore, the DRTMCs ring blank with poor plasticity is prone to cracking during large deformation ring rolling, resulting in forming failure, so it is difficult to form using the traditional multi-pass ring rolling process. In addition, the starting point of the traditional ring rolling route is the DRTMCs casting. After forging and blanking, the structural integrity of the reinforcement will be destroyed, and the material will have defects such as segregation and uneven structure, which will affect the high-temperature performance of the ring. If powder metallurgy, melt casting or additive manufacturing is used to directly form DRTMCs rings, the parts have low density, many pores, insufficient toughness, and generally require post-processing with low forming efficiency. It is difficult to directly process high-performance rings. In view of the difficulties in the forming of the above-mentioned discontinuous body reinforced titanium-based composite rings, a sintering-rolling short process ring forming method is proposed. Summary of the invention

[0005] In view of the above defects or improvement needs of the prior art, the present invention provides a discontinuum reinforced titanium-based composite material sintering-rolling short-process ring forming method and product, which solves the problem that DRTMCs ring blanks with poor plasticity are prone to cracking and resulting in forming failure due to the large number of passes, long process, large temperature drop and cumulative deformation in traditional ring rolling forming.

[0006] To achieve the above object, according to one aspect of the present invention, a method for forming a discontinuous body reinforced titanium-based composite material sintering-rolling short process ring is provided, the method comprising the following steps:

[0007] According to the actual service conditions of the ring parts, a titanium alloy matrix powder that meets the performance requirements and a reinforcing phase powder that matches the matrix powder are selected, and the optimal mass ratio of the two is determined. The matrix powder and the reinforcing phase powder are ball-milled to obtain a mixed powder in which the reinforcing phase powder is uniformly embedded in the surface of the titanium alloy matrix; the mixed powder is placed in a special-shaped mold for hot isostatic pressing and sintering to obtain a ring blank, and the ring blank is further ring-rolled and modified to finally obtain the target ring part.

[0008] Further preferably, the titanium alloy matrix powder is one or more of α-type, near-α-type, (α+β)-type, and β-type titanium alloy.

[0009] Further preferably, the reinforcing phase powder is one or more of Al2O3, TiN, B4C, SiC, TiC, TiB2 and TiB.

[0010] Further preferably, the mass ratio of the titanium alloy matrix powder to the reinforcement phase powder is determined according to the following formula:

[0011]

[0012] Among them, m is the mass of the added reinforcement phase, M is the mass of the titanium alloy matrix, r is the average radius of the reinforcement phase, R is the average radius of the titanium alloy matrix, ρ1 is the density of the reinforcement phase, and ρ2 is the density of the titanium alloy matrix.

[0013] Further preferably, the ball milling powder mixing process is carried out in an argon protected environment.

[0014] Further preferably, the ball milling speed is 150-200 r / min, the ball milling time is 5h-8h, and the ball-to-material ratio is (3:1)-(5:1).

[0015] Further preferably, the sintering pressure in the hot isostatic pressing sintering is 50 MPa to 150 MPa, the sintering temperature is 1100° C. to 1300° C., and the holding time is 40 min to 4 h.

[0016] Further preferably, in the ring rolling forming, the rotation speed of the driving roller is 10 r / s to 100 r / s, the feeding speed of the core roller is 0.05 mm / s to 1 mm / s, and the feeding speed of the tapered roller is 0.1 mm / s to 1 mm / s.

[0017] According to another aspect of the present invention, there is provided a product formed by the above-mentioned forming method.

[0018] In general, the above technical solutions conceived by the present invention have the following beneficial effects compared with the prior art:

[0019] 1. The present invention changes the starting point of the traditional ring rolling route from a casting to a sintered part with a controllable shape and high density obtained by powder sintering. The structure of the special-shaped mold during the sintering process can be continuously optimized, thereby regulating the cumulative deformation of the composite ring blank during the ring rolling process and promoting the deformation of the difficult-to-form area to prevent cracking; in addition, the ring blank obtained by hot isostatic pressing sintering is further reduced in defects introduced during the sintering process and uniformly organized after ring rolling shaping and modification, so that the organization and performance of the final DRTMCs ring are further improved, thereby obtaining a special-shaped cross-section DRTMCs ring with excellent performance;

