NO2 removal honeycomb catalyst and its preparation method and application

Through a one-step impregnation method, V2O5, WO3 and MnO2 active components are simultaneously loaded in the honeycomb SCR denitration catalyst, which solves the problems of low NO2 catalytic reduction efficiency and high production cost in traditional methods, and achieves efficient removal of NO2 emissions when the gas turbine is started. Improved production efficiency and product quality.

CN118320810BActive Publication Date: 2024-10-18HUADIAN QINGDAO ENVIRONMENTAL TECHNOLOCY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410441780.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-12
Publication Date
2024-10-18
Estimated Expiration
2044-04-12

AI Technical Summary

Technical Problem

The catalytic reduction efficiency of existing SCR denitrification catalysts for NO2 is low, resulting in excessive NO2 emissions when the gas turbine is started, affecting environmental protection and production efficiency. In traditional methods, it is difficult to load V2O5, WO3 and MnO2 active components at the same time, increasing production costs.

Method used

The porous honeycomb SCR denitrification catalyst is used as the carrier, and the active components of V2O5, WO3 and MnO2 are vertically impregnated at high temperature and normal pressure through a one-step impregnation method. The reaction between acetic acid and ammonium metavanadate is used to form soluble manganese acetate, which avoids solid precipitation of manganese oxalate and achieves three Simultaneous loading of components.

Benefits of technology

It improves the production efficiency and product quality of the NO2 removal catalyst, reduces production costs, achieves efficient removal of NO2 when the gas turbine is started, and supports large-scale commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118320810B_ABST
    Figure CN118320810B_ABST
Patent Text Reader

Abstract

The present invention discloses a NO2 removal honeycomb catalyst and its preparation method and application, belonging to the technical field of environmental protection catalysts. The technical scheme is as follows: the catalyst includes a carrier and an active component, the carrier is titanium dioxide, and the active components are V2O5, WO3 and MnO2; the steps are as follows: 1) deionized water, ammonium metavanadate and organic acid are added to the reaction container in sequence; 2) stirring and heating to react and dissolve; 3) adding manganese acetate and ammonium metatungstate and continuing to stir until dissolved to obtain an impregnation solution; 4) standing and cooling to room temperature, placing the catalyst carrier in the impregnation solution; 5) draining the impregnated sample, taking it out and placing it in an oven for drying; 6) calcining the dried catalyst sample to obtain the target product NO2 removal honeycomb catalyst. The present invention improves the production efficiency and product quality of the NO2 removal honeycomb catalyst, and reduces the production cost of the NO2 removal honeycomb catalyst, providing technical support for the large-scale commercial application of the NO2 removal catalyst in the future.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental protection catalysts, and in particular relates to a NO2 removal honeycomb catalyst and a preparation method and application thereof. Background Art

[0002] As the country's control over nitrogen oxide emissions becomes increasingly stringent, simple low-nitrogen combustion technology can no longer meet the current emission standards. At present, the most effective control measure for fixed source NOx is the selective catalytic reduction technology (SCR) using NH3 as a reducing agent. Among them, the catalyst is the core of this technology. The principle of SCR denitrification is that NOx is reduced to non-toxic and harmless N2 and H2O by NH3 under the action of a catalyst.

[0003] In recent years, with the vigorous development of green electricity such as wind, solar and hydropower, gas turbine power generation has played a more peak-shaving role. In this process, gas turbines need to be started frequently. When starting, the NO2 in the flue gas NOx accounts for as much as 50% due to the low startup temperature (the NO2 in the flue gas NOx of conventional coal-fired power plants accounts for only 5%, and NO accounts for 95%). In the selective catalytic reduction technology (SCR), the conventional SCR denitrification catalyst has a high catalytic reduction efficiency for NO (the catalytic reduction of NO is a fast reaction), but because NO2 is a slow reaction, the conventional SCR denitrification catalyst has a very low catalytic reduction efficiency for it. The NO2 that fails to react completely will be discharged into the atmosphere to produce "yellow smoke", which will cause bad environmental and social impacts on power generation companies.

[0004] In order to meet the increasingly stringent environmental protection requirements and the market demand for NO2 removal to eliminate yellow smoke when starting gas turbines, it is urgent to develop a NO2 removal honeycomb catalyst and its preparation method and process. Experimental verification shows that adding a certain amount of manganese dioxide to conventional vanadium-tungsten catalysts can effectively improve the NO2 removal efficiency of the catalyst. There are two ways of adding: one is to add it when mixing the clay, but this method of adding will seriously reduce the mixing efficiency, increase the mixing time, and there are small solid particles in the mixed clay, and there are problems such as unstable extrusion end face and mold clogging during extrusion molding, which seriously affect the production efficiency and product quality; the second is to load it by impregnation, but the de-NO2 catalyst itself contains not only MnO2 but also high content of V2O5 and WO3. These two components are impregnated with vanadium tungsten impregnation solution. Because soluble manganese salts will react with oxalic acid in the vanadium tungsten impregnation solution to form solid manganese oxalate, the loading of MnO2 cannot be carried out at the same time as vanadium tungsten. Another impregnation-drying-calcination process is required, which undoubtedly greatly increases the production cost of the de-NO2 catalyst. Therefore, it is necessary to develop a de-NO2 honeycomb catalyst and its preparation method to realize the simultaneous loading of the three active components of vanadium, tungsten and manganese on the catalyst carrier by one-time impregnation. Summary of the invention

