A short-process near-net-shape manufacturing method for ship hull steel plates

By using short-process near-net-shape manufacturing technology and controlling specific chemical compositions and processes, the problems of long production processes and high energy consumption in traditional ship hull steel plate production have been solved, enabling low-cost production of high-strength and high-toughness ship hull steel plates and improving production efficiency and material properties.

CN118326246BActive Publication Date: 2026-11-17BAOSHAN IRON & STEEL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310033302.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-10
Publication Date
2026-11-17
Estimated Expiration
2043-01-10

AI Technical Summary

Technical Problem

Existing steel plate manufacturing processes for ship hulls are lengthy and energy-intensive, making it difficult to achieve high strength and toughness in a shorter process, and they are also costly.

Method used

By employing short-process near-net-shape manufacturing technology, and controlling specific chemical compositions and process flows, including converter smelting, LF refining, VD refining, continuous casting and rolling of headless thin slabs, and laminar flow cooling, high-strength and high-toughness ship hull steel plates are prepared.

Benefits of technology

It has been achieved that high-strength (1100MPa~1150MPa) and high-toughness (≥14% elongation) hull steel plates can be obtained with low cost and low energy consumption, shortening the production process and improving production efficiency and material utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118326246B_ABST
    Figure CN118326246B_ABST
Patent Text Reader

Abstract

This invention discloses a short-process near-net-shape manufacturing method for ship hull steel plates, containing Fe and unavoidable impurity elements, as well as the following chemical elements in the following mass percentages: C: 0.06%–0.09%; Si: 0.1%–0.15%; Mn: 0.15%–0.25%; Ni: 5.5%–7%; Cr: 1.1%–1.5%; Mo: 0.6%–0.9%; Co: 5.5%–7.5%; V: 0.05%–0.08%; Nb: 0.05%–0.08%; Al: 0.06%–0.09%; Ti: 0.02%–0.03%. Correspondingly, this invention also discloses a method for manufacturing the short-process near-net-shape manufacturing method for ship hull steel plates. This invention improves the performance of steel used in shipbuilding by utilizing near-net-shape manufacturing technology while further reducing the production cost of ship hull steel plates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a type of steel and a method for manufacturing the same, and more particularly to a steel plate for ship hulls and a method for manufacturing the same. Background Technology

[0002] Shipbuilding has always been a significant part of heavy industry construction, and hull construction requires a large amount of steel plates. Traditional steel plate manufacturing processes for hulls are lengthy, discontinuous, and energy-intensive. To mass-produce related plates, the energy consumption for heating the casting billet alone accounts for 6% to 7% of the total energy consumption of the entire production process. Therefore, shortening the plate production process is an important means of achieving low-carbon and energy-saving production.

[0003] Furthermore, with the development of the shipbuilding industry, there is a desire for steel used in ship hull construction to achieve higher strength and toughness. Higher strength and toughness mean using less material under the same working conditions to achieve overall ship lightweighting, which in turn can reduce fuel consumption and carbon emissions.

[0004] Based on this, it is desirable to obtain a steel plate for ship hulls and a method for manufacturing the same, which can produce steel plates with high strength, high toughness and excellent mechanical properties by adopting a short-process manufacturing technology. Summary of the Invention

[0005] One of the objectives of this invention is to provide a short-process near-net-shape manufacturing method for ship hull steel plates. The aim is to improve the performance of steel used in shipbuilding by using near-net-shape manufacturing technology to further reduce the production cost of ship hull steel plates through short-process manufacturing of high-strength steel for ship hulls.

[0006] To achieve the above objectives, the present invention provides a steel plate for near-net-shape ship hull manufacturing via a short-process method, which contains Fe and unavoidable impurity elements, and further contains the following chemical elements in the following mass percentages:

[0007] C: 0.06% ~ 0.09%; Si: 0.1% ~ 0.15%; Mn: 0.15 ~ 0.25%; Ni: 5.5% ~ 7%; Cr: 1.1% ~ 1.5%; Mo: 0.6% ~ 0 .9%; Co: 5.5% to 7.5%; V: 0.05 to 0.08%; Nb: 0.05% to 0.08%; Al: 0.06% to 0.09%; Ti: 0.02% to 0.03%.