[0020] 2. Compared with the traditional forging billet-ring rolling forming process, the ring billet of the present invention is prepared by hot isostatic pressing and sintering process. The hot isostatic pressing technology combines the advantages of cold isostatic pressing and sintering processes, and realizes near-final forming and high density of parts under high temperature and high pressure environment, and has advantages that traditional processes do not have: ① Through the design of powder composition and sintering mold, the oxygen content and impurity content in the sintered parts of the ring billet can be effectively reduced, ensuring that the final parts formed by ring rolling have uniform structure and stable chemical composition, and can achieve very high density or even complete density, ensuring that the final ring has excellent comprehensive performance; ② The mixed powder in the mold is subjected to uniform pressure in all directions during the hot isostatic pressing and sintering process, and exhibits isotropic mechanical properties after forming. ③ The shape of the ring billet can be adjusted, which can reduce the amount of plastic deformation of subsequent rolling deformation, and improve the production efficiency and forming quality of DRTMCs ring parts;

[0021] 3. The present invention provides a discontinuum reinforced titanium-based composite material sintering-rolling short-process ring forming method, which can realize the short-cycle forming of complex-section titanium-based composite material rings, simplifies the process steps of traditional ring rolling, is more economical and efficient in the actual production process, and is conducive to the rapid forming of special-section DRTMCs rings with excellent performance through the ring rolling process. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a flow chart of a short-process ring forming method of a discontinuous body reinforced titanium-based composite material sintering-rolling according to a preferred embodiment of the present invention;

[0023] Figure 2 This is the process flow chart of traditional forging billet-ring rolling forming;

[0024] Figure 3 is a schematic diagram of the structure of a low-pressure turbine casing constructed according to a preferred embodiment 1 of the present invention;

[0025] Figure 4 It is a schematic diagram of the assembly of a ring rolling device constructed according to the preferred embodiment 1 of the present invention;

[0026] Figure 5 It is a schematic diagram of the L-shaped cross-section connecting ring structure constructed according to the preferred embodiment 2 of the present invention;

[0027] Figure 6 It is a schematic diagram of the assembly of a ring rolling device constructed according to the preferred embodiment 2 of the present invention;

[0028] Figure 7 is a schematic diagram of a sealing ring structure constructed according to a preferred embodiment 3 of the present invention;

[0029] Figure 8It is a schematic diagram of the structure of a special-shaped thin-walled ring constructed according to the preferred embodiment 4 of the present invention;

[0030] Fig. 9 It is a schematic diagram of the structure of an extra-large diameter special-section ring constructed according to the preferred embodiment 5 of the present invention.

[0031] Throughout the drawings, the same reference numerals are used to denote the same elements or structures, wherein:

[0032] 1- driving roller, 2- ring blank, 3- core roller, 4- cone roller. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0034] like Figure 1 As shown in the figure, a short-process ring forming method of sintering-rolling of discontinuous reinforced titanium-based composite materials is used. First, the structure of the special-shaped sintering mold is designed. According to the geometric shape and size of the final ring, the structure of the special-shaped sintering mold is designed and optimized in combination with simulation, so that the deformation of the obtained ring blank during ring rolling is moderate, ensuring that the DRTMCs blank will not crack due to large deformation during the ring rolling process and has an appropriate deformation, thereby reducing sintering defects and uniform organization. Then, according to the actual service conditions and performance requirements of the ring parts, a sintering process is formulated. According to the existing research on the sintering preparation of titanium-based composite materials, after selecting the reinforcing phase and titanium alloy matrix powder, the ball milling parameters are determined for low-energy ball milling to mix the powder, and hot isostatic pressing sintering is performed after obtaining the mixed powder with the best reinforcing phase mass fraction. Finally, the DRTMCs ring is rolled to determine the optimal rolling parameters, and the sintered ring blank is shaped and modified to obtain a DRTMCs ring with a target shape and size, uniform structure, and excellent performance, so as to ensure the success rate and qualified rate of the DRTMCs ring forming. The specific forming method includes the following steps:

[0035] (1) According to the actual service conditions of the ring parts, the best combination of reinforcement phase and titanium alloy matrix powder is selected, the particle size of the reinforcement phase and titanium alloy powder is determined, and the optimal mass fraction of the reinforcement phase is calculated to ensure that the reinforcement phase in the microstructure of the special-shaped cross-section ring parts obtained after hot isostatic pressing and ring rolling is distributed in a quasi-continuous network, and the DRTMCs ring parts obtained after ring rolling have the best mechanical properties;

[0036] Combined with the determined types and particle sizes of the reinforcement phase and titanium alloy matrix, the ball milling parameters are further determined to carry out low-energy ball milling powder mixing, so as to ensure that the titanium alloy matrix is ​​not damaged and impurities are not introduced, and the reinforcement phase and titanium alloy matrix powders are fully mixed under argon protection, so as to obtain a mixed powder in which the reinforcement phase is uniformly embedded on the surface of the titanium alloy matrix;