[0005] The present invention provides a NO2 removal honeycomb catalyst and a preparation method and application thereof. A porous honeycomb SCR denitration catalyst is used as a carrier to achieve one-time impregnation of multiple active components and high-content loading at the same time through impregnation. The active components of the catalyst are V2O5, WO3 and MnO2. The impregnation liquid is prepared from the precursors of V2O5, WO3 and MnO2. The impregnation liquid solves the technical problem that the precursors of V2O5, WO3 and MnO2 cannot coexist at the same time. The wet unit after impregnation is dried and calcined to finally obtain a NO2 removal catalyst containing V2O5, WO3 and MnO2 active substances.

[0006] The technical solution of the present invention is:

[0007] In the first aspect, a honeycomb catalyst for removing NO2 is disclosed, which includes a carrier and an active component. The carrier is titanium dioxide, and the active components are V2O5, WO3 and MnO2. In terms of mass percentage, V2O5 is 1%-10%; WO3 is 1-10%; MnO2 is 0.1%-3%, and the rest is titanium dioxide.

[0008] Preferably, the active components are loaded onto the catalyst carrier by a one-step impregnation method, wherein the impregnation method is vertical impregnation at normal temperature and pressure to achieve simultaneous loading of the three active components of V2O5, WO3 and MnO2.

[0009] In the second aspect, a method for preparing the NO2 removal honeycomb catalyst is disclosed, which specifically comprises the following steps:

[0010] 1) adding deionized water, ammonium metavanadate and an organic acid into a reaction container in sequence to form a mixture;

[0011] 2) Stir and heat the mixture until the solid is completely dissolved;

[0012] 3) Stop heating, add manganese acetate and ammonium metatungstate and continue stirring until dissolved to obtain an impregnation solution;

[0013] 4) Allow to stand until the temperature drops to room temperature, and immerse the catalyst carrier in the impregnation liquid;

[0014] 5) Drain the impregnated samples and place them in an oven for drying;

[0015] 6) The dried catalyst sample is calcined to obtain the target product, NO2 removal honeycomb catalyst.

[0016] Preferably, the organic acid is one of acetic acid, lactic acid, citric acid, malic acid and tartaric acid.

[0017] Preferably, the added mass of organic acid is 1.4-2.0 times that of ammonium metavanadate; the added amount of deionized water is 5-10 times that of ammonium metavanadate, preferably 8.3 times.

[0018] Preferably, the heating temperature in step 2) is 65-70°C.

[0019] Preferably, in step 3), the added mass of manganese acetate in step 3) is 0.5 times that of ammonium metavanadate, and the added mass of ammonium metatungstate is 1.67 times that of ammonium metavanadate; the added mass ratio of deionized water: ammonium metavanadate: organic acid: manganese acetate: ammonium metatungstate in the impregnation solution is 100:12:17:6:20.

[0020] Preferably, the immersion time in step 4) is 1-3 min; the drying in step 5) is performed at 110-120° C. for 2-6 h; and the calcination in step 6) is performed in a muffle furnace at 400-600° C. for 4-8 h.

[0021] Preferably, the preparation method of the de-NO2 honeycomb catalyst, the system used for the preparation of the impregnation liquid, includes a stirring tank 1, a stirring tank 2, a stirring tank 3, a stirring tank 4 and a controller, an impregnation liquid delivery pipeline 1 and an impregnation liquid delivery pipeline 2 are arranged between the stirring tank 2 and the stirring tank 1, the impregnation liquid delivery pipeline 1 and the impregnation liquid delivery pipeline 2 are connected through a vertical pipe 1 and a vertical pipe 2 arranged in parallel, a horizontal pipe 1 and a horizontal pipe 2 are arranged in parallel between the vertical pipe 1 and the vertical pipe 2, a connecting pipe 1 is arranged between the horizontal pipe 1 and the horizontal pipe 2, a high-temperature circulation pump 1 is arranged on the connecting pipe 1, a delivery valve 1 and a delivery valve 3 are arranged on the horizontal pipe 1, and a horizontal pipe 2 A delivery valve 2 and a delivery valve 4 are arranged on the top; the stirring tank 1 and the stirring tank 3 are connected to the impregnation liquid output pipeline, and the impregnation liquid output pipeline is provided with a control valve 1 and a control valve 2; the heating interlayers of the stirring tank 2 and the stirring tank 4 are connected to the high-temperature steam input pipeline and the low-temperature steam output pipeline, and the high-temperature steam input pipeline is provided with a high-temperature steam valve 1 and a high-temperature steam valve 2, and the low-temperature steam output pipeline is provided with a low-temperature steam valve 1 and a low-temperature steam valve 2; the delivery valve 1, the delivery valve 2, the delivery valve 3, the delivery valve 4, the high-temperature steam valve 1, the high-temperature steam valve 2, the low-temperature steam valve 1, the low-temperature steam valve 2 and the high-temperature circulation pump 1 are all electrically connected to the controller;

