A low compression permanent deformation battery sealing material and preparation method thereof

By adding a specific formula and modification treatment to EPDM rubber, the problems of compression permanent deformation and insufficient high temperature resistance at high temperatures have been solved, and a low-cost, high-performance battery sealing material has been realized, suitable for 200°C environments. .

CN118325268BActive Publication Date: 2024-10-15DONGGUAN XINDONG RUBBER PLASTIC HARDWARE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410590326.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-13
Publication Date
2024-10-15
Estimated Expiration
2044-05-13

AI Technical Summary

Technical Problem

EPDM rubber has compression permanent deformation problems in high-temperature environments, and its high-temperature resistance is not as good as that of perfluoroether rubber, resulting in high production costs and limiting its use.

Method used

Using EPDM rubber and carbon black, nano-modified magnesium aluminum silicate, fumed silica, polytetrafluoroethylene micropowder, paraffin oil, stearic acid, zinc oxide, polyethylene glycol, vulcanizing agent and antioxidant The combined formula is modified to improve its high temperature resistance and processing performance and reduce compression permanent deformation.

Benefits of technology

It achieves long-term stable use of EPDM rubber in an environment of 200°C, reduces production costs, improves the high temperature resistance, tensile strength and hardness of the sealing material, and reduces compression permanent deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004837063060000051
    Figure BDA0004837063060000051
  • Figure BDA0004837063060000061
    Figure BDA0004837063060000061
  • Figure BDA0004837063060000071
    Figure BDA0004837063060000071
Patent Text Reader

Abstract

The present application relates to the technical field of ethylene propylene diene monomer rubber sealing material processing, and more specifically, to a low compression permanent deformation battery sealing material and a preparation method thereof, which is prepared from the following raw materials in parts by weight: 100 parts of ethylene propylene diene monomer rubber, 40-50 parts of carbon black, 25-30 parts of nano-modified aluminum magnesium silicate, 10-15 parts of fumed white carbon black, 5-6 parts of polytetrafluoroethylene micropowder, 8-12 parts of paraffin oil, 1-2 parts of stearic acid, 6-8 parts of zinc oxide, 3-5 parts of polyethylene glycol, 2-3 parts of a vulcanizing agent and 1-2 parts of an antioxidant. By using the above raw materials in common, the high temperature resistance and electrolyte resistance of the battery sealing material can be effectively improved, the permanent compression deformation of the battery sealing material can be reduced, and the battery sealing material can be used for a long time at high temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of EPDM rubber sealing material processing, and more specifically, to a low compression permanent deformation battery sealing material and a preparation method thereof. Background Art

[0002] The function of battery seals is to prevent the leakage of electrolyte inside the battery and the entry of external impurities into the battery, so that the battery can work normally. Rubber material itself has excellent elasticity and plasticity, and can effectively adapt to the deformation and vibration of the battery shell, thereby maintaining good sealing performance. Therefore, rubber is one of the commonly used materials for battery seals.

[0003] The rubber materials used for battery seals mainly include perfluoroether rubber and EPDM rubber. Among them, perfluoroether rubber has excellent high temperature resistance and acid and alkali resistance, and can work stably for a long time in a high temperature environment, but the processing performance of perfluoroether rubber is poor, and special processing methods and equipment are required, which is difficult to process. At the same time, the raw materials of perfluoroether rubber are expensive, resulting in high production costs for perfluoroether rubber battery seals, which limits the use of perfluoroether rubber. EPDM rubber is cheaper than perfluoroether rubber, but its high temperature resistance is not as good as perfluororubber, and its compression permanent deformation is high when used at high temperatures for a long time. Summary of the invention

[0004] In order to improve the high temperature resistance of EPDM rubber and reduce the compression permanent deformation of EPDM rubber, the present application provides a low compression permanent deformation battery sealing material and a preparation method thereof.