[0037] (2) Design and optimize the sintered ring blank according to the principle of constant volume, and thus design and optimize the structure of the sintering mold to ensure that the ring blank undergoes appropriate cumulative plastic deformation during subsequent ring rolling and modification, promote the deformation of difficult-to-form areas, reduce sintering defects and make the structure uniform, avoid cracking of DRTMCs rings, and thus ensure the success rate and qualified rate of ring manufacturing;

[0038] Combined with the obtained target mixed powder, the sintering process parameters such as sintering pressure, sintering temperature, and holding time are determined according to the physical and chemical properties of the mixed powder. The sintering parameters are optimized according to the characterization results of the sintered structure to obtain the best sintering preparation process. The ball-milled mixed powder is then placed in a special-shaped sintering mold and hot isostatic pressing is performed under the given parameters.

[0039] (3) Based on the obtained ring blank, the ring rolling forming parameters are determined to make the blank further plastically deformed, so that its structure and performance are further improved, and finally a DRTMCs ring part that meets the use requirements and shape and size is obtained.

[0040] Preferably, step (1) determines the comprehensive mechanical properties and high-temperature properties that the annular component must meet when working normally according to the actual service conditions of the annular component, thereby screening the titanium alloy matrix and reinforcement phase categories, determining the best combination of reinforcement phase and titanium alloy matrix powder, and determining the reinforcement phase and titanium alloy powder particle size, thereby calculating the best reinforcement phase mass fraction to ensure the optimal structure obtained after sintering.

[0041] Further preferably, the selection principles of titanium alloy matrix and reinforcement phase are as follows: Since the titanium alloy matrix accounts for more than 80% of the mass in DRTMCs, the matrix plays a leading role in connecting the reinforcement phase, transferring and bearing stress in the composite material. At the same time, the matrix also plays a very important role in high-temperature oxidation resistance. The selection of matrix materials should be selected according to the performance indicators that need to be obtained in the end. The selection of reinforcement phase must meet the following conditions: 1) Excellent physical and mechanical properties, such as high melting point, high elastic modulus, high specific strength, high specific stiffness and high hardness. 2) The thermal expansion coefficient of the reinforcement phase and the titanium alloy matrix material should be relatively small to prevent stress concentration at the interface between the reinforcement phase and the matrix. 3) During the preparation and application process, the reinforcement phase should have good thermodynamic stability. 4) There is good chemical compatibility between the reinforcement phase and the matrix material. The selection of suitable matrix and reinforcement phase plays a vital role in the service performance of the composite material.

[0042] Preferably, the suitable matrix is ​​selected from α-type, near-α-type, (a+β)-type, and β-type titanium alloys. α-type pure titanium has excellent plasticity, near-α-type titanium alloys have excellent high-temperature performance, (α+β)-type titanium alloys have excellent comprehensive performance, and β-type titanium alloys have high room temperature strength but low high-temperature strength. Commonly used ceramic reinforcement phases mainly include: Al2O3, TiN, B4C, SiC, TiC, TiB2, TiB and other high-hardness and insoluble substances. The common characteristics of ceramic reinforcement phases are high melting point, high elastic modulus, high specific strength, high specific stiffness and high hardness, as well as excellent characteristics such as thermodynamic stability.

[0043] Further preferably, after determining the types of titanium alloy matrix and reinforcement phase based on the mechanical properties that must be met for stable operation of the annular part, in order to ensure that the reinforcement phase can be distributed in a quasi-continuous network in the titanium alloy matrix structure, the particle size of the titanium alloy matrix differs from that of the reinforcement phase by at least 15 times, and the optimal mass ratio is determined by the following formula.

[0044]

[0045] Where: m is the mass of the added reinforcement phase, M is the mass of the titanium alloy matrix, r is the average radius of the reinforcement phase, R is the average radius of the titanium alloy matrix, ρ1 is the density of the reinforcement phase, and ρ2 is the density of the titanium alloy matrix.

[0046] Preferably, a lower ball milling energy should be used when mixing powders, with a rotation speed of 150 to 200 r / min. Low-energy ball milling will evenly embed the fine reinforcing phase into the surface of the larger spherical titanium alloy matrix, while the titanium alloy matrix maintains its original size and spherical shape. The shorter ball milling time is 5 to 8 hours. If the ball milling time is too long, it is easy to cause part of the spherical titanium alloy matrix to be smashed or deformed into thin sheets, thereby affecting the sintering structure and further affecting the mechanical properties of the sintered parts. The lower ball-to-material ratio is 3:1 to 5:1. Improper selection of the ball-to-material ratio will also cause uneven mixing of the raw material powders, resulting in agglomeration, which will reduce the mechanical properties of the sintered parts.

