A chemical conversion film for improving the bonding strength of paint film on magnesium alloy surface and preparation method thereof
By forming a high-roughness, dense chemical conversion film layer on the surface of the magnesium alloy, the problems of poor bonding force between the magnesium alloy surface and the paint and insufficient corrosion resistance are solved, achieving more stable coating adhesion and extending the life of the product.
Patent Information
- Application Number
- CN202410767044.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-14
AI Technical Summary
The natural oxide film on the surface of magnesium alloy is highly alkaline and is difficult to combine well with organic paint films. It is also prone to corrosion in a wet environment, resulting in unstable coating bonding force.
By introducing a fluorine-containing treatment liquid that can directly react with the magnesium alloy matrix, a high-roughness, dense chemical conversion film layer is formed, including a porous layer and a covering layer, which improves the surface structure of the magnesium alloy and enhances the bonding force with the coating.
Significantly improves the bonding strength and corrosion resistance of magnesium alloy surface coatings, ensuring that the coating is not prone to peeling or cracking during long-term use and extending the service life of magnesium alloy products.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional coatings, and in particular to a chemical conversion film for improving the bonding strength of a paint film on a magnesium alloy surface and a preparation method thereof. Background Art
[0002] The coating of magnesium alloy surface can greatly improve the corrosion resistance. Without any treatment, a natural oxide film will form on the surface of magnesium alloy substrate. The natural oxide film has strong alkalinity and it is difficult for organic paint film to obtain good bonding strength on it. At the same time, directly coating the organic paint film on the surface of magnesium alloy bare material, even if the dry bonding strength meets the index requirements, in the wet environment of concrete, once water penetrates the organic paint film, the magnesium oxide at the interface of magnesium alloy and organic paint film will react with water to become magnesium hydroxide. Magnesium hydroxide is slightly soluble in water and cannot exist in a stable solid state, causing the wet bonding strength of the organic paint film to deteriorate rapidly.
[0003] A chemical conversion film with high bonding strength, high corrosion resistance, high stability and high roughness is formed by in-situ reaction on the surface of the magnesium alloy as the bottom layer of the organic coating. The conversion film is formed by the in-situ reaction of the magnesium alloy substrate, and is chemically or even metallurgically bonded to the substrate, with strong bonding strength. At the same time, the conversion film itself has high density, high stability in an alkaline environment, and its surface has high roughness, which provides mechanical bite points for the surface organic coating and effectively improves the bonding strength of the organic coating. During the high-temperature curing process of the powder coating, the chemical conversion film has stable performance and is chemically bonded to the surface organic coating through active bonds. The surface of the conversion film generated by the traditional magnesium alloy surface chemical conversion process is prone to floating dust. If it is not removed, it will greatly affect the bonding strength of the subsequent coating on the magnesium alloy. Summary of the invention
[0004] In order to overcome the shortcomings of the prior art, the purpose of the present application is to provide a chemical conversion film that improves the bonding strength of the paint film on the surface of the magnesium alloy. By introducing a fluorine-containing treatment liquid that can directly react with the magnesium alloy matrix, a high-roughness, high-stability, and high-density magnesium alloy surface structure is constructed to improve the bonding strength between the magnesium alloy surface and the coating.
[0005] To solve the above problems, the technical solutions adopted in this application are as follows:
[0006] An embodiment of the present application provides a chemical conversion film for improving the bonding strength of the paint film on the surface of a magnesium alloy. A fluorine-containing treatment liquid that can directly react with a magnesium alloy substrate is introduced to form a roughened film layer structure on the surface of the magnesium alloy substrate. The film layer structure includes a porous layer located on the surface of the magnesium alloy substrate and a covering layer located on the surface of the porous layer. The roughness of the film layer structure is 2.0-4.0 μm. The bonding strength of the film layer structure with the paint film after spraying is 20-30 MPa.
[0007] As a further preferred scheme, the fluorine-containing treatment liquid described in the embodiment of the present application includes a film-forming agent, an auxiliary film-forming agent and a film-forming promoter; wherein the mass ratio of the film-forming agent, the auxiliary film-forming agent and the film-forming promoter is (5-30):1:(5-15).
[0008] As a further preferred scheme, the film-forming agent described in the embodiment of the present application is one or a mixture of two or more of disodium hydrogen phosphate, sodium dihydrogen phosphate, and trisodium phosphate; the auxiliary film-forming agent is one or a mixture of two or more of fluoroboric acid, ammonium fluoride, and sodium fluorosilicate; the film-forming promoter is one or a mixture of two or more of manganese oxalate, manganese chloride, and disodium manganese ethylenediaminetetraacetate.
