Secondary batteries and electrical devices
By designing multi-layered lithium-containing transition metal oxide particles in the positive electrode active material of secondary batteries, using the layered phase and spinel phase structure to reduce side reactions and improve lithium ion transmission, the existing secondary battery cycle is solved. The problem of reduced capacity extends battery life and improves cycling performance.
Patent Information
- Application Number
- CN202410767576.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-06-14
AI Technical Summary
The existing secondary batteries are prone to side reactions with the electrolyte during the circulation process, resulting in a decrease in circulation capacity, and the resistance to lithium ions breaking out and embedding from the surface of the material is large, affecting the energy density and electrochemical properties of the material.
The positive electrode active material containing lithium transition metal oxide is adopted, and the particles include an internal area and a surface area. The surface area is divided into a first surface area and a second surface area. The first surface area and the second surface area both contain a layered phase structure. and spinel phase or lithosaline phase structure, optimize the structural stability of the material and lithium ion transmission path.
It improves the structural stability of the positive electrode active material and the migration speed of lithium ion, reduces the possibility of side reactions, extends the service life of the battery and improves the circulation performance.
Smart Images

Figure CN118335963B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a secondary battery and an electric device. Background Art
[0002] Secondary batteries have the advantages of high energy density, high operating voltage, low self-discharge rate, small size and light weight, and are widely used in the field of consumer electronics.
[0003] With the rapid development of electric vehicles and mobile electronic devices, people have higher and higher requirements for the cycle performance of secondary batteries. How to improve the cycle performance of batteries is a scientific and technological problem that needs to be solved urgently in the current application field of secondary batteries. Summary of the invention
[0004] The present application is made in view of the above-mentioned problems, and its purpose is to provide a secondary battery and an electric device, wherein the secondary battery has excellent cycle performance and a long service life.
[0005] A first aspect of the present application provides a secondary battery, comprising:
[0006] A positive electrode plate, a negative electrode plate and an electrolyte, the positive electrode plate comprising a positive electrode current collector and a positive electrode active material layer arranged on at least one side of the positive electrode current collector, the positive electrode active material layer comprising a positive electrode active material, the positive electrode active material comprising a lithium-containing transition metal oxide, wherein the particles of the lithium-containing transition metal oxide comprise an internal region and a surface region at least partially surrounding the internal region, the surface region comprises a first surface region and a second surface region, the second surface region is located between the first surface region and the internal region, the first surface region and the second surface region both comprise a first phase structure and a second phase structure, the first phase structure comprises a layered phase structure, the second phase structure comprises at least one of a spinel phase structure and a rock salt phase structure, wherein the first surface region comprises a rock salt phase structure and a layered phase structure, and the second surface region comprises a spinel phase structure and a layered phase structure.
[0007] The surface area includes both a first phase structure including a layered phase structure and a second phase structure including a spinel phase structure or a rock salt phase structure. On the one hand, the second phase structure of the non-electrochemically active spinel phase structure or the rock salt phase structure is utilized to reduce the possibility of side reactions between the positive electrode active material and the electrolyte, thereby improving the structural stability of the positive electrode active material and enhancing the cycle performance of the battery. On the other hand, the layered phase structure in the first phase structure can provide a channel for the deintercalation of lithium ions on the surface of the material, so that the positive electrode active material has a high lithium ion migration rate, which is beneficial to the utilization of the gram capacity of the positive electrode active material, reduces the loss of active lithium during the cycle, improves the cycle performance of the battery, and extends the service life of the battery. In addition, the first surface region close to the particle surface includes a rock salt phase structure and a layered phase structure. The rock salt phase structure has relatively better stability, and the effect of improving structural stability and thermal stability is more obvious. At the same time, the layered phase structure in the first surface region can provide a path for lithium ion deintercalation, accelerate lithium ion diffusion, and improve the cycle performance and kinetic performance of the battery; the second surface region close to the inner region includes a spinel phase structure and a layered phase structure. The spinel phase structure takes into account good structural stability and high lithium ion transmission speed. While improving the structural stability of the material, it also makes the material have excellent lithium ion transmission performance, taking into account the cycle stability and rate performance of the battery. At the same time, the second surface region includes a layered phase structure, which is beneficial to provide more lithium ion transmission channels and storage sites, and improves the kinetic performance and cycle performance of the battery. In addition, a second surface region is set between the inner region and the first surface region, and the spinel phase structure included therein can be used as a transition phase between the rock salt phase in the first surface region and the layered phase structure in the inner region, thereby improving the lattice adaptation of the material, which is beneficial to improving the structural stability of the material, and is beneficial to improving the cycle performance of the battery.
[0008] In any embodiment, the first surface region refers to a region extending from the surface of the lithium-containing transition metal oxide particle to the inside of the particle by a distance of 10 nm.
[0009] The area of the first surface region is controlled within a suitable range so that the rock salt phase in the first surface region can achieve the purpose of improving structural stability and thermal stability, while also making the material have good lithium ion transmission performance, thereby improving the cycle performance of the battery.
[0010] In any embodiment, the second surface region refers to a region extending from 10 nm to 60 nm from the surface of the lithium-containing transition metal oxide particle to the interior of the particle.
[0011] By controlling the area of the second surface region within an appropriate range, the spinel phase structure in the second surface region can achieve a smooth transition from the first surface region to the internal region, thereby improving the overall lattice adaptability of the material and the structural stability of the material. This is also beneficial to comprehensively improve the structural stability of the material and the transmission speed of lithium ions, thereby improving the cycle performance of the battery.