[0005] In a first aspect, the present application provides a low compression permanent deformation battery sealing material, which adopts the following technical solution: a low compression permanent deformation battery sealing material is prepared from the following raw materials in parts by weight:

[0006] EPDM 100 parts

[0007] Carbon black 40-50 parts

[0008] 25-30 parts of nano-modified magnesium aluminum silicate

[0009] Fumed silica 10-15 parts

[0010] 5-6 parts of polytetrafluoroethylene powder

[0011] 8-12 parts paraffin oil

[0012] 1-2 parts stearic acid

[0013] Zinc oxide 6-8 parts

[0014] 3-5 parts of polyethylene glycol

[0015] 2-3 parts of vulcanizing agent

[0016] 1-2 parts of antioxidant.

[0017] By adopting the above technical scheme, the prepared battery sealing material has low permanent compression deformation, good electrolyte resistance and high temperature resistance, can be used for a long time in an environment of 200°C without deformation, and has low manufacturing cost. In the present application, by using EPDM rubber together with carbon black, nano-modified aluminum magnesium silicate, fumed silica, polytetrafluoroethylene powder, paraffin oil, stearic acid, zinc oxide, polyethylene glycol, vulcanizing agent, coupling agent and antioxidant, the high temperature resistance and electrolyte resistance of EPDM rubber can be effectively improved, the permanent compression deformation of EPDM rubber can be reduced, and EPDM rubber can be used for a long time at high temperature, and the above raw material cost is low.

[0018] Polytetrafluoroethylene and nano-modified magnesium aluminum silicate can improve the high temperature resistance of EPDM rubber. Among them, nano-modified magnesium aluminum silicate has good high temperature resistance and will not decompose during use. Nano-modified magnesium aluminum silicate can undergo cross-linking reaction with EPDM rubber at high temperature, thereby increasing the stability and heat resistance of EPDM rubber, and can greatly improve the heat resistance of sealing materials, so that it can be used in an environment of 200°C. At the same time, nano-modified magnesium aluminum silicate has stable chemical properties, and is stable in both acidic and alkaline media. When used together with EPDM rubber, it can further improve the battery fluid resistance of sealing materials. Adding nano-modified magnesium aluminum silicate will further increase the processing difficulty of EPDM rubber. In this application, polyethylene glycol is added to improve the fluidity of nano-modified magnesium aluminum silicate in EPDM rubber, promote the full mixing of nano-modified magnesium aluminum silicate and EPDM rubber, improve the high temperature resistance, tensile strength and hardness of the sealing material, and reduce the compression permanent deformation of the sealing material.

[0019] Stearic acid can improve the uniform dispersion of various raw materials in EPDM rubber, penetrate into the EPDM rubber macromolecular chain to form a stable network structure, and improve the tensile strength, hardness and other mechanical properties of the sealing material.

[0020] Carbon black can effectively improve the hardness of EPDM, but too much carbon black will increase the compression set of EPDM. Therefore, in this application, by adding an appropriate amount of fumed silica and carbon black, the hardness of EPDM can be improved without increasing the compression set of EPDM. Vulcanizing agent and zinc oxide can increase the vulcanization speed and crosslinking degree, so that the vulcanization degree of EPDM is deeper and the compression set is smaller. Paraffin oil has good compatibility with EPDM and can improve the processing performance of EPDM.

[0021] Preferably, the EPDM rubber is a modified EPDM rubber, and the modified EPDM rubber is prepared by the following method:

[0022] A: mixing a silane coupling agent, cyclohexene-4,5-diglycidyl carboxylate and a solvent to obtain a mixed solution;

[0023] B: Mix the EPDM rubber and the mixed liquid, heat to 80-90°C, and then drip a solution containing an initiator at a dripping speed of 5-8g / min. After the dripping is completed, continue to keep warm and react for 4-6 hours, remove the solvent, and obtain modified EPDM rubber powder; the mass fraction of the solution containing the initiator is 30-40%.

[0024] By adopting the above technical scheme, the compatibility of EPDM rubber with carbon black, modified nano aluminum magnesium silicate and fumed white carbon black is further improved, while the processing performance and high temperature resistance of EPDM rubber are improved.

[0025] In the present application, the poor adhesion and processing performance of EPDM rubber are further improved by grafting cyclohexene-4,5-diglycidyl carboxylate, and the heat resistance and aging resistance of EPDM rubber are improved by introducing siloxane bonds, and its compatibility with carbon black, modified nano aluminum magnesium silicate, and fumed white carbon black is enhanced, thereby improving the heat resistance of the sealing material and reducing its compression permanent deformation. Through the preparation method in the present application, silane coupling agent and cyclohexene-4,5-diglycidyl carboxylate can be efficiently introduced, and the preparation process is simple and easy to operate.