[0022] An impregnation liquid delivery pipeline 3 and an impregnation liquid delivery pipeline 4 are arranged between the stirring tank 4 and the stirring tank 3, and the impregnation liquid delivery pipeline 3 and the impregnation liquid delivery pipeline 4 are connected through a vertical pipe 3 and a vertical pipe 4 arranged in parallel, and a horizontal pipe 3 and a horizontal pipe 4 are arranged in parallel between the vertical pipe 3 and the vertical pipe 4, and a connecting pipe 2 is arranged between the horizontal pipe 3 and the horizontal pipe 4, and a high-temperature circulation pump 2 is arranged on the connecting pipe 2, and a delivery valve 5 and a delivery valve 7 are arranged on the horizontal pipe 3, and a delivery valve 6 and a delivery valve 8 are arranged on the horizontal pipe 4, and the delivery valve 5, the delivery valve 6, the delivery valve 7, the delivery valve 8 and the high-temperature circulation pump 2 are all electrically connected to the controller;

[0023] A heat exchanger is arranged between the impregnation liquid delivery pipeline 1, the impregnation liquid delivery pipeline 2, the impregnation liquid delivery pipeline 3 and the impregnation liquid delivery pipeline 4, and heat exchange is achieved through the heat exchanger, and the heat exchanger is a tubular heat exchanger;

[0024] The stirring tank 1, stirring tank 2, stirring tank 3 and stirring tank 4 are all provided with a temperature sensor and an agitator, and the agitator and the temperature sensor are both electrically connected to the controller.

[0025] In a third aspect, the application of the NO2 removal honeycomb catalyst in removing NO2 when starting a gas turbine is disclosed.

[0026] The present invention selects an organic acid and reacts it with ammonium metavanadate and dissolves it according to a specific addition order and reaction method, and makes the final reactant not react with manganese salt and tungsten salt to produce solid precipitation. The three active components of vanadium, tungsten and manganese can coexist stably in the same impregnation solution, and the catalyst carrier is impregnated with the three active components of vanadium, tungsten and manganese at one time and loaded simultaneously. In the present invention, it is different from the reaction of oxalic acid and manganese acetate to produce manganese oxalate solid. The manganese acetate generated by the reaction of acetic acid with manganese ions in manganese acetate is soluble, while ammonium metavanadate basically does not react with acetic acid at room temperature, and soluble acetic acid and metavanadium complexes must be generated under the conditions of continuous stirring and continuous heating. Different from the traditional vanadium tungsten impregnation solution using oxalic acid as an organic acid to dissolve ammonium metavanadate, and then after adding manganese acetate, manganese oxalate precipitation will be formed, causing the impregnation solution to fail. The present invention uses acetic acid to react and dissolve with ammonium metavanadate under the conditions of heating and stirring, and no precipitation reaction will be formed after adding manganese acetate, so the stable coexistence of the three active component precursors of vanadium, tungsten and manganese can be achieved.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. The preparation method of the NO2 removal honeycomb catalyst of the present invention is different from the traditional method of extruding after adding MnO2 precursor through mixing, and is also different from the traditional two-time impregnation method. It adopts a one-step impregnation method to achieve the simultaneous loading of three active components of V2O5, WO3 and MnO2, and solves the technical problem that the precursor solutions of the three active components cannot coexist. It can greatly improve the production efficiency and product quality of the NO2 removal honeycomb catalyst, and reduce the production cost of the NO2 removal honeycomb catalyst, providing technical support for the subsequent large-scale commercial application of the NO2 removal catalyst.

[0029] 2. The catalyst of the present invention has a high loading capacity, and can ultimately achieve a catalyst vanadium loading capacity greater than 3%; a tungsten loading capacity greater than 6%; and a manganese loading capacity greater than 0.5%.

[0030] 3. The impregnation solution of the present invention is heated to 65-70°C during the preparation process, and can be stably stored at room temperature after the preparation is completed, achieving impregnation at room temperature and pressure without high temperature heating.

[0031] 4. The impregnation liquid preparation system can make full use of the preheating of the prepared solution and use it for heating the new round of impregnation liquid preparation, which is more environmentally friendly and reduces production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic diagram of the structure of the impregnation liquid preparation system of the present invention.