[0012] In any embodiment, the interior region comprises a lamellar phase structure.
[0013] The internal area includes a layered phase structure. The material has multiple lithium ion insertion and extraction pathways. The material has an excellent lithium ion diffusion rate, which is beneficial to the material's specific capacity and improves the battery's cycle capacity retention rate and energy density.
[0014] In any embodiment, based on the total area of the rock salt phase structure and the layered phase structure in the first surface region, the area of the rock salt phase structure accounts for 60%-80%, and / or the area of the layered phase structure in the first surface region accounts for 20%-40%.
[0015] In any embodiment, based on the total area of the rock salt phase structure and the layered phase structure in the first surface region, the area of the rock salt phase structure accounts for 65%-75%, and / or the area of the layered phase structure in the first surface region accounts for 25%-35%.
[0016] By controlling the area ratio of the rock salt phase structure and the layered phase structure in the first surface region within an appropriate range, the structural stability and thermal stability of the material are improved while also enabling the material to have good lithium ion transmission properties, thereby comprehensively improving the cycle performance of the battery.
[0017] In any embodiment, based on the total moles of metal elements other than Li in the first surface layer region, the mass content of nickel element is 50%-80%.
[0018] In any embodiment, based on the total area of the spinel phase structure and the layered phase structure in the second surface region, the area of the spinel phase structure accounts for 50%-90%, and / or, the layered phase structure in the second surface region accounts for 10%-50%.
[0019] In any embodiment, based on the total area of the spinel phase structure and the layered phase structure in the second surface region, the area of the spinel phase structure accounts for 60%-80%, and / or, the layered phase structure in the second surface region accounts for 20%-40%.
[0020] By controlling the area ratio of the spinel phase structure and the layered phase structure in the second surface region within an appropriate range, the structural stability and lattice adaptability of the material are improved, while also enabling the material to have excellent lithium ion performance and lithium ion storage sites, thereby comprehensively improving the cycle performance of the battery.
[0021] In any embodiment, the molar content of the cobalt element is 60%-90% based on the total moles of the metal elements other than Li in the second surface layer region.
[0022] In any embodiment, based on the molar amount of the metal elements other than Li in the lithium-containing transition metal oxide, the molar content of the nickel element in the lithium-containing transition metal oxide is greater than or equal to 60%.
[0023] In any embodiment, based on the molar amount of metal elements other than Li in the lithium-containing transition metal oxide, the molar content of nickel in the lithium-containing transition metal oxide is greater than or equal to 80%.
[0024] In any embodiment, based on the molar amount of metal elements other than Li in the lithium-containing transition metal oxide, the molar content of nickel in the lithium-containing transition metal oxide is greater than or equal to 90%.
[0025] In any embodiment, the lithium-containing transition metal oxide further includes a modifying element, and the modifying element includes one or more of Zr, Al, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K.
[0026] Lithium-containing transition metal oxides include modifying elements such as Zr, Al, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb or K, which can further improve the cycle stability of the material and improve the cycle stability of the battery.
[0027] In any embodiment, based on the mass of the lithium-containing transition metal oxide, the mass content of the modifying element is less than or equal to 3000 ppm.
[0028] When the mass content of the modifying elements is within an appropriate range, it can improve the cycle stability of the material while increasing the discharge capacity of the material, thereby comprehensively improving the cycle performance and energy density of the battery.
[0029] In any embodiment, the lithium-containing transition metal oxide comprises Li a1 Ni x1 Co y1 Mn 1-x1-y1 M1 w1 O 2-b1 , Li a2 Ni x2 Co y2Al 1-x2-y2 M2 w2 O 2-b2 Any of the following:
[0030] Among them, 0.8≤a1≤1.2, 0.6≤x1≤1, 0≤y1≤0.4, -0.1≤b1≤0.1, 0≤w1≤0.1;
[0031] 0.8≤a2≤1.2, 0.6≤x2≤1, 0≤y2≤0.4, -0.1≤b2≤0.1, 0≤w2≤0.1, M1 includes at least one element among Zr, Al, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K, and M2 includes at least one element among Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K.
[0032] In any embodiment, the lithium-containing transition metal oxide comprises Li a1 Ni x1 Co y1 Mn 1-x1-y1 M1 w1 O 2-b1 , Li a2 Ni x2 Co y2 Al 1-x2-y2 M2 w2 O 2-b2 Any of the following:
[0033] Among them, 0.8≤a1≤1.2, 0.8≤x1≤1, 0≤y1≤0.2, -0.1≤b1≤0.1, 0≤w1≤0.1;
[0034] 0.8≤a2≤1.2, 0.8≤x2≤1, 0≤y2≤0.2, -0.1≤b2≤0.1, 0≤w2≤0.1, M1 includes at least one element among Zr, Al, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K, and M2 includes at least one element among Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K.
[0035] A second aspect of the present application provides an electrical device, comprising the secondary battery described in the first aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 is a schematic diagram of a cross-sectional image of a particle containing a lithium transition metal oxide of the present application;
[0037] Figure 2 is a schematic diagram of an embodiment of a secondary battery of the present application;
[0038] Figure 3 is an exploded schematic diagram of an embodiment of a secondary battery of the present application;
[0039] Figure 4 is a schematic diagram of an embodiment of a battery module of the present application;
[0040] Figure 5 is a schematic diagram of an embodiment of a battery pack of the present application;
[0041] Figure 6 yes Figure 5 An exploded schematic diagram of an embodiment of a battery pack is shown;
[0042] Figure 7 It is a schematic diagram of one embodiment of an electric device including the secondary battery of the present application as a power source.