[0008] Accordingly, the present invention also provides a steel plate for near-net-shape ship hull manufacturing using a short-process method, wherein the mass percentage content of each chemical element is as follows:

[0009] C: 0.06%–0.09%; Si: 0.1%–0.15%; Mn: 0.15%–0.25%; Ni: 5.5%–7%; Cr: 1.1%–1.5%; Mo: 0.6%–0.9%; Co: 5.5%–7.5%; V: 0.05%–0.08%; Nb: 0.05%–0.08%; Al: 0.06%–0.09%; Ti: 0.02%–0.03%; balance Fe and unavoidable impurity elements.

[0010] The design principles for the chemical composition of the steel plates used in the short-process near-net-shape manufacturing of ship hulls described in this invention are as follows:

[0011] C: Carbon is the most common strengthening element in steel. It often exists in steel as a solid solution element and in the form of carbides. As the carbon content increases, the strength of steel increases rapidly, but the plasticity of the material decreases, especially the weldability deteriorates, which is not conducive to the subsequent processing and joining of the material. Therefore, this invention relates to controlling the carbon content in steel grades between 0.06% and 0.09% in order to obtain good processing and joining performance.

[0012] Silicon (Si): Silicon is an important strengthening element in steel. It often exists in a solid solution state in the matrix. Silicon has a strong affinity for oxygen. When the silicon content is high, SiO2 inclusions will exist in the matrix. SiO2 has irregular angular shape and often becomes a stress concentration area under stress, resulting in a significant reduction in the material's plasticity. Therefore, in this invention, the silicon content is controlled between 0.1% and 0.15%.

[0013] Mn: Manganese is an excellent deoxidizer and desulfurizer, playing a crucial role in controlling the sulfur content in the material matrix. Manganese strongly expands the austenite phase region and lowers the martensitic transformation temperature, thereby improving the hardenability of steel. The steel grade designed in this invention contains 0.15–0.25% Mn.

[0014] Ni: Nickel is a strong element that expands the austenite phase region. While nickel and iron can be infinitely dissolved in solid form, their atomic volumes still differ, easily causing lattice distortion in materials and thus reducing the diffusion rate of other elements, improving the hardenability of steel. It is a strong matrix strengthening element. The Ni content in this invention is 5.5%–7%. A higher Ni content ensures the strengthening ability of the matrix and the uniformity of the microstructure.

[0015] Cr: Chromium is an element that improves the hardenability of steel. It can form a continuous solid solution with iron to strengthen the matrix. Chromium has a strong affinity for carbon, and the various carbides formed play a role in second-phase strengthening. Since the steel used in this invention is in marine and atmospheric environments, the appropriate addition of chromium is beneficial to improving the corrosion resistance of the steel. Therefore, the Cr content in this invention is 1.1% to 1.5%.

[0016] Mo: When the molybdenum content is low, it forms complex carbides with carbon and other alloying elements, playing a role in second-phase strengthening. Furthermore, molybdenum combined with other alloying elements can improve the tempering stability of quenched steel. Since the steel grades involved in this invention require tempering for strengthening, ensuring good stability and preventing temper brittleness during tempering is crucial. Therefore, the Mo content in this invention is 0.6%–0.9%.

[0017] Co: Cobalt, along with nickel and manganese, can form continuous solid solutions with the matrix and is a strong matrix strengthening element. During heat treatment, it stabilizes martensite, thus maintaining the material's high strength and hardness. Therefore, it is often used in martensitic tempered steel. The Co content in this invention is 5.5% to 7.5%.

[0018] Vanadium (V) forms a continuous solid solution with iron, which strongly shrinks the austenite phase region. Vanadium has a strong affinity for carbon, nitrogen, and oxygen. In steel, it mainly exists in the form of carbides, nitrides, or oxides, forming a composite second phase with other elements. Because vanadium forms stable and refractory carbides, the steel maintains a fine-grained structure at higher temperatures, greatly reducing the overheating sensitivity of the steel. Based on this, the V content in this invention is 0.05-0.08%.

[0019] Niobium (Nb) has the effect of refining grain size, thereby achieving a comprehensive improvement in strength and toughness. Similar to elements such as titanium and vanadium, niobium has a good affinity for nitrogen and carbon, forming extremely stable compounds that act as a second-phase strengthening agent. When niobium is dissolved in the matrix in a solid solution state, it can improve the hardenability and tempering stability of steel. Based on this, the Nb content in this invention is 0.05%–0.08%.