[0009] As a further preferred solution, the porosity of the porous layer described in the embodiment of the present application is 35%-55%.
[0010] As a further preferred solution, the covering layer described in the embodiment of the present application contains elements such as Mn, P, F, etc., the porosity of the covering layer is less than 1%, and the thickness of the covering layer is 10-15 μm.
[0011] The embodiment of the present application also provides a method for preparing a chemical conversion film that improves the bonding strength of the paint film on the surface of the magnesium alloy. Through treatments such as degreasing, activation, and immersion in a treatment liquid, a rough structure is formed on the surface of the magnesium alloy, making it present a "cauliflower flake-like" structure at the microscopic level, and avoiding the appearance of floating dust and the like on the surface of the conversion film.
[0012] The preparation method described in the embodiment of the present application comprises the following steps:
[0013] Degreasing treatment: Use alkaline solution to degreasing the surface of magnesium alloy substrate to remove oil stains and impurities on the surface;
[0014] Surface activation: Use acid to activate the surface of the magnesium alloy substrate after degreasing to remove oxides and impurities on the surface;
[0015] Film-forming reaction: the magnesium alloy substrate after surface activation is immersed in a fluorine-containing treatment solution, the immersion temperature is controlled to be 50-70° C., and the immersion time is 10-20 minutes to form a chemical conversion film on the surface of the magnesium alloy.
[0016] As a further preferred scheme, the oil removal treatment step described in the embodiment of the present application is to use alkaline solution to remove oil at 55-70°C for 3-5 minutes; the alkaline solution includes sodium hydroxide and a surfactant, wherein the amount of sodium hydroxide and the surfactant is 10-20g / L and 3-5g / L respectively.
[0017] As a further preferred scheme, in the surface activation treatment described in the embodiment of the present application, the magnesium alloy substrate is washed with an acid solution at room temperature for 10-15s, and then washed with clean water after being taken out; the acid solution used includes an organic acid and a surfactant, and the amounts of the organic acid and the surfactant are 10-30g / L and 0.1-1g / L, respectively.
[0018] As a further preferred scheme, the surfactant described in the embodiment of the present application is one or a mixture of two or more of cetyltrimethylammonium bromide, sodium dodecylbenzene sulfonate, sodium 2-ethylhexyl sulfate, and fatty alcohol polyoxyethylene ether; the organic acid is one or a mixture of two or more of formic acid, acetic acid, and citric acid.
[0019] As a further preferred scheme, the fluorine-containing treatment liquid described in the embodiment of the present application includes a film-forming agent, an auxiliary film-forming agent and a film-forming promoter; the film-forming agent is one of disodium hydrogen phosphate, sodium dihydrogen phosphate, and trisodium phosphate, or a mixture of two or more thereof, the auxiliary film-forming agent is one of fluoroboric acid, ammonium fluoride, and sodium fluorosilicate, or a mixture of two or more thereof, and the film-forming promoter is one of manganese oxalate, manganese chloride, and disodium manganese ethylenediaminetetraacetate, or a mixture of two or more thereof.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The chemical conversion film provided in the embodiment of the present application has a high roughness. This roughened surface not only increases the surface area, but also provides more attachment points for subsequent paint or coating, thereby significantly improving the bonding force between the coating and the magnesium alloy substrate. The high roughness also helps to improve the wettability and fluidity of the coating, making the coating more uniform and smooth.
[0022] 2. The chemical conversion film described in this application has high stability. The covering layer located on the porous layer is a key part of the film structure. The covering layer is formed by a fluorine-containing treatment liquid that directly reacts with the magnesium alloy substrate, is tightly bonded to the substrate, and has high stability. It can resist the influence of adverse factors such as chemical corrosion, mechanical wear and temperature changes, thereby extending the service life of the magnesium alloy product.
[0023] 3. The chemical conversion film described in this application has high density and can prevent the corrosion of water, oxygen and other corrosive media in the external environment to the magnesium alloy substrate, thereby improving the corrosion resistance of the magnesium alloy; at the same time, the dense layer can also reduce the gaps and defects between the coating and the substrate, further improving the adhesion and durability of the coating.
[0024] 4. The chemical conversion film described in this application has excellent bonding strength. Since the film layer structure has high roughness, high stability and high density, its bonding strength with the paint or coating is also correspondingly improved. Experimental data show that the bonding strength of the film layer structure with the paint film on the surface of the magnesium alloy substrate is greater than 28MPa; this excellent bonding strength can ensure that the coating is not easy to peel off or crack during long-term use, thereby improving the reliability and durability of magnesium alloy products.