[0043] In the accompanying drawings, the drawings are not necessarily drawn according to the actual scale. The description of the accompanying drawings is as follows:
[0044] 1 battery pack, 2 upper box, 3 lower box, 4 battery module, 5 secondary battery, 51 shell, 52 electrode assembly, 53 cover plate, 100 particles containing lithium transition metal oxide, 101 internal area, 102 surface area, 1021 second surface area, 1022 first surface area. DETAILED DESCRIPTION
[0045] Below, the embodiments of the secondary battery and the electrical device of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0046] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0047] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0048] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0049] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0050] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0051] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0052] High-capacity, low-cost lithium-containing transition metal oxides are likely to be widely used as positive electrode active materials for high-energy lithium-ion batteries. However, this series of materials are prone to side reactions with the electrolyte during the cycle, resulting in a decrease in the cycle capacity, which is not conducive to its large-scale practical application. Since the area where the material reacts with the electrolyte is concentrated in the surface structure of the material, a large amount of research work has focused on improving the unstable surface structure of lithium-containing transition metal oxides. In the prior art, the structural stability of the material is improved by setting a rock salt phase or a spinel phase in the surface structure of the lithium-containing transition metal oxide, thereby improving the cycle performance of the battery. However, the rock salt phase or the spinel phase itself has poor electrochemical activity, and the surface structure is a rock salt phase or a spinel phase structure, resulting in a large resistance to the release and embedding of lithium ions from the surface of the material, which will affect the energy density and electrochemical performance of the material, resulting in the loss of active lithium, but failing to achieve the purpose of improving the cycle performance of the battery.
[0053] [Secondary battery]
[0054] Based on this, the present application provides a secondary battery, comprising:
[0055] A positive electrode plate, a negative electrode plate and an electrolyte, the positive electrode plate comprising a positive electrode current collector and a positive electrode active material layer arranged on at least one side of the positive electrode current collector, the positive electrode active material layer comprising a positive electrode active material, the positive electrode active material comprising a lithium-containing transition metal oxide, wherein the particles of the lithium-containing transition metal oxide comprise an internal region and a surface region at least partially surrounding the internal region, the surface region comprises a first surface region and a second surface region, the second surface region is located between the first surface region and the internal region, the first surface region and the second surface region both comprise a first phase structure and a second phase structure, the first phase structure comprises a layered phase structure, the second phase structure comprises at least one of a spinel phase structure and a rock salt phase structure, wherein the first surface region comprises a rock salt phase structure and a layered phase structure, and the second surface region comprises a spinel phase structure and a layered phase structure.
[0056] Figure 1 is a schematic diagram of a cross-sectional image of a particle 100 containing a lithium transition metal oxide of the present application. Figure 1As shown, the particles of the lithium-containing transition metal oxide 100 include an internal region 101 and a surface region 102 at least partially surrounding the internal region 101 , wherein the surface region 102 includes a first surface region 1022 and a second surface region 1021 , and the second surface region 1021 is located between the first surface region 1022 and the internal region 101 .
[0057] As used herein, the term "spinel phase structure" refers to a crystal structure in which oxygen ions are closely packed in a cubic pattern, cations fill one eighth of tetrahedral voids, and cations fill one half of octahedral voids, with the space group being Fd-3m.
[0058] In this article, the term "rock salt phase structure" refers to the sodium chloride type structure, which is the crystal structure of a class of AB type ionic compounds represented by sodium chloride, belonging to the cubic crystal system, face-centered cubic lattice, and space group Fm-3m.
[0059] In this context, the term “lamellar phase structure” means that in its crystal structure, oxygen ions (O 2- ) are closely packed in cubic form to form a space skeleton, lithium ions (Li + ) and cobalt ions (Co 3+ ) are located in alternating octahedral positions in the cubic close-packed framework of oxygen ions, with a layered structure of α-sodium ferrite type. The crystal structure formed by this has a space group of R-3m.
[0060] The phase structure in the first surface area and the second surface area can be tested by methods and equipment known in the art. An example is as follows: disassemble the battery to obtain the positive electrode sheet, peel the positive electrode film layer from the current collector, and then dissolve it in N-methylpyrrolidone solvent. After the binder, dispersant, etc. in the positive electrode film layer are dissolved in the solvent, filter and dry to obtain a sample powder. The sample powder is sectioned by a focused ion beam (FIB), and then a layer of sample slice with a thickness of 20nm is cut from the section. Then, the surface of the sample slice is subjected to HR-TEM test to obtain an HR-TEM original image, and the phase structure of the particles in the original image is calibrated by Fourier transform (FFT). Specifically, a particle is randomly selected from the original image, and FFT is used to obtain a diffraction pattern of the area extending 100nm from the surface of the particle to the inside of the particle. The distance from the diffraction spot to the center of the diffraction pattern is measured, and the reciprocal is calculated, which is the interplanar spacing of the corresponding crystal plane. According to the difference in interplanar spacing of the three phase structures, the interplanar spacing The (003) crystal plane spacing of 4.75Å~4.8Å (angstroms) is the layered phase structure, the (220) crystal plane spacing of 2.7Å~3.0Å (angstroms) is the spinel phase structure, and the (002) crystal plane spacing of 2.0Å~2.2Å (angstroms) is the rock salt phase. The three phase structures can be determined, and then the phase distribution structure diagram of the area extending 100nm from the surface of the particle to the interior of the particle is obtained. According to the distribution differences of the three phase structures, the dividing lines between the first surface area, the second surface area, and the internal area can be distinguished, and then the phase structures in the first surface area and the second surface area can be determined.