[0020] Al: Aluminum has a strong affinity for oxygen and nitrogen, and is a deoxidizing and nitrogen-fixing agent in steelmaking. Aluminum strongly shrinks the austenite phase region in steel, refines the essential grains of steel, and increases the temperature of grain coarsening. However, when the content of solid-solution aluminum in steel exceeds a certain value, the austenite grains tend to grow and coarsen. Therefore, the Al content should be strictly controlled. In addition, aluminum has an adverse effect on the weldability and machinability of materials. Based on this, the Al content in this invention is 0.06% to 0.09%.

[0021] Ti: Titanium has a strong affinity for nitrogen, oxygen, and carbon, making it an excellent deoxidizing and degassing agent and an effective element for fixing nitrogen and carbon. The compound bond between titanium and carbon is extremely strong and highly stable. Titanium carbide particles can inhibit the growth and coarsening of steel grains, thereby increasing the coarsening temperature. Therefore, Ti is a good second-phase strengthening element. Based on this, the Ti content in this invention is 0.02% to 0.03%.

[0022] Furthermore, in the short-process near-net-shape manufacturing steel plate for ship hulls described in this invention, the mass percentage content of Co and Ni satisfies: Co+Ni≤14%.

[0023] Although both Co and Ni can improve the hardenability of steel and have a good grain refinement effect, the high price of Co and Ni means that adding large amounts would increase the cost of steel production. Therefore, this invention controls the total content of the two to be less than 14%.

[0024] Furthermore, in the unavoidable impurity elements of the short-process near-net-shape manufacturing steel plates for ship hulls described in this invention: S≤0.003%; P≤0.0028%.

[0025] In this invention, the unavoidable impurities are mainly sulfur (S) and phosphorus (P), and their content should be as low as possible. In some embodiments of this invention, S ≤ 0.003% and P ≤ 0.0028% can be controlled.

[0026] Furthermore, the microstructure of the short-process near-net-shape manufacturing steel plate for ship hulls described in this invention includes a tempered martensite matrix and dispersed nanoscale precipitates.

[0027] Furthermore, the nanoscale precipitated phases include Ni carbonitrides and Ti carbonitrides.

[0028] Furthermore, the thickness of the steel plate used for near-net-shape ship hull manufacturing in the short-process method described in this invention is 4mm-7mm.

[0029] Furthermore, the mechanical properties of the steel plate for ship hull manufacturing using the short-process near-net-shape method described in this invention meet the following requirements: its yield strength is 1100MPa~1150MPa, its tensile strength is 1200MPa~1250MPa, and its elongation is ≥14%.

[0030] Another object of the present invention is to provide a method for manufacturing steel plates for ship hulls using a short-process near-net-shape manufacturing process, comprising the following steps:

[0031] (1) Converter smelting, LF refining, VD refining, and then direct drawing to obtain 90mm~100mm thick steel billets in the continuous casting step.

[0032] (2) Hot rolling: The total reduction rate is controlled at 92-96% to obtain a microstructure matrix of ferrite + granular bainite in the rolled plate;

[0033] (3) Laminar flow cooling in-line quenching;

[0034] (4) Winding;

[0035] (5) Tempering.

[0036] Near-net-shape manufacturing technology is a short-process steel production technology. Among them, continuous casting and rolling of headless thin slabs is a near-net-shape manufacturing technology, characterized by its short process and low cost. The continuous casting machine used in this invention employs a parallel-plate straight-arc crystallizer, and the slab is guided by a casting-rolling structure. After being pressed down by a liquid core, the slab directly enters the primary rolling mill to be rolled into medium-thick plates, and then into thin plates by the finishing mill. The subsequent laminar cooling process can complete part of the tempering process, and after shearing, it can directly enter the subsequent tempering treatment, thus significantly shortening the traditional casting and hot rolling processes.

[0037] The method described in this invention employs near-net-shape manufacturing technology. After molten steel undergoes converter smelting, LF refining, and VD refining, it is directly drawn into thick steel billets using continuous casting without a head. The steel billets are then hot-rolled with a large reduction to obtain hot-rolled plates. The large reduction rolling process breaks down the grains and microstructure, resulting in a microstructure beneficial to performance.

[0038] Furthermore, in step (1) of the manufacturing method described in this invention, the casting speed is controlled to be 4.0 m / min to 5.5 m / min during continuous casting.