[0026] Preferably, the weight parts of the raw materials used to prepare the modified EPDM rubber are as follows:

[0027] Silane coupling agent 10-15 parts

[0028] Cyclohexene-4,5-diglycidyl carboxylate 20-25 parts

[0029] Solvent 200-250 parts

[0030] 100 parts of EPDM rubber

[0031] Contains 10-20 parts of the solution of initiator.

[0032] By adopting the above technical scheme, the amount of raw materials used in the preparation of modified EPDM rubber is optimized, so that the grafting rate of EPDM rubber is high, and it is easier to mix evenly with carbon black, modified nano-aluminum magnesium silicate, and fumed silica, thereby improving the high temperature resistance, tensile strength and hardness of the sealing material, while reducing its compression permanent deformation.

[0033] Preferably, the silane coupling agent includes at least one of γ-(methacryloyloxy)propyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane and γ-methacryloyloxypropyltrimethoxysilane.

[0034] By adopting the silane coupling agent, the grafting rate of EPDM rubber is improved, so that the compatibility of EPDM rubber with carbon black, modified nano aluminum magnesium silicate and fumed white carbon black is better.

[0035] Preferably, the average particle size of the polytetrafluoroethylene powder is 5-40 μm.

[0036] By adopting the above technical solution, the average particle size of the polytetrafluoroethylene powder is further optimized, so that the polytetrafluoroethylene and the EPDM rubber can be fully mixed, so that the high temperature resistance of the sealing material is further improved and the compression permanent deformation is reduced.

[0037] Preferably, the ethylene content of the EPDM rubber is 40-60%, the Mooney viscosity ML (1+4) at 125° C. is 50-100, and the content of the third monomer is 5-10%.

[0038] By adopting the above technical solution, the parameters of EPDM rubber are optimized so that the EPDM rubber has appropriate fluidity during processing, which is beneficial to improving the processing performance of the EPDM rubber. More preferably, EPDM rubbers with different ethylene contents are used in combination.

[0039] Preferably, the average particle size of the carbon black is 50-100 nm, and the average particle size of the fumed silica is 200-400 nm.

[0040] By adopting the above technical solution, the average particle size of carbon black and fumed silica is optimized, the heat resistance, tensile strength and hardness of the sealing material are further improved, and the compression permanent deformation of the sealing material is reduced.

[0041] Preferably, the vulcanizing agent includes at least one of dicumyl peroxide, diisopropyl di-tert-butyl peroxide, N,N'-bisfurfurylideneacetone, 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

[0042] By adopting the above-mentioned vulcanizing agent, the processing performance of EPDM rubber can be greatly optimized. Even if a small amount is added, the cross-linking density of the sealing material can be increased, thereby improving the heat resistance, electrolyte resistance and mechanical strength of the sealing material, improving the electrolyte resistance and extending the service life of the product.

[0043] Preferably, the antioxidant includes at least one of 2,6-di-tert-butyl-4-methylphenol, styrenated diphenylamine, 2,2-bis-4-hydroxyphenyl-hexafluoropropane, 2,2-methylene-bis(4-methyl-6-tert-butylphenol), nickel dibutyl dithiocarbamate and 4,4-bis(2,2-dimethylbenzyl)diphenylamine.

[0044] By adopting the antioxidant, the heat resistance of EPDM rubber is improved, the aging of EPDM rubber is delayed, and the service life of the sealing material is further increased.

[0045] In a second aspect, the present application provides a method for preparing a low compression permanent deformation battery sealing material, using the following technical solution:

[0046] A method for preparing a low compression set battery sealing material comprises the following preparation steps:

[0047] S1. Mix EPDM rubber according to parts by weight for 5-10 min at a temperature of 40-50°C.