[0061] The first surface region and the second surface region simultaneously include a first phase structure including a layered phase structure and a second phase structure including a spinel phase structure or a rock salt phase structure. On the one hand, the second phase structure of the non-electrochemically active spinel phase structure or the rock salt phase structure is utilized to reduce the possibility of side reactions between the positive electrode active material and the electrolyte, thereby improving the structural stability of the positive electrode active material and enhancing the cycle performance of the battery. On the other hand, the layered phase structure in the first phase structure can provide a channel for the deintercalation of lithium ions on the surface of the material, so that the positive electrode active material has a high lithium ion migration speed and can also provide a sufficient number of lithium ion storage sites, which is beneficial to the utilization of the gram capacity of the positive electrode active material, reduces the loss of active lithium during the cycle, improves the cycle performance of the battery, and extends the service life of the battery. In addition, the first surface area close to the particle surface includes a rock salt phase structure and a layered phase structure. The rock salt phase structure has relatively better stability, and the effect of improving structural stability and thermal stability can be more obvious. At the same time, the layered phase structure in the first surface area can provide a path for lithium ion deintercalation, accelerate lithium ion diffusion, provide a certain amount of lithium ion storage sites, increase the material's gram capacity and kinetic properties, and comprehensively improve the battery's cycle performance. The second surface area close to the inner area includes a spinel phase structure and a layered phase structure. The spinel phase structure has both good structural stability and high lithium ion transmission speed, which can improve the material's structure. While improving the stability, the material also has excellent lithium ion transmission performance. The battery has both cycle stability and rate performance. At the same time, the second surface area including the layered phase structure is also beneficial to accelerate the diffusion of lithium ions, providing certain lithium ion storage sites, which is beneficial to the material's specific capacity. In addition, a second surface area including a spinel phase structure and a layered phase structure is arranged between the internal area and the first surface area. The spinel phase structure included in the second surface area can serve as a transition phase between the rock salt phase in the first surface area and the layered phase structure in the internal area, thereby improving the lattice adaptation of the material, which is beneficial to improving the structural stability of the material and the cycle performance of the battery.
[0062] Compared with the first surface region and the second surface region containing a single first phase structure or a second phase structure, the first surface region and the second surface region of the present application both contain a mixed phase structure, which can improve the cycle stability of the material while taking into account the lithium ion transmission path and storage site of the material, thereby comprehensively improving the cycle performance of the battery.
[0063] Compared with the first surface region containing a layered phase structure and a rock salt phase structure, the second surface region contains a layered phase structure and a rock salt phase structure, that is, the second phase structure in the second surface region close to the inner region is a rock salt phase structure. The present application arranges a spinel phase structure with good structural stability and excellent lithium ion transmission performance in the second surface region close to the inner region, which can reduce the possibility of side reactions between the second surface region and the electrolyte, and can also increase the transmission speed of the active ions of the material, improve the rate performance of the material, and improve the cycle performance and rate performance of the material.
[0064] Compared with the first surface region containing layered phase structure and spinel phase structure, the second surface region contains layered phase structure and spinel phase structure, that is, the second phase structure in the first surface region close to the particle surface is the spinel phase structure. The present application arranges a rock salt phase structure with excellent structural stability and thermal stability in the first surface region close to the particle surface. The rock salt phase structure has a more significant effect on reducing the side reaction between the particle surface and the electrolyte, which is beneficial to achieving the purpose of improving the structural stability of the material and improving the cycle performance of the battery.
[0065] Compared with the first surface region containing layered phase structure and spinel phase structure, the second surface region contains layered phase structure and rock salt phase structure, that is, the second phase structure in the first surface region close to the particle surface is the spinel phase structure, and the second phase structure close to the internal region is the rock salt phase structure. The present application selects a rock salt phase structure with better structural stability in the first surface region close to the particle surface, and selects a spinel phase structure with certain structural stability and excellent lithium ion transmission performance in the internal region. This can reduce the possibility of side reactions between the material and the electrolyte, while improving the ion transmission performance of the material, improving the lattice adaptation of the material, and improving the cycle performance of the material.
[0066] In some embodiments, the first surface region refers to a region extending from the surface of the lithium-containing transition metal oxide particle to the interior of the particle by a distance of 10 nm.
[0067] By referring to the testing method for the phase structure in the first surface area and the second surface area described above, the boundary between the first surface area, the second surface area and the internal area can be distinguished, and the position area of the first surface area and the second surface area can be tested.
[0068] By controlling the area of the first surface region within a suitable range, the rock salt phase in the first surface region can achieve the purpose of improving structural stability and thermal stability, while also enabling the material to have good lithium ion transmission performance, thereby comprehensively improving the cycle performance of the battery.