[0039] Furthermore, in step (2) of the manufacturing method described in this invention, the roughing rolling start temperature is controlled at 1200℃~1250℃, the roughing rolling exit temperature is controlled at 1080℃~1150℃; the finishing rolling start temperature is controlled at 1000℃~1040℃, the finishing rolling finish temperature is controlled at 850℃~900℃, and after finishing rolling, the temperature is held at 850℃~900℃ for 3-10 seconds.

[0040] In some embodiments of the present invention, the finishing rolling temperature is controlled at 850°C to 900°C, which facilitates dynamic grain recovery and reduces deformation texture. Finally, combined with post-coiling heat treatment, the uniformity of the material's microstructure can be improved, further enhancing the steel plate's performance.

[0041] Furthermore, in step (3) of the manufacturing method described in this invention, laminar cooling is performed to 260°C to 300°C.

[0042] Furthermore, in step (4) of the manufacturing method described in this invention, the winding temperature is 200°C to 250°C.

[0043] Furthermore, in step (5) of the manufacturing method described in this invention, the tempering temperature is 500°C to 550°C.

[0044] The short-process near-net-shape manufacturing method for ship hulls described in this invention has the following characteristics and beneficial effects:

[0045] The short-process near-net-shape manufacturing method for ship hull steel plates described in this invention has continuity and adjustability.

[0046] In the short-process near-net-shape manufacturing method for ship hull steel plates described in this invention, converter smelting and LF refining are combined, resulting in molten steel with high cleanliness and precise composition control. The billet solidifies rapidly, thus exhibiting minimal compositional segregation and a uniform microstructure. Water quenching cooling is achieved during continuous rolling, shortening the length of subsequent heat treatment processes and reducing energy consumption.

[0047] Through the control of composition and process, the present invention obtains steel plates with uniform structure and stable performance. The yield strength Rp0.2 of the finished product is 1100MPa~1150MPa, the tensile strength Rm is 1200MPa~1250MPa, and the elongation A≥14.0%.

[0048] This invention obtains a nanoscale second phase through the control of composition and process, which has a good effect on the optimization of material strength and the control of microstructure.

[0049] Compared with existing technologies, this invention is the first to use near-net-shape technology to manufacture steel plates for shipbuilding. Its continuous casting billet thickness is controllable, the rolled plate thickness is controllable, and the dimensional accuracy is high. It can greatly shorten the gap between processes such as smelting, casting, cutting, heating, and rolling in traditional production. It has the characteristics of low heat loss and high production efficiency, and has high social and economic benefits. Attached Figure Description

[0050] Figure 1 The microstructure diagram of the steel plate used for near-net-shape manufacturing of ship hulls in the short-process method of Embodiment 2 of this case is shown.

[0051] Figure 2 This image shows nanoscale precipitates (transmission bright-field image) of the steel plate for hull manufacturing using the short-process near-net-shape method in Example 2 of this case. Detailed Implementation

[0052] The following will further explain and illustrate the steel plate for near-net-shape ship hull manufacturing and its manufacturing method according to the present invention, with reference to the accompanying drawings and specific embodiments. However, this explanation and illustration do not constitute an undue limitation on the technical solution of the present invention.

[0053] Examples 1-8

[0054] The short-process near-net-shape manufacturing steel plates for ship hulls described in Examples 1-8 of this invention are obtained using the following steps:

[0055] (1) Batching and pretreatment of molten iron;

[0056] (2) Converter smelting: Top and bottom blowing converter smelting, tapping temperature is 1600~1630℃; tapping slag thickness is controlled within 40mm; tapping carbon content is controlled within 0.1%;

[0057] (3) LF refining: The internal O content in the molten steel is controlled to be within 30ppm by LF refining, and the refining time can be 30min.

[0058] (4) VD refining: During the VD refining process, the vacuum degree inside the furnace is maintained at 60Pa to 80Pa for 15min to 20min, while argon gas at 0.3 to 0.45MPa is used for blowing and stirring. After the VD vacuum stirring is completed, Ti wire is fed in, and then a soft blowing operation at 0.25MPa for 10min to 15min is performed. The final outlet temperature is 1580℃ to 1600℃.