[0048] S2, mixing the mixed EPDM rubber with zinc oxide, polytetrafluoroethylene powder, stearic acid and a crosslinking agent, the mixing time is 5-10 minutes, the mixing temperature is 60-70° C., and a mixture A is obtained;

[0049] S3, mixing the mixture A with carbon black, fumed silica, paraffin oil, vulcanizing agent, nano-modified magnesium aluminum silicate and antioxidant for 10-15 min at a temperature of 60-70° C. to obtain a mixture B;

[0050] S4. The mixture B is vulcanized, wherein the vulcanization temperature of the primary vulcanization is 150-160° C., the vulcanization time is 5-10 min, and the vulcanization temperature of the secondary vulcanization is 120-140° C., the vulcanization time is 1-1.5 h, to obtain a low compression set battery sealing material.

[0051] By adopting the above technical solution, the above raw materials are fully mixed to obtain a sealing material with good high temperature resistance, tensile strength, electrolyte resistance and sealing performance, and low compression permanent deformation. The second stage vulcanization can further increase the crosslinking density, remove small molecules, and reduce the compression permanent deformation.

[0052] In summary, this application has the following beneficial effects:

[0053] 1. In the present application, by using EPDM rubber together with carbon black, nano-modified aluminum magnesium silicate, fumed silica, polytetrafluoroethylene powder, paraffin oil, stearic acid, zinc oxide, polyethylene glycol, vulcanizing agent, coupling agent and antioxidant, the high temperature resistance and electrolyte resistance of EPDM rubber can be effectively improved, the permanent compression deformation of EPDM rubber can be reduced, and the EPDM rubber can be used for a long time at high temperature.

[0054] 2. In the present application, ethylene propylene diene monomer rubber is modified by using silane coupling agent and cyclohexene-4,5-diglycidyl carboxylate, so that the compatibility of ethylene propylene diene monomer rubber with carbon black, modified nano aluminum magnesium silicate and fumed silica is improved, and the processing performance and heat resistance of ethylene propylene diene monomer rubber can also be improved. DETAILED DESCRIPTION

[0055] Example

[0056] In this application, the polytetrafluoroethylene powder was purchased from Suzhou Lutuo Materials Co., Ltd., with an average particle size of 5 μm and a brand name of Zonyl; the model of nano-modified magnesium aluminum silicate is SiliterN95, which was purchased from Lianyungang Ruiba Chemical Co., Ltd.

[0057] Example 1

[0058] A low compression permanent deformation battery sealing material is prepared by the following method:

[0059] S1. Mix 1000 g of EPDM rubber for 5 min at a temperature of 40°C.

[0060] S2, mixing the kneaded EPDM rubber with 60 g of zinc oxide, 50 g of polytetrafluoroethylene powder (average particle size of 5 μm) and 10 g of stearic acid, the mixing time is 5 min, the mixing temperature is 60° C., to obtain a mixture A;

[0061] S3, the mixture A was mixed with 400 g of carbon black (average particle size 50 nm), 100 g of fumed silica (average particle size 200 nm), 80 g of paraffin oil, 20 g of a vulcanizing agent (dicumyl peroxide), 250 g of nano-modified magnesium aluminum silicate and 10 g of an antioxidant (2,6-di-tert-butyl-4-methylphenol) for 15 min at a mixing temperature of 60° C. to obtain a mixture B;

[0062] S4. The mixture B is vulcanized. The vulcanization temperature of the primary vulcanization is 150° C. and the vulcanization time is 5 min. The vulcanization temperature of the secondary vulcanization is 120° C. and the vulcanization time is 1 h, to obtain a low compression set battery sealing material.

[0063] The ethylene content of the EPDM rubber is 40%, the Mooney viscosity ML (1+4) at 125° C. is 50, and the content of the third monomer is 10%.

[0064] The difference between Example 1 and Example 2-3 is that the types, amounts and parameters of some raw materials for preparing low compression set battery sealing materials are different. The specific differences are shown in Table 1:

[0065] Table 1 Types, amounts and parameters of raw materials for preparing low compression set battery sealing materials in Examples 1-3

[0066]

[0067]

[0068]

[0069] Example 4

[0070] A low compression permanent deformation battery sealing material, the difference between this embodiment and embodiment 1 is that the EPDM rubber is a modified EPDM rubber, and the modified EPDM rubber is prepared by the following method:

[0071] A: 100 g of silane coupling agent (γ-(methacryloyloxy)propyltrimethoxysilane), 200 g of cyclohexene-4,5-diglycidyl carboxylate and 2000 g of solvent (ethyl acetate) were mixed to obtain a mixed solution;

[0072] B: Mix 1000g of EPDM rubber and the mixed liquid, heat to 80°C, and then drop 100g of a solution containing an initiator (di-(tert-butylperoxyisopropyl)benzene) at a dropping rate of 5g / min. After the addition is completed, continue to keep warm and react for 4h, then remove the solvent to obtain a modified EPDM rubber powder; the mass fraction of the solution containing the initiator is 30%.