[0033] In the figure, 1, stirring tank 1; 2, stirring tank 2; 3, stirring tank 3; 4, stirring tank 4; 5, impregnation liquid delivery pipeline 1; 6, impregnation liquid delivery pipeline 2; 7, vertical pipe 1; 8, vertical pipe 2; 9, horizontal pipe 1; 901, delivery valve 1; 902, delivery valve 3; 10, horizontal pipe 2; 1001, delivery valve 2; 1002, delivery valve 4; 11, connecting pipe 1; 12, high-temperature circulation pump 1; 13, impregnation liquid output pipeline; 1301, control valve 1; 1302, control valve 2; 14, high-temperature steam input pipeline; 1401, high-temperature steam valve one; 1402, high-temperature steam valve two; 15, low-temperature steam output pipeline; 1501, low-temperature steam valve one; 1502, low-temperature steam valve two; 16, impregnation liquid delivery pipeline three; 17, impregnation liquid delivery pipeline four; 18, vertical pipe three; 19, vertical pipe four; 20, horizontal pipe three; 2001, delivery valve five; 2002, delivery valve seven; 21, horizontal pipe four; 2101, delivery valve six; 2102, delivery valve eight; 22, connecting pipe two; 23, high-temperature circulation pump two; 24, heat exchanger. DETAILED DESCRIPTION

[0034] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0035] like Figure 1As shown, the system used for preparing the impregnation liquid in the embodiments of the present invention and the comparative examples includes a stirring tank 1, a stirring tank 2, a stirring tank 3, a stirring tank 4 and a controller, an impregnation liquid delivery pipeline 15 and an impregnation liquid delivery pipeline 26 are arranged between the stirring tank 22 and the stirring tank 1, the impregnation liquid delivery pipeline 15 and the impregnation liquid delivery pipeline 26 are connected through a vertical pipe 17 and a vertical pipe 28 arranged in parallel, a horizontal pipe 19 and a horizontal pipe 210 are arranged in parallel between the vertical pipe 17 and the vertical pipe 218, a connecting pipe 11 is arranged between the horizontal pipe 19 and the horizontal pipe 210, a high-temperature circulating pump 12 is arranged on the connecting pipe 11, a delivery valve 1901 and a delivery valve 3902 are arranged on the horizontal pipe 19, and a delivery valve 2101 and a delivery valve 4102 are arranged on the horizontal pipe 210; the stirring tank 1 1 and stirring tank three 3 are connected to the impregnation liquid output pipeline 13, and the impregnation liquid output pipeline 13 is provided with a control valve one 1301 and a control valve two 1302; the heating interlayers of stirring tank two 2 and stirring tank four 4 are connected to the high-temperature steam input pipeline 14 and the low-temperature steam output pipeline 15, and the high-temperature steam input pipeline 14 is provided with a high-temperature steam valve one 1401 and a high-temperature steam valve two 1402, and the low-temperature steam output pipeline 15 is provided with a low-temperature steam valve one 1501 and a low-temperature steam valve two 1502; the delivery valve one 901, the delivery valve two 1001, the delivery valve three 902, the delivery valve four 1002, the high-temperature steam valve one 1401, the high-temperature steam valve two 1402, the low-temperature steam valve one 1501, the low-temperature steam valve two 1502 and the high-temperature circulation pump one 12 are all electrically connected to the controller;

[0036] An impregnation liquid delivery pipeline three 16 and an impregnation liquid delivery pipeline four 17 are arranged between the stirring tank four 4 and the stirring tank three 3, and the impregnation liquid delivery pipeline three 16 and the impregnation liquid delivery pipeline four 17 are connected through a vertical pipe three 18 and a vertical pipe four 19 arranged in parallel, and a horizontal pipe three 20 and a horizontal pipe four 21 are arranged in parallel between the vertical pipe three 18 and the vertical pipe four 19, and a connecting pipe two 22 is arranged between the horizontal pipe three 20 and the horizontal pipe four 21, and a high-temperature circulation pump two 23 is arranged on the connecting pipe two 22, and a delivery valve five 2001 and a delivery valve seven 2002 are arranged on the horizontal pipe three 20, and a delivery valve six 2101 and a delivery valve eight 2102 are arranged on the horizontal pipe four 21, and the delivery valve five 2001, the delivery valve six 2101, the delivery valve seven 2002, the delivery valve eight 2102 and the high-temperature circulation pump two 23 are all electrically connected to the controller;

[0037] A heat exchanger 24 is provided between the impregnation liquid delivery pipeline 1 5, the impregnation liquid delivery pipeline 2 6, the impregnation liquid delivery pipeline 3 16 and the impregnation liquid delivery pipeline 4 17, and heat exchange is achieved through the heat exchanger 24, and the heat exchanger 24 is a tubular heat exchanger;

[0038] The stirring tank 1 1 , the stirring tank 2 2 , the stirring tank 3 3 , and the stirring tank 4 4 are all provided with a temperature sensor and an agitator, and the agitator and the temperature sensor are both electrically connected to the controller.

[0039] The specific preparation method of the impregnation solution is as follows:

[0040] In the initial state, all switches are in the off state.