[0059] (5) Continuous casting: Directly draw to obtain a steel billet with a thickness of 90mm to 100mm, a billet width of 1800mm to 2000mm, and a drawing speed of 4.0m / min to 5.5m / min; the chemical element composition of the billet is shown in Table 1;

[0060] (6) Hot rolling: Rough rolling of continuously cast billet → rotary drum shear → induction heating → finish rolling; the rough rolling start temperature is 1200℃~1250℃, and the rough rolling exit thickness is 65mm; after several passes, for example, three passes of rough rolling, the exit rolling temperature is 1080℃~1150℃, and the exit thickness is 25mm~30mm; after rough rolling, the head is cut off by a rotary drum shear to keep the head flat; then high-pressure water descaling is used to remove the oxide scale from the surface after rough rolling to prevent it from being pressed into the surface, and the water pressure is maintained at 15MPa~20MPa; then induction heating is performed to finish the rough rolling. The slab is heated to 1000℃~1040℃ for finish rolling; the initial temperature of finish rolling is controlled at 1000℃~1040℃, and the exit thickness is 15mm~20mm; the final temperature of finish rolling is 850℃~900℃, and the exit thickness is 4mm~7mm; after finish rolling, the slab is kept at 850℃~900℃ for 3s~10s in an insulation hood to ensure that the rolled plate has sufficient time to achieve recovery and recrystallization processes; the total reduction rate of the hot rolling process is controlled at 92~96%, and the microstructure of the rolled plate is ferrite + granular bainite.

[0061] (7) Laminar flow cooling online quenching: The steel plate is rapidly cooled to 260℃~300℃ by water spraying to achieve the quenching effect;

[0062] (8) Winding: The winding temperature is 200℃~250℃, followed by flying shearing to separate the windings;

[0063] (9) Tempering: The steel coil is placed directly into a holding furnace at 500℃~550℃ and held for 1~2 hours. Then it is taken out and cooled naturally to remove quenching stress, reduce hard and brittle martensite structure, and obtain tempered martensite.

[0064] For example, Figure 1This shows a microstructure diagram of the steel plate used in the short-process near-net-shape manufacturing of ship hulls in Example 2 of this case.

[0065] from Figure 1 As can be seen, the microstructure of the finished steel plate is tempered martensite.

[0066] Figure 2 This illustrates the nanoscale precipitates in the short-process near-net-shape manufacturing of ship hull steel plates in Example 2 of this case.

[0067] This invention employs near-net-shape manufacturing technology to produce steel for shipbuilding. The carbon content is strictly controlled during the smelting process, and Ni and Ti elements are added to facilitate the formation of near-net-shape steel during smelting. Figure 2 The Ni and Ti carbonitrides shown have high melting points and short formation times. This invention can achieve second-phase reinforcement through such fine and dispersed second phases.

[0068] Table 1 lists the mass percentage of each chemical element in the steel plates for near-net-shape ship hull manufacturing in Examples 1-8.

[0069] Table 1. (wt%, balance Fe and other unavoidable impurities besides S and P)

[0070]

[0071] It should be noted that the Co+Ni mass percentage content in Examples 5 and 8 of the present invention exceeds 14%, therefore, although better mechanical properties can be obtained compared with other examples, the cost is higher.

[0072] Table 2 lists the specific process parameters for the short-process near-net-shape manufacturing of ship hull steel plates in Examples 1-8.

[0073] Table 2.

[0074]

[0075] To verify the implementation effects of each embodiment, the steel plates for ship hull manufacturing obtained from the short-process near-net-shape manufacturing of each embodiment of the present invention were subjected to tensile tests to determine their mechanical properties according to GB / T228.-2010 Metallic Materials - Tensile Testing - Part 1: Test Method at Room Temperature. The mechanical properties were measured according to JIS13A standard for processing tensile samples. Rp0.2 is the yield strength value with stress value that produces 0.2% residual deformation, and A% is the elongation. The mechanical property test results of each embodiment are listed in Table 3 below.

[0076] Table 3.

[0077]

[0078] As can be seen from Table 3 above, the steel plates for near-net-shape ship hull manufacturing using the short-process method of the present invention (Examples 1-8) all possess excellent mechanical properties, with yield strengths ≥1100MPa, tensile strengths ≥1200MPa, and elongations ≥14%. Therefore, the steel plates for near-net-shape ship hull manufacturing using the short-process method of the present invention achieve excellent mechanical properties under the premise of low cost, low energy consumption, and short manufacturing process.