[0047] Further preferably, the sintering parameters during hot isostatic pressing are determined, and the choice of pressure is: during the sintering process of preparing DRTMCs, the greater the pressure applied by the outside world, the higher the density of the prepared composite material, the greater the material forming rate, which is conducive to inhibiting grain growth, thereby refining the grains. When selecting the pressure, the equipment tonnage and powder properties should also be considered, and from the principle of economy, the sintering pressure is generally 50-150MPa. The choice of sintering temperature: if the sintering temperature is too low, the chemical reaction between the uniformly mixed powders cannot occur. If the sintering temperature is increased, not only the chemical reaction can proceed normally, but also the defects of the sintered material can be reduced and the density can be increased. However, too high a temperature will accelerate the growth rate of grains in the composite material, causing its grains to grow abnormally, and causing overburning to reduce the mechanical properties of the composite material. The optimal sintering temperature should be determined before sintering and forming, and the sintering temperature is generally 1100℃~1300℃. Selection of holding time: If the holding time is too short, the chemical reaction between the matrix and the reinforcing phase powder raw materials will be insufficient, which will easily lead to sintering defects, resulting in low density and sintering defects of the composite material. However, if the holding time is too long, the grains of the composite material will become coarse, thereby reducing the performance of the composite material. In recent years' research, it has been found that the sintering holding time of different titanium-based composite materials generally ranges from 40 minutes to 4 hours.

[0048] Preferably, the geometry of the sintering mold is designed, the geometry of the ring blank is designed according to the final shape and size of the ring, and the special-shaped mold is structurally designed and optimized in combination with the Deform simulation results. When designing the mold structure, the mold design principles should be followed, and the mold life and the final forming quality of the ring should be fully considered. Preferably, the evenly mixed powder is placed in a special-shaped mold, and the vacuum environment is first extracted and the protective gas is filled, and then sintered under high temperature and high pressure according to the established hot isostatic pressing sintering parameters. The sintering pressure is generally 50MPa~150MPa, the sintering temperature is generally 1100℃~1300℃, and the sintering holding time is generally 40min~4h. After parting, a DRTMCs ring blank with high density and similar shape to the final ring can be obtained, thereby ensuring that the ring blank undergoes less plastic deformation after subsequent ring rolling and modification.

[0049] Further preferably, the process parameters of ring rolling are determined, and the speed of driving roller 1 is: when the speed of driving roller is slow, the number of turns of the ring is reduced in the same rolling time, and the ring is not easy to bite; when the speed of driving roller is fast, the contact area between the roller and the ring per unit time is increased, which is conducive to the forming of the ring. In terms of engineering application, the speed of driving roller is generally 10r / s~100r / s. Feed speed of core roller 3: when a larger core roller feed speed is used, the width of the outer diameter and inner diameter of the ring is significantly reduced, while the width of the middle diameter of the ring is increased, so that the width is more evenly distributed on the end face of the ring, and the surface quality of the ring is higher. When a smaller feed speed is used, the width of the outer diameter and inner diameter of the ring is significantly increased, and the width of the middle diameter is very small. The shape of the free end face of the entire ring is prominent, the convex and concave changes dramatically, and the forming quality is poor. The core roller feed speed generally varies from 0.05mm / s to 1mm / s. Feed speed of tapered roller 4: As the feed speed of tapered roller increases, the surface quality of the upper end face of the ring gradually decreases, and the roundness error of the outer circle of the ring gradually increases; the increase in the feed speed of tapered roller aggravates the flow deformation of the ring blank 2 in the radial and axial directions, and the ring forming quality decreases within the same rolling time. Considering the rolling efficiency and the ring forming quality comprehensively, the feed speed of tapered roller 4 is generally determined to be 0.1mm / s~1mm / s.

[0050] The present invention manufactures DRTMCs rings with complex cross-sections by combining hot isostatic pressing and ring rolling forming technologies, and obtains ring blanks by hot isostatic pressing, thereby ensuring that the DRTMCs ring blanks will not crack due to large deformation during the ring rolling forming process and will have a certain amount of deformation, and will promote the forming of difficult-to-form areas to prevent cracking, thereby reducing sintering defects and achieving uniform organization, thereby ensuring that the final DRTMCs ring organization and performance are optimal, so as to obtain the best mechanical properties.

[0051] The sintering-rolling short-process ring forming method proposed in the present invention changes the starting point of the traditional ring rolling route from a casting to a powder sintered part, thereby solving the problem of cracking of DRTMCs ring blanks with poor plasticity and subsequent forming failure due to the large number of forming passes, long process, temperature drop and cumulative deformation in traditional ring rolling, and improving the success rate and qualification rate of manufacturing DRTMCs ring parts with special cross-sections.