[0041] (1) First, deionized water, ammonium metavanadate and acetic acid are added to the stirring tank 2 in sequence, and stirring is started to prepare the first batch of impregnation solution;

[0042] (2) Open the high-temperature steam valve 1401 and the low-temperature steam valve 1501, and the high-temperature steam enters the heating compartment of the stirring tank 2 to heat the solid-liquid coexistence in the stirring tank 2. As the high-temperature steam continues to heat, the temperature of the solid-liquid coexistence in the stirring tank 2 continues to rise. When the temperature sensor in the stirring tank 2 shows that the temperature reaches 70°C, the ammonium metavanadate and acetic acid in the tank are completely reacted and dissolved;

[0043] (3) Close the high-temperature steam valve 1401 and the low-temperature steam valve 1501;

[0044] (4) At this time, deionized water, ammonium metavanadate and acetic acid are added to the stirring tank 3 in sequence, stirring is started, and the second batch of impregnation solution is prepared;

[0045] (5) Open the transfer valve 1 901, the transfer valve 2 1001, the transfer valve 5 2001 and the transfer valve 6 2101, and at the same time start the high-temperature circulation pump 1 12 and the high-temperature circulation pump 2 23, start the stirring of the stirring tank 1 1 and the stirring tank 4 4, transfer the high-temperature impregnation liquid in the stirring tank 2 2 to the stirring tank 1 1, and transfer the room-temperature solid-liquid coexistence in the stirring tank 3 3 to the stirring tank 4 4. During this transfer process, the high-temperature impregnation liquid transferred from the stirring tank 2 2 will heat the low-temperature solid-liquid coexistence transferred from the stirring tank 3 3 to 50-60°C in the tubular heat exchanger and transfer it to the stirring tank 4 4; the volume of the solution in the stirring tank 2 2 and the stirring tank 3 3 should be adjusted according to the volume of the solution in the stirring tank 2 Control the flow of high-temperature circulation pump 12 and high-temperature circulation pump 23 to ensure that the transfer is completed at the same time. After the transfer is completed, close the high-temperature circulation pump 12 and high-temperature circulation pump 23, and close the delivery valve 1 901, delivery valve 2 1001, delivery valve 5 2001 and delivery valve 6 2101; after the transfer is completed, the solution transferred from stirring tank 2 2 to stirring tank 1 is a solution that has dropped to room temperature. At this time, manganese acetate and ammonium metatungstate are added in sequence, stirred and dissolved, and the preparation of the NO2 removal catalyst impregnation solution is completed. Open the control valve 1301 set in the impregnation solution output pipeline 13, and the impregnation solution in the stirring tank 1 is transported to the impregnation process, and then the control valve 1301 is closed;

[0046] (6) After the transfer is completed, the temperature of the low-temperature solid-liquid coexistence in the stirring tank 33 transferred to the stirring tank 44 rises to about 50-60°C. At this time, the high-temperature steam valve 2 1402 and the low-temperature steam valve 2 1502 are opened, and the high-temperature steam enters the heating interlayer of the stirring tank 44 to heat the solid-liquid coexistence in the stirring tank 44; as the high-temperature steam continues to heat, the temperature of the solid-liquid coexistence in the stirring tank 44 continues to rise. When the temperature sensor in the tank shows that the temperature reaches 70°C, the ammonium metavanadate and acetic acid in the tank are completely reacted and dissolved, and the high-temperature steam valve 2 1402 and the low-temperature steam valve 2 1502 are closed, and stirring continues;

[0047] (7) At this time, deionized water, ammonium metavanadate and acetic acid are added to the mixing tank 1 in sequence, stirring is started, and the third batch of impregnation solution is prepared.

[0048] (8) Open transfer valve eight 2102, transfer valve seven 2002, transfer valve three 902 and transfer valve four 1002, and simultaneously start high-temperature circulation pump one 12 and high-temperature circulation pump two 23, transfer the high-temperature impregnation liquid in stirring tank four 4 to stirring tank three 3, and transfer the room-temperature solid-liquid coexistence in stirring tank one 1 to stirring tank two 2. During this transfer process, the high-temperature impregnation liquid transferred from stirring tank four 4 will heat the low-temperature solid-liquid coexistence transferred from stirring tank one 1 to 50-60°C in the tubular heat exchanger and transfer it to stirring tank two 2. The flow rates of high-temperature circulation pump 12 and high-temperature circulation pump 23 need to be controlled according to the volume of the solution in stirring tank 4 and stirring tank 1 to ensure that the transfer is completed at the same time. After the transfer is completed, close the high-temperature circulation pump 12 and high-temperature circulation pump 23, and close the delivery valve 8 2102, delivery valve 7 2002, delivery valve 3 902 and delivery valve 4 1002. After the transfer is completed, the solution transferred from stirring tank 4 4 to stirring tank 3 3 is a solution that has been cooled to room temperature. At this time, add manganese acetate and ammonium metatungstate in turn, stir and dissolve, and complete the preparation of the NO2 removal catalyst impregnation solution.