[0025] 5. In the preparation method of the chemical conversion film described in the present application, the surface of the magnesium alloy substrate is degreased by alkaline solution, which can completely remove the oil and impurities on the surface, ensuring the smooth progress of the subsequent processing steps. The surface of the magnesium alloy substrate after degreasing is activated by acid solution, which can remove the oxides and impurities on the surface, and at the same time improve the activity and wettability of the surface, which is conducive to the formation of a bonding film layer structure. The magnesium alloy substrate is immersed in a fluorine-containing treatment solution, and by controlling the immersion temperature and time, a film layer with a specific structure and performance can be formed on the surface of the magnesium alloy substrate. This film layer structure can significantly improve the corrosion resistance and wear resistance of the magnesium alloy, and improve its bonding with the coating.
[0026] The present invention is further described in detail below in conjunction with specific implementation modes. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The organizational structure diagram of the chemical conversion film described in Example 1;
[0028] Figure 2 is a diagram of the organizational structure of the chemical conversion film described in Example 2;
[0029] Figure 3 The organizational structure diagram of the chemical conversion film described in Example 3;
[0030] Figure 4 The organizational structure diagram of the chemical conversion film described in Comparative Example 1;
[0031] Figure 5 The organizational structure diagram of the chemical conversion film described in Comparative Example 2;
[0032] Figure 6 The organizational structure diagram of the chemical conversion film described in Comparative Example 3;
[0033] Figure 7 It is a comparison chart of the salt spray test results of the chemical conversion film described in Example 1 and Comparative Example 1, wherein A is the salt spray test result of Comparative Example 1, and B is the salt spray test result of Example 1. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0035] The term "comprising" and other equivalent descriptions involved in the specification and claims of this application are intended to cover non-exclusive inclusions, including both the contents clearly described in the specification and claims, and the steps or units that are not described in the specification and claims but are inherent in the product, method or structure.
[0036] The embodiment of the present application provides a chemical conversion film, which forms a roughened film layer structure on the surface of the magnesium alloy substrate by introducing a fluorine-containing treatment liquid that can directly react with the magnesium alloy substrate. On the one hand, the roughened surface increases the surface area of the magnesium alloy substrate, provides more attachment points for the coating or coating, can significantly improve the bonding force between the coating or coating and the substrate, and ensure that the coating or coating is not easy to peel off or crack; on the other hand, the roughened surface has better wettability, which is conducive to the full contact and reaction between the conversion film forming liquid and the substrate surface, and helps to form a uniform and dense conversion film layer, thereby improving the quality and performance of the conversion film; in addition, the roughened surface can form an uneven microstructure, which can block the penetration and erosion of corrosive media (such as water, oxygen, etc.), and at the same time, the conversion film itself also has a certain corrosion resistance. The combination of the roughened surface and the coating or coating can further improve the corrosion resistance of the magnesium alloy. In the embodiment of the present application, the roughened film layer structure actually includes a double-layer structure, which includes a porous layer located on the surface of the magnesium alloy substrate and a covering layer on the surface. In the embodiments of the present application, the porous layer mainly provides an in-situ growth point for the covering layer; the covering layer is formed by a fluorine-containing treatment liquid that directly reacts with the magnesium alloy substrate, and is mainly composed of compounds generated by the reaction of the fluorine-containing treatment liquid and the magnesium alloy, which can resist the influence of adverse factors such as chemical corrosion, mechanical wear and temperature changes, and the covering layer presents a cauliflower-like structure, which is conducive to subsequent bonding with a coating or coating. The roughness of the film layer structure is 2.0-4.0μm. This high-roughness surface helps to improve the bonding between the paint film and the substrate. The bonding strength of the film layer structure with the paint film after spraying the paint film is 20-30MPa. Controlling the bonding strength between the film layer structure and the magnesium alloy substrate can ensure that the coating is not easy to peel off or crack during long-term use, thereby improving the reliability and durability of magnesium alloy products.
[0037] As a further preferred solution, the fluorine-containing treatment liquid described in the embodiment of the present application includes a film-forming agent, an auxiliary film-forming agent and a film-forming accelerator.