[0073] Example 5

[0074] A low compression permanent deformation battery sealing material, the difference between this embodiment and embodiment 2 is that the EPDM rubber is a modified EPDM rubber, and the modified EPDM rubber is prepared by the following method:

[0075] A: 120 g of a silane coupling agent (γ-mercaptopropyltriethoxysilane), 220 g of cyclohexene-4,5-diglycidyl carboxylate and 2300 g of a solvent (ethylene glycol ethyl ether) were mixed to obtain a mixed solution;

[0076] B: Mix 1000g of EPDM rubber and the mixed liquid, heat to 85°C, and then add 150g of a solution containing an initiator (tert-butyl isopropylbenzene peroxide) at a dropping rate of 6g / min. After the addition is completed, continue to keep warm and react for 5h, then remove the solvent to obtain a modified EPDM rubber powder; the mass fraction of the solution containing the initiator is 30%.

[0077] Example 6

[0078] A low compression permanent deformation battery sealing material, the difference between this embodiment and embodiment 3 is that the EPDM rubber is a modified EPDM rubber, and the modified EPDM rubber is prepared by the following method:

[0079] A: 150 g of silane coupling agent (γ-aminopropyltriethoxysilane), 250 g of cyclohexene-4,5-diglycidyl carboxylate and 2500 g of solvent (acetone) were mixed to obtain a mixed solution;

[0080] B: Mix 1000g of EPDM rubber and the mixed liquid, heat to 90°C, and then add 40g of a solution containing an initiator (ethyl 3,3-bis(tert-amylperoxy)butyrate) at a dropping rate of 8g / min. After the addition is completed, continue to keep warm and react for 6h, then remove the solvent to obtain a modified EPDM rubber powder; the mass fraction of the solution containing the initiator is 40%.

[0081] Example 7

[0082] A low compression permanent deformation battery sealing material, the difference between this embodiment and embodiment 4 is that a solvent is used to replace an equal amount of a silane coupling agent, and the amounts, types and experimental parameters of other raw materials are consistent with those of embodiment 4.

[0083] Example 8

[0084] A low compression permanent deformation battery sealing material, the difference between this embodiment and embodiment 4 is that: a solvent is used to replace an equal amount of cyclohexene-4,5-diglycidyl carboxylate, and the amount, type and experimental parameters of other raw materials are consistent with those of embodiment 4.

[0085] Example 9

[0086] A low compression permanent deformation battery sealing material, the difference between this embodiment and embodiment 4 is that the silane coupling agent is vinyl triethoxy silane, and the amount, type and experimental parameters of other raw materials are consistent with those of embodiment 4.

[0087] Example 10

[0088] A low compression permanent deformation battery sealing material, the difference between this embodiment and embodiment 4 is that maleic anhydride is used to replace an equal amount of cyclohexene-4,5-diglycidyl carboxylate, and the amount, type and experimental parameters of other raw materials are consistent with those of embodiment 4.

[0089] Embodiment 11

[0090] A low compression permanent deformation battery sealing material, the difference between this embodiment and embodiment 1 is that the average particle size of carbon black is 200nm, and the amount, type and experimental parameters of other raw materials are consistent with those in embodiment 1.

[0091] Comparative Example

[0092] Comparative Example 1

[0093] A battery sealing material. The difference between this comparative example and Example 1 is that silicon dioxide is used to replace nano-modified magnesium aluminum silicate, and the amounts, types and experimental parameters of other raw materials are consistent with those in Example 1.

[0094] Comparative Example 2

[0095] A battery sealing material. The difference between this comparative example and Example 1 is that silicon dioxide is used to replace an equal amount of carbon black, and the amounts, types and experimental parameters of other raw materials are consistent with those in Example 1.