[0069] In some embodiments, the second surface region refers to a region extending from 10 nm to 60 nm from the surface of the lithium-containing transition metal oxide particle to the interior of the particle.
[0070] By controlling the area of the second surface region within an appropriate range, the spinel phase structure in the second surface region can achieve a smooth transition from the first surface region to the internal region, thereby improving the overall lattice adaptability of the material and the structural stability of the material. This is also beneficial to comprehensively improve the structural stability of the material and the transmission speed of lithium ions, thereby improving the cycle performance of the battery.
[0071] In some embodiments, the interior region comprises a lamellar phase structure.
[0072] The phase structure of the inner region may be tested by referring to the aforementioned testing method for the phase structure in the first surface region and the second surface region.
[0073] The internal area includes a layered phase structure. The material has multiple lithium ion insertion and extraction pathways. The material has an excellent lithium ion diffusion rate, which is beneficial to the material's specific capacity and improves the battery's cycle capacity retention rate and energy density.
[0074] In some embodiments, based on the total area of the rock salt phase structure and the layered phase structure in the first surface region, the area proportion of the rock salt phase structure is 60%-80%, and can be 65%-75%. In some embodiments, based on the total area of the rock salt phase structure and the layered phase structure in the first surface region, the area proportion of the rock salt phase structure can be 60%, 65%, 70%, 75%, 80% or any range therebetween.
[0075] Referring to the testing method for the phase structure in the first surface region and the second surface region in the previous article, the phase structure distribution map of the first surface region and the second surface region obtained according to the aforementioned method was used, and the phase structure distribution area in the first surface region and the second surface region was calculated using ImageJ software to obtain the area proportion of different phase structures in the first surface region and the second surface region.
[0076] By controlling the area ratio of the rock salt phase structure and the layered phase structure in the first surface region within an appropriate range, the structural stability and thermal stability of the material are improved while also enabling the material to have good lithium ion transmission properties, thereby comprehensively improving the cycle performance of the battery.
[0077] In some embodiments, based on the total moles of metal elements other than Li in the first surface region, the molar content of nickel is 50%-80%. In some embodiments, based on the total moles of metal elements other than Li in the first surface region, the molar content of nickel can be 50%, 60%, 65%, 70%, 75%, 80% or any range therebetween.
[0078] The testing method for the molar content of nickel in the first surface area can be tested by methods known in the art. As an example, the battery is disassembled to obtain the positive electrode sheet, the positive electrode sheet is cut into samples of appropriate size (5mm*5mm) and affixed to the sample plate, the sample is placed in the XPS sample chamber, and the sample is sent to the analysis chamber after vacuuming. An Ar ion source of 0.5keV~5keV is used as an ion gun for depth analysis, and the spot size is 50μm-400μm. Then, the depth profiling parameters are set for testing. After the surface is sputtered to a certain depth (according to the specific area of the first surface area determined above, the example is that the surface is sputtered to 10nm), a narrow scan analysis of the nickel element is performed, and the peak area is calculated using C1s as the calibration to obtain the molar content of the nickel element.
[0079] The molar content of nickel in the first surface region is within a suitable range, which is conducive to the formation of a rock salt phase with a suitable area ratio in the first surface region, so as to achieve the purpose of taking into account both the stability of the material and the transmission performance of lithium ions, and comprehensively improve the cycle performance of the battery.
[0080] In some embodiments, based on the total area of the spinel phase structure and the layered phase structure in the second surface region, the area proportion of the spinel phase structure is 50%-90%, and can be 60%-80%. In some embodiments, based on the total area of the spinel phase structure and the layered phase structure in the second surface region, the area proportion of the spinel phase structure can be 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90% or any range of values therebetween.
[0081] In some embodiments, based on the total area of the spinel phase structure and the layered phase structure in the second surface region, the layered phase structure area in the second surface region accounts for 10%-50%, and can be optionally 20%-40%. In some embodiments, based on the total area of the spinel phase structure and the layered phase structure in the second surface region, the layered phase structure area in the second surface region can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, or any range of values therebetween.
[0082] By controlling the area ratio of the spinel phase structure and the layered phase structure in the second surface region within an appropriate range, the structural stability and lattice adaptability of the material are improved, while also enabling the material to have excellent lithium ion performance and lithium ion storage sites, thereby comprehensively improving the cycle performance of the battery.
[0083] In some embodiments, based on the total moles of metal elements other than Li in the second surface region, the molar content of the cobalt element is 60%-90%. In some embodiments, based on the total moles of metal elements other than Li in the second surface region, the molar content of the cobalt element can be 60%, 65%, 70%, 75%, 80%, 85%, 90% or any range therebetween.
[0084] The test method for the molar content of the cobalt element in the second surface area can be tested by a method known in the art. As an example, the test method for the molar content of the nickel element in the first surface area can be referred to. The positions of the first surface area and the second surface area are determined according to the aforementioned test method. For example, the first surface area is an area formed by a distance of 10 nm extending from the surface of the particle to the interior of the particle, and the second surface area is an area formed by a distance of 10 nm extending from the surface of the particle to 60 nm extending from the surface of the particle to the interior of the particle. First, sputter 10 nm from the surface to obtain the elemental analysis data of the first surface area, and then continue to sputter to 60 nm into the particle to obtain the elemental analysis data of the second surface area, and obtain the molar content of the cobalt element in the second surface area.