[0038] The film former is the main component of the chemical conversion film. It can react on the surface of the magnesium alloy to form a dense film layer. This film layer not only has good corrosion resistance, but also improves the bonding force between the magnesium alloy substrate and the coating. The auxiliary film former plays an auxiliary role in the formation of the chemical conversion film, such as adjusting the pH value of the solution, controlling the reaction rate, etc., which helps to form a uniform and dense film layer and improve the performance of the chemical conversion film. The film promoter can accelerate the formation process of the chemical conversion film, shorten the film formation time, and improve the performance of the film layer. The film promoter can play a role by increasing the ion concentration in the solution, reducing the reaction activation energy, etc. The film former used in the embodiment of the present application is phosphate. First, the selection of phosphate as a film-forming agent can form a layer of phosphate chemical conversion film, namely, phosphating film, on the surface of magnesium alloy through chemical reaction. This phosphating film is tightly bonded to the base metal, which can significantly improve the wear resistance and corrosion resistance of the magnesium alloy surface and provide a high-quality adhesion basis for subsequent coatings; secondly, the phosphating film formed by the phosphate film-forming agent has a certain roughness, which can increase the contact area between the coating and the substrate and improve the adhesion of the coating. At the same time, the rough surface can also increase the mechanical bite force of the coating, making the coating more firm; thirdly, the phosphating film can effectively prevent the magnesium alloy from contacting the corrosive medium in the external environment and reduce the occurrence of corrosion reactions. The phosphate component can react with the ions in the corrosive medium to form a protective isolation layer, further improving the corrosion resistance of the magnesium alloy. Further, in the embodiments of the present application, it is found that within the appropriate concentration range of the phosphate film-forming agent, as the concentration increases, the chemical conversion film formed is more compact, and can better isolate the contact between the base metal and the external corrosive medium, which is beneficial to improve the corrosion resistance of the film layer, and the appropriate concentration helps to form a film layer that is closely bonded to the substrate and improves adhesion; however, if the concentration is too high, it may cause the film layer to be too thick and have internal defects, which will reduce the corrosion resistance and affect the bonding between the film layer and the substrate. The concentration of the phosphate film-forming agent is a key factor affecting the thickness of the chemical conversion film. As the concentration increases, the thickness of the film layer will also increase accordingly, but an overly thick film layer may cause an increase in internal stress and reduce the stability of the film layer. The concentration of the phosphate film-forming agent will also affect the size and organizational morphology of the grains in the chemical conversion film. The appropriate concentration helps to form fine grains, making the film layer more compact. Too high or too low a concentration may cause the grain size to increase, resulting in defects such as unevenness and looseness in the film layer, affecting the performance of the film layer. Therefore, in the embodiments of the present application, the amount of the phosphate film-forming agent is 10 g / L-30 g / L; in other embodiments, the amount of the phosphate film-forming agent is 15 g / L-22 g / L, or 20 g / L-25 g / L. The phosphate film-forming agent can be selected from, but not limited to, disodium hydrogen phosphate, sodium dihydrogen phosphate, trisodium phosphate, etc., or a mixture of two or more thereof.
[0039] In the present application, the addition of auxiliary film-forming agents to the fluorine-containing treatment liquid can affect and control the reaction conditions in the process of chemical conversion film formation, such as pH value, temperature, etc.; by adjusting these reaction conditions, specific chemical reactions can be promoted or inhibited, thereby affecting the structure and performance of the chemical conversion film. The auxiliary film-forming agent can improve the performance of the chemical conversion film, such as improving corrosion resistance, adhesion, hardness, etc., and can react chemically or physically with the base metal to form a film layer that is tightly bonded to the base, thereby improving the overall performance of the film layer. Moreover, the type and amount of the auxiliary film-forming agent can affect the thickness and morphology of the chemical conversion film. In the present application, fluoride is used as an auxiliary film-forming agent. The amount of fluoride has a significant effect on the performance of the chemical conversion film. Since fluoride is corrosive, it can promote the uniform and fine distribution of cathode points during the film formation process, increase the density and flatness of the film; therefore, an appropriate amount of fluoride can accelerate the dissolution of the oxide film on the surface of the magnesium alloy, so that the magnesium alloy base is quickly exposed, which is conducive to the formation of a more uniform and dense chemical conversion film. However, excessive fluoride will corrode the magnesium alloy matrix, further damaging the performance and film quality of the magnesium alloy. Therefore, in the embodiments of the present application, the amount of the fluoride auxiliary film-forming agent is 1-2 g / L; in other embodiments, the amount of the fluoride auxiliary film-forming agent is 1.2-1.5 g / L. Specifically, in the embodiments of the application, the auxiliary film-forming agent is selected from but not limited to one or a mixture of two or more of fluoroboric acid, ammonium fluoride, sodium fluorosilicate, etc.