[0049] (9) Open the control valve 2 1302 to transfer the impregnation liquid in the mixing tank 3 to the impregnation process and then close the control valve 2 1302;

[0050] (10) After the transfer is completed, the temperature of the low-temperature solid-liquid coexistence in the stirring tank 1 transferred to the stirring tank 2 rises to about 50-60°C. At this time, the high-temperature steam valve 1401 and the low-temperature steam valve 1501 are opened, and the high-temperature steam enters the heating compartment of the stirring tank 2 to heat the solid-liquid coexistence in the stirring tank, and step (2) and subsequent steps are repeated.

[0051] The catalyst supports used in the examples of the present invention and the comparative examples are all commercially available from Huadian Qingdao Environmental Protection Technology Co., Ltd., and the acetic acid used is acetic acid with a mass concentration of 50-55%, which is purchased from Henan Jindan Lactic Acid Technology Co., Ltd.

[0052] Example 1

[0053] This embodiment provides a honeycomb catalyst for removing NO2, in which the mass contents of active components V2O5, WO3 and MnO2 are respectively 3% vanadium pentoxide; 6% tungsten trioxide; and 0.5% manganese dioxide.

[0054] The preparation method of the NO2 removal honeycomb catalyst specifically comprises the following steps:

[0055] 1) 100 g of deionized water, 12 g of ammonium metavanadate and 16.8 g of acetic acid were added to a reaction vessel in sequence to form a mixture;

[0056] 2) Stir the mixture and heat it to 60°C. The ammonium metavanadate reacts significantly with the acetic acid, and the dissolution rate of the ammonium metavanadate increases significantly. When the temperature rises to 70°C, the ammonium metavanadate is completely dissolved.

[0057] 3) Stop heating, add 6g manganese acetate and 20g ammonium metatungstate and continue stirring until dissolved to obtain an impregnation solution;

[0058] 4) Let it stand until the temperature drops to room temperature, and immerse the catalyst carrier in the impregnation liquid for 1 minute;

[0059] 5) Drain the impregnated samples and place them in an oven at 120°C for 6 hours;

[0060] 6) The dried catalyst sample was calcined in a muffle furnace at 400°C for 4 h to obtain the target product, NO2 removal honeycomb catalyst.

[0061] Example 2

[0062] This embodiment provides a honeycomb catalyst for removing NO2, in which the mass contents of active components V2O5, WO3 and MnO2 in the catalyst are 1.5% vanadium pentoxide; 6% tungsten trioxide; and 0.5% manganese dioxide.

[0063] The preparation method of the NO2 removal honeycomb catalyst specifically comprises the following steps:

[0064] 1) 100 g of deionized water, 6 g of ammonium metavanadate and 8.4 g of acetic acid were added to a reaction vessel in sequence to form a mixture;

[0065] 2) Stir the mixture and heat it to 60°C. The ammonium metavanadate reacts significantly with the acetic acid, and the dissolution rate of the ammonium metavanadate increases significantly. When the temperature rises to 70°C, the ammonium metavanadate is completely dissolved.

[0066] 3) Stop heating, add 6g manganese acetate and 20g ammonium metatungstate and continue stirring until dissolved to obtain an impregnation solution;

[0067] 4) Let it stand until the temperature drops to room temperature, and immerse the catalyst carrier in the impregnation liquid for 1 minute;

[0068] 5) Drain the impregnated samples and place them in an oven at 120 °C for 6 h;

[0069] 6) The dried catalyst sample was calcined in a muffle furnace at 400°C for 4-8 hours to obtain the target product, NO2 removal honeycomb catalyst.

[0070] Example 3

[0071] This embodiment provides a honeycomb catalyst for removing NO2, in which the mass contents of active components V2O5, WO3 and MnO2 are 6% vanadium pentoxide; 6% tungsten trioxide; and 0.5% manganese dioxide.

[0072] The preparation method of the NO2 removal honeycomb catalyst specifically comprises the following steps:

[0073] 1) 100 g of deionized water, 24 g of ammonium metavanadate and 34 g of acetic acid were added to a reaction vessel in sequence to form a mixture;

[0074] 2) Stir the mixture and heat it to 60°C. The ammonium metavanadate reacts significantly with the acetic acid, and the dissolution rate of the ammonium metavanadate increases significantly. When the temperature rises to 70°C, the ammonium metavanadate is completely dissolved.

[0075] 3) Stop heating, add 6g manganese acetate and 20g ammonium metatungstate and continue stirring until dissolved to obtain an impregnation solution;

[0076] 4) Let it stand until the temperature drops to room temperature, and then place the catalyst carrier vertically in the impregnation liquid and immerse it for 1 minute;

[0077] 5) Drain the impregnated samples and place them in an oven at 120 °C for 6 h;

[0078] 6) The dried catalyst sample was calcined in a muffle furnace at 500°C for 8 h to obtain the target product, NO2 removal honeycomb catalyst.