[0052] The present invention will be further described below with reference to specific embodiments.

[0053] Example 1

[0054] like Figure 3As shown in the figure, the target ring is the low-pressure turbine casing of an aircraft engine. It is large in size, with significant changes in diameter between the large and small ends, uneven wall thickness, and axial asymmetry. The actual service conditions of the ring are complex, requiring uniform structure and fine grain size of the parts to ensure sufficient high-temperature strength, creep resistance and fatigue resistance. The working temperature should be higher than 500°C. The traditional forging billet-ring rolling process to form DRTMCs rings will cause cracking due to large deformation, resulting in forming failure. The powder sintering-rolling short process ring forming method can produce rings with excellent performance and meet the use requirements in a relatively short time, such as Figure 4 As shown, the specific steps include:

[0055] (1) The service conditions of the low-pressure turbine casing are complex. The titanium alloy matrix should have high-temperature strength. The near-α-type Ti60 titanium alloy is selected as the matrix. According to the principle that the reinforcing phase and the matrix should be compatible, the reinforcing phase is determined to be TiB2. The particle size of the Ti60 titanium alloy powder is 80-120um, and the particle size of the TiB2 powder is 2-4um, which ensures that the grain size obtained by sintering is uniform and small, and can ensure that the ring has excellent mechanical properties.

[0056] In order to ensure that the ring parts obtained after hot isostatic pressing have excellent mechanical properties and good plasticity, the matrix should be connected and the reinforcement phase should be distributed around the titanium alloy matrix in a quasi-continuous network structure. The particle size of the Ti60 titanium alloy matrix powder is about 20 times that of the TiB2 reinforcement phase, which can achieve discontinuous reinforcement and meet the optimal mass ratio calculation formula, so that the respective masses of the titanium alloy matrix and reinforcement phase powder can be calculated based on the total mass of the finished ring parts.

[0057] (2) Combined with ball milling, the mixed powder with the best mass ratio is obtained. Due to the high hardness of Ti60 titanium powder, the ball milling energy can be appropriately increased while ensuring the integrity of the titanium alloy matrix. In order to ensure that the reinforcing phase and the titanium alloy matrix powder can be fully mixed, a longer ball milling time is required. A single planetary ball mill with a volume of 500 ml is selected for ball milling. The ball milling speed is determined to be 200r / min, the ball milling time is 8h, and the ball-to-material ratio is 5: 1. When the reinforcing phase powder is unevenly distributed, the ball milling speed should be appropriately reduced and the ball milling time should be extended to ensure that the reinforcing phase is evenly distributed on the surface of the titanium alloy matrix.

[0058] (2) Combined with the target titanium-based composite material mixed powder with quasi-continuous network distribution of the reinforcement phase, the geometry of the sintering mold is designed. The corresponding principles should be followed when designing the sintering mold. The mixed powder is placed in the sintering mold to sinter and prepare a ring blank, so that the obtained blank is close to the cross-sectional shape of the final ring-rolled part, so as to ensure that the blank undergoes appropriate plastic deformation during the subsequent ring rolling shaping and modification, so as to obtain a DRTMCs ring with excellent performance. The sintering pressure, sintering temperature, and holding time vary according to the type of titanium-based composite material to be sintered. In order to ensure the sintering of DRTMCs with high density, uniform structure, and fine grains, the sintering pressure is preliminarily determined to be 150MPa, the sintering temperature is 1300℃, and the holding time is 4h, which can ensure the high density of the sintered part, excellent comprehensive performance, and meet the mechanical performance requirements of the ring.

[0059] (3) Combined with the ring blank obtained by sintering, the ring rolling process parameters are further determined, and the next step of rolling shaping and modification is carried out. During rolling, the deformation resistance of the Ti60 matrix is ​​large, the axial load is large, and the ring rolling process parameters are improperly selected. It is easy to cause the ring to become unstable during the rolling process, and the microstructure and performance are difficult to meet the use requirements. According to the conclusions of previous studies, the driving roller speed of 10r / s, the core roller feed speed of 0.05mm / s, and the cone roller feed speed of 0.1mm / s can obtain DRTMCs ring parts with good surface quality and excellent performance.