[0040] Adding a film-forming promoter to the fluorine-containing treatment liquid can effectively reduce the surface tension of the polymer compound, making it easier to form a uniform and dense film, which helps to improve the appearance and performance of the coating; the film-forming promoter can form a uniform, dense, protective film-like substance, thereby blocking the contact between the metal surface and the external environment, reducing or preventing the corrosion of the metal material. In addition, it can also change the ion concentration in the treatment liquid to make the metal surface present a more stable chemical state and improve its corrosion resistance. In the embodiment of the present application, the film-forming promoter is selected as a manganese salt. The manganese salt film-forming promoter can significantly increase the film-forming speed of the chemical conversion film, so that a layer of chemical conversion film can be formed on the surface of the magnesium alloy in a short time, which can not only improve production efficiency, but also ensure the quality and performance of the film layer. The manganese salt film-forming promoter can also improve the structure of the chemical conversion film, making it more uniform and dense, which helps to improve the corrosion resistance, wear resistance and adhesion of the film layer, thereby enhancing the protection ability of the magnesium alloy. The manganese ions in the manganese salt film-forming promoter can react with the oxides on the surface of the magnesium alloy to form stable compounds, which helps to improve the hardness and corrosion resistance of the film layer; at the same time, the manganese ions can also work together with film-forming agents such as phosphates to further improve the performance of the film layer. Of course, the amount of manganese salt film-forming promoter will affect the performance and organizational structure of the chemical conversion film. The effect of the amount of manganese salt on the chemical conversion film is mainly manifested in: manganese salt can promote the uniformity and density of the film layer, thereby enhancing the barrier properties of the film layer, preventing the corrosive medium from corroding the base metal, and can promote the formation of hard manganese compounds in the film layer, thereby improving the hardness and wear resistance of the film layer, and can also promote the bonding force between the film layer and the base metal, and improve the adhesion of the film layer; however, excessive manganese salt may not only cause the film layer to be too thick, with defects or cracks inside, but may also cause other impurities or by-products to appear in the film layer, affecting the performance of the film layer. Therefore, in the embodiments of the present application, the dosage of the manganese salt is 10 g / L-30 g / L, preferably, in some embodiments, the dosage of the manganese salt is 12 g / L-15 g / L, or 20 g / L-25 g / L. The manganese salt film-forming promoter can be selected from, but not limited to, one or a mixture of two or more of manganese oxalate, manganese chloride, and disodium manganese ethylenediaminetetraacetate.
[0041] In the embodiments of the present application, in order to obtain a chemical conversion film with suitable roughness, it is necessary to adjust the mass ratio of the film former, the auxiliary film former, and the film-forming promoter in the fluorine-containing treatment liquid. Specifically, the mass ratio of the film former, the auxiliary film former, and the film-forming promoter is (5-30):1:(5-15). Preferably, in some embodiments, the mass ratio is (10-15):1:(8-12). In the embodiments of the present application, regulating the pH value of the fluorine-containing treatment liquid can control the reaction rate, and the speed of the reaction has a significant effect on the surface structure of the film layer. In the present application, in order to obtain a film layer with a reasonable roughness, the pH value of the fluorine-containing treatment liquid described in some embodiments is 2.9-3.1.
[0042] As a further preferred solution, the porosity of the porous layer in the embodiment of the present application is 35%-55%. In this solution, the porous layer mainly provides in-situ growth points for the covering layer.
[0043] As a further preferred solution, the porosity of the covering layer described in the embodiment of the present application is less than 1%, the thickness of the dense layer is 5-10μm, and the covering layer mainly contains elements such as Mn, P, and F. The covering layer can effectively block the penetration of corrosive media (such as water, oxygen, ions, etc.) in the external environment, thereby protecting the magnesium alloy substrate from corrosion. Lower porosity usually means that the film layer is denser and can provide better protection performance. Appropriate thickness can also ensure good bonding between the film layer and the substrate, avoiding problems such as peeling or cracking during use.
[0044] The embodiment of the present application also provides a method for preparing a chemical conversion film that improves the bonding strength of the paint film on the surface of the magnesium alloy. Through treatments such as degreasing, activation, and immersion in a treatment liquid, a rough structure is formed on the surface of the magnesium alloy, making it present a "cauliflower flake-like" structure at the microscopic level, and avoiding the appearance of floating dust and the like on the surface of the conversion film.
[0045] The preparation method described in the embodiment of the present application comprises the following steps:
[0046] Degreasing treatment: Use alkaline solution to degreasing the surface of magnesium alloy substrate to remove oil stains and impurities on the surface; the alkaline solution can undergo saponification reaction or emulsification with the oil stains, thereby removing the oil stains from the substrate surface.
[0047] Surface activation: Use acid to activate the surface of the magnesium alloy substrate after degreasing to remove oxides and impurities on the surface;
[0048] Film-forming reaction: the magnesium alloy substrate after surface activation is immersed in a fluorine-containing treatment solution, the immersion temperature is controlled to be 50-70° C., and the immersion time is 10-20 minutes to form a chemical conversion film on the surface of the magnesium alloy.