[0085] The molar content of the cobalt element in the second surface region is within a suitable range, which is conducive to forming a spinel phase structure with a suitable area ratio in the second surface region, achieving the purpose of taking into account both the stability of the material and the transmission speed of lithium ions, and comprehensively improving the cycle performance of the battery.
[0086] In some embodiments, based on the total area of the phase structures in the first surface region, the total area of the rock salt phase structure and the layered phase structure accounts for greater than or equal to 98%.
[0087] In some embodiments, based on the total area of the phase structures in the first surface region, the total area ratio of the rock salt phase structure and the layered phase structure can be selected to be 98%, 99%, 99.5%, 100% or any numerical range therebetween.
[0088] The method for determining the total area ratio of the rock salt phase structure and the layered phase structure refers to the test method for the area ratio of the rock salt phase structure mentioned above.
[0089] The total area ratio of the rock salt phase structure and the layered phase structure in the first surface region is within an appropriate range, so that the first surface region has a rock salt phase structure and a layered phase structure with an appropriate area ratio, so that the rock salt phase structure and the layered phase structure in the first surface region can maximize their respective structural advantages and achieve the purpose of improving the cycle performance of the battery.
[0090] In some embodiments, based on the total area of the phase structures in the second surface region, the total area of the spinel phase structure and the layered phase structure accounts for greater than or equal to 98%.
[0091] In some embodiments, based on the total area of the phase structures in the second surface region, the total area ratio of the spinel phase structure and the layered phase structure can be selected to be 98%, 99%, 99.5%, 100% or any numerical range therebetween.
[0092] The total area ratio of the spinel phase structure and the layered phase structure in the second surface region is within an appropriate range, so that the second surface region has a spinel phase structure and a layered phase structure with an appropriate area ratio, so that the spinel phase structure and the layered phase structure in the second surface region can maximize their respective structural advantages and achieve the purpose of improving the cycle performance of the battery.
[0093] In some embodiments, based on the molar amount of metal elements other than Li in the lithium-containing transition metal oxide, the molar content of nickel element in the lithium-containing transition metal oxide is greater than or equal to 60%, optionally greater than or equal to 80%, and more optionally greater than or equal to 90%.
[0094] In some embodiments, based on the molar amount of metal elements other than Li in the lithium-containing transition metal oxide, the molar content of nickel element in the lithium-containing transition metal oxide can be selected as 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 98% or any numerical range therebetween.
[0095] The test method for the molar content of nickel in lithium-containing transition metal oxides can be tested by methods known in the art. As an example, the test is performed with reference to EPA 6010D-2014 standard; specifically, the battery is disassembled to obtain the positive electrode sheet, the positive electrode film layer is peeled off from the current collector, and then dissolved in N-methylpyrrolidone solvent. After the binder, dispersant, etc. in the positive electrode film layer are dissolved in the solvent, the sample to be tested is filtered and dried to obtain the sample to be tested. ICP-OES (element analysis-inductively coupled plasma emission spectrometry) can be used to test the sample to be tested. The sample to be tested is first dissolved into a liquid with a strong acid, and then the liquid is introduced into an ICP light source by atomization. The gaseous atoms to be tested are further ionized and excited in a strong magnetic field, and then restored from the excited state to the ground state; energy is released in the above process and recorded as different characteristic spectral lines for elemental quantitative analysis.
[0096] In order to increase the energy density of the battery, high-nickel lithium-containing transition metal oxides are generally used. However, the increase in nickel content will intensify the side reactions between the material and the electrolyte, resulting in a decrease in the battery's cycle capacity.
[0097] The present application improves the structural stability of the material while providing the material with a certain lithium ion transmission path by simultaneously including a first phase structure including a layered phase structure and a second phase structure including a spinel phase structure or a layered phase structure in the first surface region and the second surface region of the lithium-containing transition metal oxide, thereby comprehensively improving the cycle performance of the battery.
[0098] In some embodiments, the positive electrode active material further includes a modifying element, and the modifying element includes any one or more of Zr, Al, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K.
[0099] The type of the modifying element is determined by referring to the above-mentioned test method for the molar content of nickel element.
[0100] The positive electrode active material includes modifying elements of Zr, Al, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb or K, which can further improve the cycle stability of the material and improve the cycle stability of the battery.
[0101] In some embodiments, based on the mass of the lithium-containing transition metal oxide, the mass content of the modifying element is less than or equal to 3000 ppm.
[0102] In some embodiments, based on the mass of the lithium-containing transition metal oxide, the mass content of the modifying element may be 10 ppm, 50 ppm, 100 ppm, 200 ppm, 500 ppm, 1000 ppm, 1500 ppm, 2000 ppm, 2500 ppm, 3000 ppm or any range therebetween.
[0103] The mass content of the modifying element is determined by referring to the test method for the molar content of the nickel element mentioned above.
[0104] When the mass content of the modifying elements is within an appropriate range, it can improve the cyclic stability of the material while increasing the gram capacity of the material, thereby comprehensively improving the cyclic performance and energy density of the battery.
[0105] In some embodiments, the positive electrode active material includes Li a1 Ni x1 Co y1 Mn 1-x1-y1 M1 w1 O 2-b1 , Li a2 Ni x2 Co y2 Al 1-x2-y2 M2 w2 O 2-b2 Any of the following;
[0106] Among them, 0.8≤a1≤1.2, 0.6≤x1≤1, 0≤y1≤0.4, -0.1≤b1≤0.1, 0≤w1≤0.1;
[0107] 0.8≤a2≤1.2, 0.6≤x2≤1, 0≤y2≤0.4, -0.1≤b2≤0.1, 0≤w2≤0.1, M1 includes at least one element among Zr, Al, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K, and M2 includes at least one element among Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K.