[0060] Example 2

[0061] like Figure 5 As shown in the figure, the target ring is an L-shaped cross-section connecting ring. Its actual service conditions are complex, requiring uniform microstructure of the parts to ensure sufficient high and low temperature strength, fatigue resistance and certain toughness. The wall thickness of the connecting ring is uneven and has a certain slope. The traditional forging billet-ring rolling forming process is difficult to produce DRTMCs L-shaped rings and is prone to forming failure due to large deformation. The powder sintering-rolling short process ring forming method can produce excellent performance connecting rings in a short time. Figure 6 As shown, the specific steps include:

[0062] (1) According to the service conditions of the connecting ring, the titanium alloy matrix material and the reinforcement phase are determined. Since the TA15 titanium alloy material has excellent high-temperature strength, oxidation resistance and creep resistance, and meets the complex service conditions of the ring, TiB2 is usually used as the reinforcement phase of the TA15 titanium alloy material. The reinforcement phase is determined to be TiB2, and the particle size of the selected TA15 titanium alloy powder is 80-120um, and the particle size of the TiB2 powder is 3-5um, which can ensure that relatively uniform grains are obtained and a certain high-temperature plasticity is guaranteed.

[0063] In order to ensure that the ring-shaped blank obtained after hot isostatic pressing has excellent mechanical properties and good plasticity, the matrix should be interconnected and the reinforcement phase should be distributed around the titanium alloy matrix in a quasi-continuous network structure. The particle size of the TA15 titanium alloy matrix powder is about 25 times that of the TiB2 reinforcement phase, which meets the optimal mass ratio calculation formula.

[0064] Combined with ball milling, the mixed powder with the best mass ratio is obtained. Since TA15 titanium powder has moderate hardness, lower ball milling energy is required to ensure the integrity of the titanium alloy matrix, and sufficient ball milling time is required to ensure that the reinforcing phase and the titanium alloy matrix powder can be fully mixed. A single planetary ball mill with a volume of 500 ml is selected for ball milling, and the ball milling speed is determined to be 150r / min, the ball milling time is 6h, and the ball-to-material ratio is 5:1.

[0065] (2) Combined with the target titanium-based composite material mixed powder with quasi-continuous network distribution of the reinforcement phase obtained in step (3), the geometry of the sintering mold is designed. The corresponding principles should be followed when designing the sintering mold so that the obtained ring blank is close to the cross-section of the final ring-rolled product, so as to ensure that the ring blank undergoes less plastic deformation during the subsequent ring rolling shaping and modification, so as to obtain a DRTMCs ring part with superior performance. The sintering pressure is preliminarily determined to be 100Mpa, the sintering temperature is 1200℃, and the holding time is 2h, which can ensure that the sintered DRTMCs ring blank with high density, uniform organization and excellent performance is obtained.

[0066] (3) The process parameters of ring rolling are determined in combination with the sintered blank, and the next step of rolling shaping and modification is carried out. The titanium-based composite material has a large deformation resistance and a large axial load during rolling. Improper selection of ring rolling process parameters can easily cause the ring to become unstable during the rolling process, and the microstructure and performance are also difficult to meet the use requirements. It is preliminarily determined that the driving roller speed is 50r / s, the core roller feed speed is 0.5mm / s, and the cone roller feed speed is 0.5mm / s to obtain DRTMCs ring parts with good surface quality and excellent performance.

[0067] Example 3

[0068] like Figure 7 As shown in the figure, the target ring is a compressor sealing ring, which has a high actual service temperature and requires the part to have high temperature stability and strength that meets the performance requirements. The wall thickness of the sealing ring has a certain slope, and it is difficult to produce DRTMCs sealing rings using the traditional forging billet-ring rolling forming process. The powder sintering-rolling short process ring forming method can produce sealing rings with excellent performance in a relatively short time, which specifically includes the following steps:

[0069] (1) According to the service conditions of the sealing ring, the titanium alloy matrix material and the reinforcement phase are determined. Since the TC4 titanium alloy material has excellent mechanical properties and meets the service mechanical performance requirements of the ring, TiB2 is usually used as the reinforcement phase of the TC4 titanium alloy material. The reinforcement phase is determined to be TiB2, the particle size of the TC4 titanium alloy powder is 45-105um, and the particle size of the TiB2 powder is 3-5um, which can ensure that the organizational structure that meets the performance requirements is obtained.

[0070] In order to ensure that the rings obtained after hot isostatic pressing have excellent mechanical properties and good plasticity, the matrix should be connected to each other. The particle size of the TC4 titanium alloy matrix powder is about 15 times that of the TiB2 reinforcement phase, which meets the optimal mass ratio calculation formula.

[0071] Combined with step (2), the mixed powder is ball-milled to obtain a mixed powder with the best mass ratio. Due to the low hardness of TC4 titanium powder, a lower ball-milling energy is required to ensure the integrity of the titanium alloy matrix. In order to ensure that the reinforcing phase and the titanium alloy matrix powder can be fully mixed, the ball-milling speed is determined to be 150 r / min, the ball-milling time is 5 h, and the ball-to-material ratio is 3:1, and a mixed powder that meets the requirements can be obtained.