[0049] In the degreasing process, the temperature of the alkali solution, the treatment time and the concentration of the alkali solution have an important influence on the degreasing effect and subsequent processes. The effect of the alkali solution temperature on the degreasing effect is manifested as follows: a higher temperature can accelerate the chemical reaction between the alkali solution and the oil stains and improve the degreasing efficiency, but too high a temperature may cause the alkali solution to cause excessive corrosion to the magnesium alloy matrix and damage the surface of the matrix. At a lower temperature, the reaction rate of the alkali solution and the oil stains is slower, which may lead to incomplete degreasing. Therefore, it is necessary to select a suitable treatment temperature to ensure that the oil can be removed efficiently without damaging the matrix. In the embodiment of the present application, the temperature of the alkali solution is 55-70°C. The preferred degreasing temperature is 60-65°C. The effect of the degreasing treatment time on the degreasing effect is manifested as follows: too short a time may cause the oil stains to not be completely removed, affecting the subsequent process, and too long a time may cause the alkali solution to cause excessive corrosion to the matrix, while increasing production costs. Therefore, in order to ensure the degreasing effect while reducing production costs, the degreasing time is 3-5min. The concentration of the alkali solution determines its chemical reaction speed with the oil stain and the oil removal effect; when the concentration is too high, the reaction speed is too fast, which may cause excessive corrosion of the substrate surface. Excessive alkali solution concentration may also pollute the environment and increase the difficulty and cost of wastewater treatment; when the concentration is too low, it may not be possible to completely remove the oil stain. The alkali solution used in the embodiment of the present application includes sodium hydroxide and a surfactant, wherein the mass ratio of sodium hydroxide to the surfactant is (2-6): 1; the dosage of the two is 10-20g / L and 3-5g / L, respectively. The surfactant is one or a mixture of two or more of hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, and fatty alcohol polyoxyethylene ether.
[0050] Surface activation can remove oxides and impurities on the surface of the magnesium alloy substrate after degreasing treatment, making the substrate surface more active, which is conducive to the reaction between the chemical substances in the subsequent treatment liquid and the substrate. As a further preferred scheme, in the surface activation treatment described in the embodiment of the present application, the magnesium alloy substrate is washed with acid solution at room temperature for 10-15s, and then washed with clean water after being taken out; the acid solution used includes organic acid and surfactant, and the amount of the organic acid and surfactant is 10-30g / L and 0.1-1g / L respectively. As a further preferred scheme, the organic acid is a mixture of one or more of formic acid, acetic acid, and lactic acid; the surfactant is a mixture of one or more of hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, and 2-ethylhexyl sodium sulfate.
[0051] Example 1
[0052] This embodiment provides a chemical conversion film that improves the adhesion of the paint film on the surface of the magnesium alloy, which is prepared by the following method:
[0053] Degreasing treatment: The magnesium alloy workpiece is degreased at 60°C for 3 minutes;
[0054] Surface activation: After degreasing, the magnesium alloy workpiece is pickled at room temperature for 15 seconds, and then taken out for water washing;
[0055] Film-forming reaction: After surface activation, the magnesium alloy workpiece is immersed in a fluorine-containing treatment solution for 15 minutes. The pH of the treatment solution is 3.0 and the immersion temperature is 60°C. After being taken out and washed and dried, a "cauliflower flake" structure can be formed on the surface. For the surface structure of the chemical conversion film, see Figure 1 .
[0056] The composition of the fluorine-containing treatment liquid used in this embodiment is as follows: sodium dihydrogen phosphate: 30 g / L, manganese oxalate: 30 g / L, ammonium fluoride: 1 g / L.
[0057] Example 2
[0058] This embodiment provides a chemical conversion film that improves the adhesion of the paint film on the surface of the magnesium alloy, which is prepared by the following method:
[0059] Degreasing treatment: The magnesium alloy workpiece is degreased at 60°C for 3 minutes;
[0060] Surface activation: After degreasing, the magnesium alloy workpiece is pickled at room temperature for 12 seconds, and then taken out for water washing;
[0061] Film formation reaction: After surface activation, the magnesium alloy workpiece is immersed in a fluorine-containing treatment solution for 10 minutes. The pH of the treatment solution is 2.9 and the immersion temperature is 70°C. After being taken out and washed and dried, a "cauliflower flake" structure can be formed on the surface. The surface structure of the chemical conversion film can be found in Figure 2 .
[0062] The composition of the fluorine-containing treatment liquid used in this embodiment is as follows: sodium dihydrogen phosphate: 30 g / L, manganese oxalate: 30 g / L, ammonium fluoride: 1.5 g / L.