[0096] Comparative Example 3

[0097] A sealing material. The difference between this comparative example and Example 1 is that polyimide is used to replace an equal amount of polytetrafluoroethylene powder, and the amounts, types and experimental parameters of other raw materials are consistent with those in Example 1.

[0098] Polyimide was purchased from Guangzhou Xichuan Plastic Raw Materials Co., Ltd. with the brand name PISP-1.

[0099] Comparative Example 4

[0100] A pool sealing material. The difference between this comparative example and Example 1 is that oleic acid is used to replace an equal amount of stearic acid, and the amounts, types and experimental parameters of other raw materials are consistent with those in Example 1.

[0101] Comparative Example 5

[0102] A low compression permanent deformation battery sealing material. The difference between this comparative example and Example 1 is that polyoxyethylene alkyl ether is used to replace an equal amount of polyethylene glycol, and the amount, type and experimental parameters of the other raw materials are consistent with those of Example 1.

[0103] Performance Testing The low compression permanent deformation battery sealing materials prepared in Examples 1-11 and the battery sealing materials prepared in Comparative Examples 1-5 were subjected to tensile strength tests, hardness tests, compression permanent deformation tests and hot air aging performance tests.

[0104] Detection method / test method

[0105] Tensile strength test: The tensile strength of the obtained battery sealing material was tested using the standard ASTM D412;

[0106] Hardness test: The hardness of the obtained battery sealing material was tested using the standard number ASTM D2240;

[0107] Compression permanent deformation: The compression permanent deformation of the obtained battery sealing material was tested using the standard number ASTM D395 (test method B, 120°C×70h, 25%);

[0108] Hot air aging performance was measured according to GB / T 3512, conditions: 200°C, 72h, and then tensile strength and hardness were tested; the experimental data are shown in Table 2:

[0109] Table 2 Experimental data of Examples 1-11 and Comparative Examples 1-5

[0110]

[0111]

[0112] It can be seen from Examples 1-11 and Comparative Examples 1-5 in combination with Table 2 that the low compression permanent deformation battery sealing material prepared by adopting the formula of the present application has good heat resistance, high tensile strength, good hardness, and low compression permanent deformation.

[0113] By comparing Example 1 with Comparative Example 1, the tensile strength and hardness of Comparative Example 1 are reduced, the compression permanent deformation is increased, and the tensile strength and hardness of Comparative Example 1 change greatly after the heat aging test, indicating that the addition of nano-modified aluminum magnesium silicate can further improve the high temperature resistance, tensile strength and hardness of the sealing material, while reducing the compression permanent deformation of the sealing material.

[0114] Comparing Example 1 with Comparative Example 2, the tensile strength and hardness of Comparative Example 2 remain substantially unchanged, but the compression set increases, indicating that the compression set of the sealing material can be effectively reduced by adding an appropriate amount of carbon black.

[0115] By comparing Example 1 with Comparative Examples 3-5, the tensile strength and hardness of Comparative Examples 3-5 are reduced, the compression permanent deformation is increased, and the tensile strength and hardness of Comparative Examples 3-5 change greatly after the heat aging test, indicating that the addition of polytetrafluoroethylene, stearic acid and polyethylene glycol is beneficial to improving the high temperature resistance, tensile strength and hardness of the sealing material, while reducing the compression permanent deformation of the sealing material.

[0116] Compared with Example 1 and Example 4, Example 2 and Example 5, and Example 3 and Example 6, the tensile strength and hardness of Examples 4-6 are improved, and the compression permanent deformation is reduced; and after the heat aging test, the tensile strength and hardness of Examples 4-6 change little, indicating that by modifying the EPDM rubber, the high temperature resistance, tensile strength and hardness of the sealing material can be effectively improved, while the compression permanent deformation of the sealing material can be reduced.

[0117] Compared with Example 4 and Example 7-10, the tensile strength and hardness of Example 7-9 are not as good as those of Example 4, and the compression permanent deformation of Example 7-10 is reduced more than that of Example 4; and after the heat aging test, the tensile strength and hardness of Example 4-9 change little; This shows that the modified EPDM rubber prepared in this application can effectively improve the high temperature resistance, tensile strength and hardness of the sealing material, while reducing the compression permanent deformation of the sealing material.