[0079] Comparative Example 1

[0080] The difference from Example 1 is that manganese acetate is not added in step 3), and the other steps are the same as Example 1.

[0081] Comparative Example 2

[0082] Different from Example 1, in step 1), 100 g of deionized water, 12 g of ammonium metavanadate and 15 g of acetic acid were added in sequence to form a mixture, but the ammonium metavanadate and acetic acid could not be completely dissolved, the preparation of the impregnation solution failed, and subsequent experiments could not be carried out.

[0083] Comparative Example 3

[0084] Different from Example 1, step 1) and step 2) are: 100 g of deionized water are added to the reaction container in sequence, heated to 60°C, and then 12 g of ammonium metavanadate and 16.8 g of acetic acid are added to form a mixture, and then stirred. The ammonium metavanadate and acetic acid cannot be completely dissolved, the preparation of the impregnation solution fails, and subsequent experiments cannot be carried out.

[0085] Comparative Example 4

[0086] Different from Example 1, step 1) and step 2) are: 100 g of deionized water are added to the reaction container in sequence, heated to 60°C, 16.8 g of acetic acid is added, stirred, and finally 12 g of ammonium metavanadate is added to form a mixture, which is stirred again. The ammonium metavanadate and acetic acid cannot be completely dissolved, the preparation of the impregnation solution fails, and subsequent experiments cannot be carried out.

[0087] Comparative Example 5

[0088] Different from Example 1, the heating temperature in step 2) is 60° C., and ammonium metavanadate cannot be completely dissolved.

[0089] The catalysts prepared in Examples 1-3 and Comparative Examples 1-4 were introduced into a NO2 micro-reactor, the reaction device having application number 202021195964.3 and named aging device for SCR denitrification catalyst activity detection. The specific measurement results are shown in Table 1.

[0090]

[0091] In Comparative Example 1, manganese acetate was not added, and the NO2 removal efficiency was significantly reduced. In Comparative Example 2, the amount of acetic acid added was reduced, and soluble acetic acid and metavanadium complexes could not be formed, and the preparation of the impregnation solution failed. In Comparative Examples 3 and 4, the order of adding materials was changed, and the heating temperature in step 2) was reduced in Comparative Example 5. However, the stable coexistence of the three active component precursors of vanadium, tungsten and manganese could not be achieved, and the impregnation solution could not be successfully prepared. The implementation of the scheme of the present invention must control the specific order of adding materials, the proportion of raw materials added, and the heating temperature to successfully configure the impregnation solution for subsequent catalyst impregnation experiments.

[0092] Although the present invention has been described in detail by combining the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.