[0063] Example 3
[0064] This embodiment provides a chemical conversion film that improves the adhesion of the paint film on the surface of the magnesium alloy, which is prepared by the following method:
[0065] Degreasing treatment: The magnesium alloy workpiece is degreased at 60°C for 5 minutes;
[0066] Surface activation: After degreasing, the magnesium alloy workpiece is pickled at room temperature for 10 seconds, then taken out and washed with water;
[0067] Film-forming reaction: After surface activation, the magnesium alloy workpiece is immersed in a fluorine-containing treatment solution for 20 minutes. The pH of the treatment solution is 3.1 and the immersion temperature is 50°C. After being taken out and washed and dried, a "cauliflower flake" structure can be formed on the surface. The surface structure of the chemical conversion film can be found in Figure 3 .
[0068] The composition of the fluorine-containing treatment liquid used in this embodiment is as follows: sodium dihydrogen phosphate: 25 g / L, manganese oxalate: 25 g / L, ammonium fluoride: 2 g / L.
[0069] Comparative Example 1
[0070] Provided is a chemical conversion film, which is prepared by the following method: a magnesium alloy workpiece is degreased at 60°C for 3-5 minutes, pickled at room temperature for 10-15 seconds, taken out and washed with water, and then immersed in a treatment solution for 15 minutes (the treatment solution does not contain an auxiliary film-forming agent, and other components and amounts are the same as those in Example 1), the pH of the treatment solution is 2.6, the immersion temperature is 60°C, and the workpiece is taken out and washed with water and dried; the surface structure of the chemical conversion film is shown in Figure 4 .
[0071] Comparative Example 2
[0072] Provided is a chemical conversion film, which is prepared by the following method: the magnesium alloy workpiece is degreased at 60°C for 3-5 minutes, pickled at room temperature for 10-15 seconds, taken out and washed with water, and then immersed in a treatment liquid for 15 minutes (the auxiliary film-forming agent in the treatment liquid is fluoroboric acid, and the other components and amounts are the same as those in Example 2), the pH of the treatment liquid is 2.9, the immersion time is 60°C, and the workpiece is taken out and washed with water and dried. The surface structure of the chemical conversion film can be found in Figure 5 .
[0073] Comparative Example 3
[0074] Provided is a chemical conversion film, which is prepared by the following method: the magnesium alloy workpiece is degreased at 60°C for 3-5 minutes, pickled at room temperature for 10-15 seconds, taken out and washed with water, and then immersed in a treatment solution for 15 minutes (the auxiliary film-forming agent content is 2g / L, and the other components and amounts are the same as those in Example 1), the pH of the treatment solution is 2.9, the temperature is 60°C, and the workpiece is taken out and washed with water and dried. The surface structure of the chemical conversion film can be found in Figure 6 .
[0075] Performance Testing
[0076] 1. Surface morphology test
[0077] Scanning electron microscopy (SEM) was used to test the microstructure of the chemical conversion film.
[0078] 2. The roughness test is carried out by a roughness tester. Place the roughness tester on the surface of the sample and press the start button to perform the surface roughness test.
[0079] 3. To test the adhesion of the coating by the pull-out method, you need to clean the bottom of the spindle first, mix the required two-component glue in a 1:1 ratio, and apply it to the test point. Press the spindle hard on the prepared test surface, apply pressure to squeeze out the excess glue, then wipe off the overflowed glue, and wait for the glue to fully cure for about 24 hours. Align the pull-out tester with the spindle and fully embed it and fix it. Turn on the pull-out tester and perform a pull-out test on the adhesion of the coating. The test conditions are 10mm spindle and pull 1MPa / S.
[0080] 4. The salt spray test is carried out according to the neutral salt spray test described in GB / T 10125-2021. Prepare 50g / L sodium chloride solution with deionized water, adjust the pH of the solution to the specified value, and add the sodium chloride solution into the salt spray test chamber. The chamber temperature is set to 35°C and the spray pressure is set to 1kg / cm 2 The sample was placed at a certain angle for the experiment.
[0081] The bonding strength of the surface paint films obtained by the same process on the surfaces of the examples and comparative examples is shown in Table 1. Figure 7 shown.
[0082] Table 1: Performance test results of embodiments and comparative examples
[0083]
[0084] The results in Table 1 show that the roughness of the chemical conversion films obtained in Examples 1-3 is relatively appropriate, and in combination with the organizational structure, it presents a clear cauliflower shape. The pull-out bonding test results of Example 1 and Example 2 are both greater than 28 MPa, which is greatly improved compared to the comparative example, which is attributed to the "cauliflower-like" rough surface generated in situ on the surface of Examples 1 and 2. The improvement of Example 3 is smaller, which is because only a part of the surface of the sample in Example 3 forms a "cauliflower-like" structure.