[0072] (2) Combined with the target mass fraction of the mixed powder, the geometry of the sintering mold is designed to make the obtained sintered ring blank close to the final ring cross section, so as to ensure that the ring blank undergoes appropriate plastic deformation during the subsequent ring rolling and modification, so as to obtain a DRTMCs ring with excellent performance. The sintering pressure is preliminarily determined to be 50MPa, the sintering temperature is 1100℃, and the holding time is 40min.

[0073] (3) The ring rolling process parameters are determined based on the obtained sintered parts, and the next step of ring rolling forming is carried out. Since TC4 has good plastic deformation ability, the rolling forming parameters can be appropriately increased. It is preliminarily determined that the driving roller speed is 100r / s, the core roller feed speed is 1mm / s, and the cone roller feed speed is 1mm / s to obtain a DRTMCs sealing ring that meets the requirements.

[0074] Example 4

[0075] like Figure 8 As shown, the target ring is a special-shaped thin-walled ring, and both the inner and outer surfaces have a certain slope. The powder sintering-rolling short-process ring forming method can produce a special-shaped thin-walled ring with excellent performance in a relatively short time, which specifically includes the following steps:

[0076] (1) According to the service conditions of thin-walled rings, the titanium alloy matrix and reinforcement phase are determined. Since TC18 titanium alloy material has excellent high and low temperature strength and meets the service performance of thin-walled rings, B4C is a common reinforcement phase of TC18 titanium alloy. The powder particle size of 15-53um TC18 titanium alloy and the B4C powder particle size of 1-2um are selected to ensure that the microstructure that meets the performance requirements is obtained.

[0077] In order to ensure that the rings obtained after hot isostatic pressing have excellent mechanical properties and good plasticity, the matrix should be interconnected. The particle size of the TC18 titanium alloy matrix powder is about 15 times that of the B4C reinforcement phase, which meets the optimal mass ratio calculation formula and can achieve discontinuous reinforcement of the reinforcement.

[0078] Combined with ball milling, the mixed powder with the best mass ratio is obtained. Since TC18 titanium powder has moderate hardness, appropriate ball milling energy is required to ensure the integrity of the titanium alloy matrix. In order to ensure that the reinforcement phase and the titanium alloy matrix powder can be fully mixed, the ball milling speed is determined to be 200r / min, the ball milling time is 6h, and the ball-to-material ratio is 5:1, and a mixed powder that meets the requirements can be obtained.

[0079] (2) Based on the obtained mixed powder, the geometry of the sintering mold is designed to make the cross-section of the obtained sintered blank close to that of the final ring-rolled product, so as to ensure that the ring blank undergoes appropriate plastic deformation during subsequent ring rolling and modification, so as to obtain DRTMCs ring parts with excellent performance. The sintering pressure is preliminarily determined to be 120MPa, the sintering temperature is 1200℃, and the holding time is 2h.

[0080] (3) The ring rolling process parameters are determined based on the obtained ring blank for the next step of ring rolling forming. The sintered blank is further shaped and modified. Due to the large deformation resistance of TC18, the rolling forming parameters can be appropriately reduced. It is preliminarily determined that the driving roller speed is 20r / s, the core roller feed speed is 0.2mm / s, and the cone roller feed speed is 0.2mm / s to obtain DRTMCs special-shaped thin-walled ring parts that meet the requirements.

[0081] Example 5

[0082] like Fig. 9 As shown in the figure, the target ring is an ultra-large diameter special-shaped cross-section ring. The powder sintering-rolling short-process ring forming method can be used to process the special-shaped cross-section ring with excellent performance in a relatively short time, which specifically includes the following steps:

[0083] (1) According to the service conditions of the ring, the titanium alloy matrix and reinforcement phase are determined. Since the Ti153 titanium alloy material has excellent room temperature strength and good high temperature performance, which meets the service conditions of the ring, TiB2 is usually selected as the reinforcement phase. The particle size of the Ti153 titanium alloy powder is 45-120um, and the particle size of the TiB2 powder is 2-5um, which can ensure that the organization that meets the performance requirements is obtained.

[0084] In order to ensure that the blank obtained after hot isostatic pressing has excellent mechanical properties and good plasticity, the matrix should be connected with each other. The particle size of the Ti153 titanium alloy matrix powder is about 20 times different from the size of the TiB2 reinforcement phase, which meets the optimal mass ratio calculation formula.