[0118] Compared with Example 1 and Example 11, the tensile strength and hardness of Example 11 are slightly improved, and the compression permanent deformation is slightly reduced, which shows that the performance of the sealing material is improved by optimizing the average particle size of carbon black and fumed silica.

[0119] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A low compression set battery sealing material, characterized in that: Prepared from the following raw materials in parts by weight: EPDM 100 parts Carbon black 40-50 parts 25-30 parts of nano-modified magnesium aluminum silicate Fumed silica 10-15 parts 5-6 parts of polytetrafluoroethylene powder 8-12 parts paraffin oil 1-2 parts stearic acid Zinc oxide 6-8 parts 3-5 parts of polyethylene glycol 2-3 parts of vulcanizing agent 1-2 parts of antioxidant; The EPDM rubber is a modified EPDM rubber, and the modified EPDM rubber is prepared by the following method: A: mixing a silane coupling agent, cyclohexene-4,5-diglycidyl carboxylate and a solvent to obtain a mixed solution; B: Mix the EPDM rubber and the mixed solution, heat to 80-90°C, and then drip a solution containing an initiator at a dripping speed of 5-8g / min. After the dripping is completed, continue to keep the temperature for 4-6 hours, remove the solvent, and obtain a modified EPDM rubber powder; the mass fraction of the solution containing the initiator is 30-40%; The weight parts of the raw materials used for preparing the modified EPDM rubber are as follows: Silane coupling agent 10-15 parts Cyclohexene-4,5-diglycidyl carboxylate 20-25 parts Solvent 200-250 parts EPDM 100 parts Contains 10-20 parts of the initiator solution.

2. The low compression set battery sealing material according to claim 1, characterized in that: The silane coupling agent includes at least one of γ-(methacryloyloxy)propyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane and γ-methacryloyloxypropyltrimethoxysilane.

3. The low compression set battery sealing material according to claim 1, characterized in that: The ethylene content of the EPDM rubber is 40-60%, the Mooney viscosity ML (1+4) at 125° C. is 50-100, and the content of the third monomer is 5-10%.

4. The low compression set battery sealing material according to claim 1, characterized in that: The vulcanizing agent includes at least one of diisopropylbenzene peroxide, diisopropyl di-tert-butyl peroxide, N,N'-difurfurylideneacetone, 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

5. The low compression set battery sealing material according to claim 1, characterized in that: The average particle size of the polytetrafluoroethylene powder is 5-40 μm.

6. The low compression set battery sealing material according to claim 1, characterized in that: The average particle size of the carbon black is 50-100 nm, and the average particle size of the fumed silica is 200-400 nm.

7. The low compression set battery sealing material according to claim 1, characterized in that: The antioxidant includes at least one of 2,6-di-tert-butyl-4-methylphenol, styrenated diphenylamine, 2,2-bis-4-hydroxyphenyl-hexafluoropropane, 2,2-methylene-bis(4-methyl-6-tert-butylphenol), nickel dibutyl dithiocarbamate and 4,4-bis(2,2-dimethylbenzyl)diphenylamine.

8. A method for preparing a low compression set battery sealing material according to any one of claims 1 to 7, characterized in that: The method comprises the following preparation steps: S1. Mix EPDM rubber according to parts by weight for 5-10 min at a temperature of 40-50°C. S2, mixing the mixed EPDM rubber with zinc oxide, polytetrafluoroethylene powder and stearic acid for 5-10 min at a mixing temperature of 60-70° C. to obtain a mixture A; S3, mixing the mixture A with insulating carbon black, fumed silica, paraffin oil, vulcanizing agent, nano-modified magnesium aluminum silicate and antioxidant, the mixing time is 10-15min, the mixing temperature is 60-70°C, to obtain a mixture B; S4. The mixture B is vulcanized, wherein the vulcanization temperature of the primary vulcanization is 150-160° C., the vulcanization time is 5-10 min, and the vulcanization temperature of the secondary vulcanization is 120-140° C., the vulcanization time is 1-1.5 h, to obtain a low compression set battery sealing material.