[0085] See also Figure 7 The results of the salt spray test show that: a large number of corrosion spots appear on the surface of the sample prepared without auxiliary film-forming agent in the 72h neutral salt spray test, and the corrosion resistance level only reaches level 6; while for the sample prepared with auxiliary film-forming agent, only one tiny corrosion spot appears on the surface after the 72h neutral salt spray test, and the corrosion resistance level reaches level 9. This shows that the invention itself has good corrosion resistance.
[0086] The components listed in the present invention, as well as the upper and lower limits and interval values of the components of the present invention can realize the present invention, and the embodiments are not listed one by one here. Some specific embodiments are listed above to illustrate the present invention. It is necessary to point out here that the above and below specific embodiments are only used to further illustrate the present invention and do not represent a limitation on the protection scope of the present invention.
Claims
1. A chemical conversion film for improving the bonding strength of paint film on the surface of magnesium alloy, characterized in that: A roughened film structure is formed on the surface of the magnesium alloy metal by introducing a fluorine-containing treatment liquid that can directly react with the magnesium alloy matrix, wherein the film structure comprises a porous layer located on the surface of the magnesium alloy matrix and a covering layer located on the surface of the porous layer, wherein the porosity of the porous layer is 35%-55%, the covering layer comprises Mn, P, and F elements, the porosity of the covering layer is less than 1%, and the thickness of the covering layer is 5-10 μm; the roughness of the film structure is 2.0-4.0 μm, and the bonding strength between the film and the paint film after the paint film is sprayed on the surface of the film structure is 20-30 MPa a; the fluorine-containing treatment liquid is composed of a film-forming agent, an auxiliary film-forming agent and a film-forming accelerator; the film-forming agent is one or a mixture of two or more of disodium hydrogen phosphate, sodium dihydrogen phosphate and trisodium phosphate, and the amount of the film-forming agent is 25g / L-30g / L; the auxiliary film-forming agent is ammonium fluoride, and the amount of ammonium fluoride is 1-1.5g / L; the film-forming accelerator is one or a mixture of two or more of manganese oxalate, manganese chloride and disodium manganese ethylenediaminetetraacetate, and the amount of the film-forming accelerator is 25g / L-30g / L; the pH value of the fluorine-containing treatment liquid is 2.9-3.
1.
2. A method for preparing a chemical conversion film for improving the bonding strength of a paint film on a magnesium alloy surface as claimed in claim 1, characterized in that: The following steps are included: Degreasing treatment: Use alkaline solution to degreasing the surface of magnesium alloy substrate to remove oil stains and impurities on the surface; Surface activation: Use acid to activate the surface of the magnesium alloy substrate after degreasing to remove oxides and impurities on the surface; Film-forming reaction: the magnesium alloy substrate after surface activation is immersed in a fluorine-containing treatment liquid, the immersion temperature is controlled to be 50-70°C, the immersion time is 10-20min, and a chemical conversion film is formed on the surface of the magnesium alloy; the fluorine-containing treatment liquid is composed of a film-forming agent, an auxiliary film-forming agent and a film-forming promoter; the film-forming agent is a mixture of one or more of disodium hydrogen phosphate, sodium dihydrogen phosphate and trisodium phosphate, and the amount of the film-forming agent is 25g / L-30g / L; the auxiliary film-forming agent is ammonium fluoride, and the amount of ammonium fluoride is 1-1.5g / L; the film-forming promoter is a mixture of one or more of manganese oxalate, manganese chloride and disodium manganese ethylenediaminetetraacetate, and the amount of the film-forming promoter is 25g / L-30g / L; the pH value of the fluorine-containing treatment liquid is 2.9-3.
1.
3. The preparation method according to claim 2, characterized in that: The degreasing step is to use alkaline solution to remove oil at 55-70°C for 3-5 minutes; the alkaline solution includes sodium hydroxide and a surfactant, wherein the dosage of sodium hydroxide and the surfactant is 10-20g / L and 3-5g / L respectively.
4. The preparation method according to claim 2, characterized in that: In the surface activation treatment, the magnesium alloy substrate is washed with acid solution at room temperature for 10-15s, and then washed with clean water; the acid solution used includes organic acid and surfactant, and the dosage of the organic acid and surfactant is 10-30g / L and 0.1-1g / L respectively.
5. The preparation method according to claim 3, characterized in that: The surfactant is one or a mixture of two or more of hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, sodium 2-ethylhexyl sulfate and fatty alcohol polyoxyethylene ether.
Citation Information
Patent Citations
Surface treating method for magnesium alloy
CN101130864A
Film-forming solution for chromium-free conversion film of magnesium alloy and method for preparing conversion film by using film-forming solution
CN102191493A