[0108] In any embodiment, the positive electrode active material includes Li a1 Ni x1 Co y1 Mn 1-x1-y1 M1 w1 O 2-b1 , Li a2 Ni x2 Co y2 Al 1-x2-y2 M2 w2 O 2-b2 Any of the following;
[0109] Among them, 0.8≤a1≤1.2, 0.8≤x1≤1, 0≤y1≤0.2, -0.1≤b1≤0.1, 0≤w1≤0.1;
[0110] 0.8≤a2≤1.2, 0.8≤x2≤1, 0≤y2≤0.2, -0.1≤b2≤0.1, 0≤w2≤0.1, M1 includes at least one element among Zr, Al, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K, and M2 includes at least one element among Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K.
[0111] In some embodiments, a1 can be selected as 0.8, 0.9, 1.0, 1.1, 1.2 or any range therebetween.
[0112] In some embodiments, x1 can be selected as 0.6, 0.7, 0.8, 0.9, 1.0 or any range of values therebetween.
[0113] In some embodiments, y1 may be 0, 0.1, 0.2, 0.3, 0.4, or any range of values therebetween.
[0114] In some embodiments, b1 can be selected as -0.1, 0, 0.1, or any range of values therebetween.
[0115] In some embodiments, w1 can be selected as 0, 0.05, 0.1, or any range of values therebetween.
[0116] In some embodiments, a2 can be selected as 0.8, 0.9, 1.0, 1.1, 1.2 or any range therebetween.
[0117] In some embodiments, x2 can be selected to be 0.6, 0.7, 0.8, 0.9, 1.0, or any range of values therebetween.
[0118] In some embodiments, y2 can be selected as 0, 0.1, 0.2, 0.3, 0.4 or any range of values therebetween.
[0119] In some embodiments, b2 can be selected as -0.1, 0, 0.1, or any range of values therebetween.
[0120] In some embodiments, w2 can be selected as 0, 0.05, 0.1, or any range of values therebetween.
[0121] The chemical formula of the positive electrode active material can be confirmed by any method and any testing equipment in the art, and an example is as follows: specifically, the battery is disassembled to obtain the positive electrode sheet, the positive electrode film layer is peeled off from the current collector, and then dissolved in N-methylpyrrolidone solvent. After the binder, dispersant, etc. in the positive electrode film layer are dissolved in the solvent, it is filtered and dried to obtain a sample to be tested, which is digested with HF and added to an ICP-OES instrument to detect the content of Li, Ni, Co, Mn, Al, M1, and M2 elements to obtain a specific molar ratio of the element content and a specific chemical composition.
[0122] In some embodiments, a method for preparing a lithium-containing transition metal oxide is provided:
[0123] Step S0: Providing a precursor, the chemical composition of which is Ni x1 Co y1 Mn 1-x1-y1 (OH) 2 or Ni x2 Co y2 Al 1-x2-y2 (OH) 2 , where 0.6≤x1≤1, 0≤y1≤0.4, 0.6≤x2≤1, 0≤y2≤0.4;
[0124] Step S1: performing a first sintering on a first raw material including a lithium source and a precursor to obtain an initial product;
[0125] Step S2: performing a second sintering treatment on the second raw material including the initial product and the cobalt source to obtain a secondary product;
[0126] Step S3: stirring the secondary product with the weakly acidic additive solution, and drying the intermediate product;
[0127] Step S4: subjecting the intermediate product to a third sintering treatment to obtain a lithium-containing transition metal oxide, wherein the particles of the lithium-containing transition metal oxide include an internal region and a surface region that at least partially surrounds the internal region, the surface region includes a first surface region and a second surface region, the second surface region is located between the first surface region and the internal region, the first surface region and the second surface region both contain a first phase structure and a second phase structure, wherein the first phase structure includes a layered phase structure, and the second phase structure includes at least one of a spinel phase structure and a rock salt phase structure, wherein the first surface region includes a layered phase structure and a rock salt phase structure, and the second surface region includes a layered phase structure and a spinel phase structure.
[0128] In some embodiments, the ratio of the molar number of cobalt in the cobalt source to the total molar number of Ni, Co, and Mn in the precursor is 0.005:0.995-0.025:0.975.
[0129] In some embodiments, the temperature of the second sintering process is 400°C-650°C.
[0130] In some embodiments, the second sintering treatment lasts for 4 hours to 10 hours.
[0131] In some embodiments, the first raw material further includes one or more of a Zr source, an Al source, a B source, a Mg source, a Ti source, a W source, a Mo source, a Nb source, a Ta source, a Sr source, a Sb source, and a K source.
[0132] In some embodiments, the molar content of the weak acidic additive in the weak acidic additive solution is 0.05 mol / L-0.2 mol / L.
[0133] In some embodiments, the stirring time in step S3 is 1 min-10 min.
[0134] In some embodiments, the weak acid additive includes one or more of malic acid, maleic acid, benzoic acid, and the like.
[0135] In some embodiments, the sintering time of the third sintering is 6 hours to 12 hours.
[0136] In some embodiments, the sintering temperature of the third sintering is 200°C-450°C.