Claims

1. Remove NO 2 Preparation method of honeycomb catalyst, It is characterized in that The catalyst comprises a carrier and an active component, wherein the carrier is titanium dioxide and the active component is V 2 O 5 , WO 3 and MnO 2 , expressed as mass percentage, V 2 O 5 1%-10%; WO 3 1-10%; MnO 2 0.1%-3%, the rest is titanium dioxide; The de-NO 2 The preparation method of the honeycomb catalyst specifically comprises the following steps: 1) adding deionized water, ammonium metavanadate and an organic acid into a reaction container in sequence to form a mixture; 2) Stir and heat the mixture until the solid is completely dissolved; 3) Stop heating, add manganese acetate and ammonium metatungstate and continue stirring until dissolved to obtain an impregnation solution; 4) Allow to stand until the temperature drops to room temperature, and immerse the catalyst carrier in the impregnation liquid; 5) Drain the impregnated samples and place them in an oven for drying; 6) Calcine the dried catalyst sample to obtain the target product, deNO 2 Honeycomb catalyst; The system used for preparing the impregnation liquid comprises a stirring tank 1 (1), a stirring tank 2 (2), a stirring tank 3 (3), a stirring tank 4 (4) and a controller. An impregnation liquid delivery pipeline 1 (5) and an impregnation liquid delivery pipeline 2 (6) are arranged between the stirring tank 2 (2) and the stirring tank 1 (1). The impregnation liquid delivery pipeline 1 (5) and the impregnation liquid delivery pipeline 2 (6) are connected through a vertical pipe 1 (7) and a vertical pipe 2 (8) arranged in parallel. The vertical pipe 1 (7) and A horizontal pipe 1 (9) and a horizontal pipe 2 (10) are arranged in parallel between the vertical pipe 2 (8); a connecting pipe 1 (11) is arranged between the horizontal pipe 1 (9) and the horizontal pipe 2 (10); a high-temperature circulation pump 1 (12) is arranged on the connecting pipe 1 (11); a delivery valve 1 (901) and a delivery valve 3 (902) are arranged on the horizontal pipe 1 (9); a delivery valve 2 (1001) and a delivery valve 4 (1002) are arranged on the horizontal pipe 2 (10); the mixing tank 1 (1) and the mixing tank 2 (1) are connected to the mixing tank 1 (1). The mixing tank three (3) is connected to the soaking liquid output pipeline (13), and the soaking liquid output pipeline (13) is provided with a control valve one (1301) and a control valve two (1302); the heating interlayers of the mixing tank two (2) and the mixing tank four (4) are connected to the high-temperature steam input pipeline (14) and the low-temperature steam output pipeline (15), and the high-temperature steam input pipeline (14) is provided with a high-temperature steam valve one (1401) and a high-temperature steam valve two (1402), and the low-temperature steam output pipeline (15) is provided with a low-temperature steam valve one (1501) and a low-temperature steam valve two (1502); the delivery valve one (901), the delivery valve two (1001), the delivery valve three (902), the delivery valve four (1002), the high-temperature steam valve one (1401), the high-temperature steam valve two (1402), the low-temperature steam valve one (1501), the low-temperature steam valve two (1502) and the high-temperature circulation pump one (12) are all electrically connected to the controller; An impregnation liquid delivery pipeline 3 (16) and an impregnation liquid delivery pipeline 4 (17) are arranged between the stirring tank 4 (4) and the stirring tank 3 (3); the impregnation liquid delivery pipeline 3 (16) and the impregnation liquid delivery pipeline 4 (17) are connected through a vertical pipe 3 (18) and a vertical pipe 4 (19) arranged in parallel; a horizontal pipe 3 (20) and a horizontal pipe 4 (21) are arranged in parallel between the vertical pipe 3 (18) and the vertical pipe 4 (19); a connecting pipe 3 (20) and a connecting pipe 4 (21) are arranged between the horizontal pipe 3 (20) and the horizontal pipe 4 (21). Connecting pipe 2 (22), connecting pipe 2 (22) is provided with high-temperature circulation pump 2 (23), transverse pipe 3 (20) is provided with delivery valve 5 (2001) and delivery valve 7 (2002), transverse pipe 4 (21) is provided with delivery valve 6 (2101) and delivery valve 8 (2102), delivery valve 5 (2001), delivery valve 6 (2101), delivery valve 7 (2002), delivery valve 8 (2102) and high-temperature circulation pump 2 (23) are all electrically connected to the controller; A heat exchanger (24) is provided between the impregnation liquid delivery pipeline 1 (5), the impregnation liquid delivery pipeline 2 (6), the impregnation liquid delivery pipeline 3 (16) and the impregnation liquid delivery pipeline 4 (17), and heat exchange is achieved through the heat exchanger (24); The stirring tank 1 (1), the stirring tank 2 (2), the stirring tank 3 (3), and the stirring tank 4 (4) are all provided with a temperature sensor and an agitator, and the agitator and the temperature sensor are both electrically connected to the controller.

2. The deNOx method according to claim 1 2 Preparation method of honeycomb catalyst, It is characterized in that The active components are loaded onto the carrier by a one-step impregnation method, which is a vertical impregnation method at room temperature and pressure to achieve V 2 O 5 , WO 3 and MnO 2 Simultaneous loading of three active components.

3. The deNOx method according to claim 1 2 Preparation method of honeycomb catalyst, It is characterized in that The organic acid is one of acetic acid, lactic acid, citric acid, malic acid and tartaric acid.

4. The deNOx according to claim 1 2 Preparation method of honeycomb catalyst, It is characterized in that The added amount of organic acid is 1.4-2.0 times that of ammonium metavanadate; the added amount of deionized water is 4-20 times that of ammonium metavanadate.

5. The deNOx method according to claim 1 2 Preparation method of honeycomb catalyst, It is characterized in that The amount of deionized water added is 8.3 times that of ammonium metavanadate.

6. The deNOx according to claim 1 2 Preparation method of honeycomb catalyst, It is characterized in that In step 2), the temperature is raised to 65-70°C.

7. The deNOx according to claim 4 2 Preparation method of honeycomb catalyst, It is characterized in that In step 3), the added mass of manganese acetate is 0.2-1.0 times of ammonium metavanadate, and the added mass of ammonium metatungstate is 2-4 times of ammonium metavanadate.

8. The deNOx method according to claim 4 2 Preparation method of honeycomb catalyst, It is characterized in that The added mass ratio of deionized water: ammonium metavanadate: organic acid: manganese acetate: ammonium metatungstate in the impregnation solution is 100:12:17:6:

20.

9. The deNOx according to claim 1 2 Preparation method of honeycomb catalyst, It is characterized in that In step 4), the impregnation time is 1-3 minutes; in step 5), the drying is carried out at 110-120° C. for 2-6 hours; and in step 6), the calcination is carried out in a muffle furnace at 400-600° C. for 4-8 hours.

10. The deNO prepared by the preparation method according to claim 1 or 2 2 Honeycomb catalyst removes NO during gas turbine startup 2 Application in.

Citation Information

Patent Citations

  • Aging device for activity detection of SCR denitration catalyst

    CN212410566U

  • Low-temperature low-vanadium SCR denitration catalyst and preparation method thereof

    CN114870833A