[0085] Combined with ball milling, the mixed powder with the best mass ratio is obtained. Since Ti153 titanium powder is relatively hard, relatively high ball milling energy is required. In order to ensure that the reinforcing phase and titanium alloy matrix powder can be fully mixed, the ball milling speed is determined to be 200r / min, the ball milling time is 8h, and the ball-to-material ratio is 3:1, and a mixed powder that meets the requirements can be obtained.

[0086] (2) Based on the target mass fraction of the mixed powder, the geometry of the sintering mold is designed to make the obtained ring blank close to the cross section of the final ring, so as to ensure that the ring undergoes appropriate plastic deformation during the subsequent ring rolling and modification, so as to obtain a DRTMCs ring with excellent performance. The sintering pressure is preliminarily determined to be 100 MPa, the sintering temperature is 1200 ° C, and the holding time is 3 h.

[0087] (3) The ring rolling process parameters are determined based on the sintered blank to carry out the next step of ring rolling forming. The sintered parts are further shaped and modified. Due to the good thermal deformation performance of Ti153, the rolling forming parameters can be appropriately increased. It is preliminarily determined that the driving roller speed is 50r / s, the core roller feed speed is 0.5mm / s, and the cone roller feed speed is 0.5mm / s to obtain DRTMCs special-section ring parts that meet the requirements.

[0088] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A discontinuous body reinforced titanium-based composite material sintering-rolling short process ring forming method, characterized in that: The method comprises the following steps: A titanium alloy matrix powder and a reinforcing phase powder for reinforcing the matrix are selected, and the mass ratio of the two is determined; the matrix powder and the reinforcing phase powder are mixed by ball milling to obtain a mixed powder in which the reinforcing phase powder is uniformly embedded in the surface of the titanium alloy matrix; the mixed powder is hot isostatically pressed to obtain a ring blank, and the ring blank is ring-rolled to obtain a target ring.

2. A discontinuous body reinforced titanium-based composite material sintering-rolling short process ring forming method as claimed in claim 1, characterized in that: The titanium alloy matrix powder is one or more of α-type, near-α-type, (α+β)-type, and β-type titanium alloys.

3. A discontinuous body reinforced titanium-based composite material sintering-rolling short process ring forming method as claimed in claim 1, characterized in that: The reinforcing phase powder is one or more of Al2O3, TiN, B4C, SiC, TiC, TiB2 and TiB.

4. A discontinuous body reinforced titanium-based composite material sintering-rolling short process ring forming method as claimed in claim 3, characterized in that: The particle size difference between the titanium alloy matrix powder and the reinforcement phase powder is greater than or equal to 15 times, and the mass ratio of the two is determined according to the following formula: Among them, m is the mass of the added reinforcement phase powder, M is the mass of the titanium alloy matrix powder, r is the average radius of the reinforcement phase, R is the average radius of the titanium alloy matrix, ρ1 is the density of the reinforcement phase, and ρ2 is the density of the titanium alloy matrix.

5. The method for forming a discontinuous body reinforced titanium-based composite material by sintering-rolling short-process ring according to claim 1, characterized in that: The powder mixing process of the ball mill is carried out under the protection of argon gas.

6. A discontinuous body reinforced titanium-based composite material sintering-rolling short process ring forming method as claimed in claim 5, characterized in that: The rotation speed of the ball mill is 150-200 r / min, the ball milling time is 5h-8h, and the ball-to-material ratio during the ball milling process is (3-5):

1.

7. A discontinuous body reinforced titanium-based composite material sintering-rolling short process ring forming method as claimed in claim 1, characterized in that: The sintering pressure in the hot isostatic pressing sintering is 50MPa-150MPa, the sintering temperature is 1100°C-1300°C, and the heat preservation time is 40min-4h.

8. A discontinuous body reinforced titanium-based composite material sintering-rolling short process ring forming method as claimed in claim 1, characterized in that: In the ring rolling, the rotation speed of the driving roller is 10 r / s to 100 r / s, the feeding speed of the core roller is 0.05 mm / s to 1 mm / s, and the feeding speed of the cone roller is 0.1 mm / s to 1 mm / s.

9. A product formed by the forming method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Structure property regulation and control process for Ti2AlNb aero-engine case part

    CN116065110A

  • Near-net forming method of TC4 thin-wall special-shaped ring forging

    CN116329468A

  • Preparation method and application of high-temperature alloy ring piece with short process and high material utilization rate

    CN117206527A

  • Preparation method of large-specification titanium alloy ring material

    CN117259760A

  • Method for fabricating metal matrix composite

    US20030082311A1

Cited By

  • Design and preparation method of thin-wall annular near-net forming graphite mold

    CN121491339A