[0079] It should be noted that the combination of the technical features in this case is not limited to the combination methods described in the claims of this case or the combination methods described in the specific embodiments. All technical features described in this case can be freely combined or combined in any way, unless they contradict each other.

[0080] It should also be noted that the embodiments listed above are merely specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made thereto are those that can be directly derived or easily conceived by those skilled in the art from the content disclosed in the present invention, and should all fall within the protection scope of the present invention.

Claims

1. A short flow near-net shape manufacturing hull steel sheet containing Fe and inevitable impurity elements, characterized by, It also contains the following chemical elements in the following mass percentages: C: 0.06%~0.09%; Si: 0.1%~0.15%; Mn: 0.15~0.25%; Ni: 5.5%~7%; Cr: 1.1%~1.5%; Mo: 0.6%~0.9%; Co: 5.5%~7.5%; V: 0.05~0.08%; Nb: 0.05%~0.08%; Al: 0.06%~0.09%; Ti: 0.02%~0.03%; The mass percentage content of Co and Ni satisfies the following condition: Co + Ni ≤ 14%.

2. The steel plate for ship hull manufacturing using a short-process near-net-shape method as described in claim 1, characterized in that, Its mass percentage content of each chemical element is as follows: C: 0.06%~0.09%; Si: 0.1%~0.15%; Mn: 0.15~0.25%; Ni: 5.5%~7%; Cr: 1.1%~1.5%; Mo: 0.6%~0.9%; Co: 5.5%~7.5%; V: 0.05~0.08%; Nb: 0.05%~0.08%; Al: 0.06%~0.09%; Ti: 0.02%~0.03%; balance is Fe and unavoidable impurity elements.

3. The steel plate for near-net-shape manufacturing of ship hulls via a short-process method as described in claim 1 or 2, characterized in that, Among unavoidable impurity elements: S≤0.003%; P≤0.0028%.

4. The steel plate for near-net-shape ship hull manufacturing via a short-process method as described in claim 1 or 2, characterized in that, Its microstructure includes a tempered martensite matrix and diffusely distributed nanoscale precipitates.

5. The steel plate for ship hull manufacturing using a short-process near-net-shape method as described in claim 4, characterized in that, The nanoscale precipitated phases include Ni carbonitrides and Ti carbonitrides.

6. The steel plate for near-net-shape manufacturing of ship hulls via a short-process method as described in claim 1 or 2, characterized in that, Its thickness is 4mm~7mm.

7. The steel plate for near-net-shape manufacturing of ship hulls via a short-process method as described in claim 1 or 2, characterized in that, Its mechanical properties meet the following requirements: yield strength of 1100MPa~1150MPa, tensile strength of 1200MPa~1250MPa, and elongation ≥14%.

8. The method for manufacturing steel plates for ship hulls using a short-process near-net-shape manufacturing method as described in any one of claims 1-7, characterized in that, Including the following steps: (1) Converter smelting, LF refining, VD refining, and then direct drawing to obtain 90mm~100mm thick steel billets in the continuous casting step; (2) Hot rolling: The total reduction rate is controlled at 92~96% to obtain a microstructure matrix of ferrite + granular bainite in the rolled plate; (3) Laminar flow cooling online quenching; (4) Winding up; (5) Tempering.

9. The manufacturing method as described in claim 8, characterized in that, In step (1), the casting speed is controlled to be 4.0 m / min to 5.5 m / min during continuous casting.

10. The manufacturing method as described in claim 8, characterized in that, In step (2), the roughing rolling start temperature is controlled at 1200℃~1250℃, the roughing rolling exit temperature is controlled at 1080℃~1150℃; the finishing rolling start temperature is controlled at 1000℃~1040℃, the finishing rolling end temperature is controlled at 850℃~900℃, and after finishing rolling, the temperature is held at 850℃~900℃ for 3-10 seconds.

11. The manufacturing method as described in claim 8, characterized in that, In step (3), laminar cooling is performed to 260°C~300°C.

12. The manufacturing method as described in claim 8, characterized in that, In step (4), the winding temperature is 200℃~250℃.

13. The manufacturing method as described in claim 8, characterized in that, In step (5), the tempering temperature is 500℃~550℃.

Citation Information

Patent Citations

  • In-situ nanoparticle reinforced ultra-high-strength steel for ocean engineering and preparation method

    CN113249654A