[0137] In some embodiments, a method for preparing a lithium-containing transition metal oxide is provided:
[0138] Step S0: Providing a precursor, the chemical composition of which is Ni x1 Co y1 Mn 1-x1-y1 (OH) 2 or Ni x2 Co y2 Al 1-x2-y2 (OH) 2 , where 0.6≤x1≤1, 0≤y1≤0.4, 0.6≤x2≤1, 0≤y2≤0.4;
[0139] Step S1: performing a first sintering on a first raw material including a lithium source and a precursor to obtain an initial product;
[0140] Step S2: subjecting a second raw material comprising an initial product and a cobalt source to a second sintering treatment to obtain a lithium-containing transition metal oxide, wherein the particles of the lithium-containing transition metal oxide include an internal region and a surface region that at least partially surrounds the internal region, the surface region includes a first surface region and a second surface region, the second surface region is located between the first surface region and the internal region, the first surface region and the second surface region both include a first phase structure and a second phase structure, wherein the first phase structure includes a layered phase structure, and the second phase structure includes a spinel phase structure.
[0141] In some embodiments, a method for preparing a lithium-containing transition metal oxide is provided:
[0142] Step S0: Providing a precursor, the chemical composition of which is Ni x1 Co y1 Mn 1-x1-y1 (OH) 2 or Ni x2 Co y2 Al 1-x2-y2 (OH) 2 , where 0.6≤x1≤1, 0≤y1≤0.4, 0.6≤x2≤1, 0≤y2≤0.4;
[0143] Step S1: performing a first sintering on a first raw material including a lithium source and a precursor to obtain an initial product;
[0144] Step S2: stirring the initial product and the weakly acidic additive solution, and drying the intermediate product;
[0145] Step S3: subjecting the intermediate product to a third sintering treatment to obtain a lithium-containing transition metal oxide.
[0146] The lithium-transition metal oxide-containing particles include an internal region and a surface region that at least partially surrounds the internal region, the surface region includes a first surface region and a second surface region, the second surface region is located between the first surface region and the internal region, the first surface region and the second surface region both contain a first phase structure and a second phase structure, wherein the first phase structure includes a layered phase structure, and the second phase structure includes a rock salt phase structure.
[0147] In some embodiments, a method for preparing a lithium-containing transition metal oxide is provided:
[0148] Step S0: Providing a precursor, the chemical composition of which is Ni x1 Co y1 Mn 1-x1-y1 (OH) 2 or Ni x2 Coy2 Al 1-x2-y2 (OH) 2 , where 0.6≤x1≤1, 0≤y1≤0.4, 0.6≤x2≤1, 0≤y2≤0.4;
[0149] Step S1: performing a first sintering on a first raw material including a lithium source and a precursor to obtain a first product;
[0150] Step S2: stirring the initial product and the weakly acidic additive solution, and drying the second product;
[0151] Step S3: performing a second sintering treatment on the second product to obtain a third product;
[0152] Step S4: subjecting the second raw material comprising the third product and the cobalt source to a third sintering treatment to obtain a lithium-containing transition metal oxide, wherein the particles of the lithium-containing transition metal oxide include an internal region and a surface region that at least partially surrounds the internal region, the surface region includes a first surface region and a second surface region, the second surface region is located between the first surface region and the internal region, the first surface region and the second surface region both include a first phase structure and a second phase structure, wherein the first phase structure includes a layered phase structure, and the second phase structure includes at least one of a spinel phase structure and a rock salt phase structure, wherein the first surface region includes a layered phase structure and a spinel phase structure, and the second surface region includes a layered phase structure and a rock salt phase structure.
[0153] [Positive electrode]
[0154] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes a lithium-containing transition metal oxide.
[0155] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0156] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0157] In some embodiments, the positive electrode active material layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0158] In some embodiments, the positive electrode active material layer may further include a conductive agent, which may include, for example, at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0159] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0160] [Negative electrode]
[0161] The negative electrode sheet comprises a negative electrode current collector and a negative electrode film layer which is optionally arranged on at least one surface of the negative electrode current collector. The negative electrode film layer comprises a negative electrode active material.
[0162] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0163] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0164] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0165] In some embodiments, the negative electrode film layer may further include a binder, which may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0166] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0167] In some embodiments, the negative electrode film layer may further optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0168] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0169] [Electrolytes]
[0170] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.
[0171] In some embodiments, the electrolyte is an electrolyte solution.
[0172] In some embodiments, the electrolyte includes a lithium salt.
[0173] In some embodiments, the electrolyte includes an organic solvent.
[0174] In some embodiments, the lithium salt can be selected from lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethanesulfonyl imide), lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0175] In some embodiments, the organic solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0176] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0177] [Isolation film]
[0178] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.
[0179] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation. In some embodiments, the isolation membrane can also have one or more coatings.
[0180] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0181] [Outer packaging]
[0182] In some embodiments, the secondary battery may include an outer package for packaging the positive electrode sheet, the negative electrode sheet and the electrolyte. As an example, the positive electrode sheet, the negative electrode sheet and the separator may be laminated or wound to form a laminated structure battery cell or a wound structure battery cell, and the battery cell is packaged in the outer package; the electrolyte adopts the electrolyte described in the first aspect of the present application, and the electrolyte is infiltrated in the battery cell. The number of batteries in the secondary battery may be one or more, which can be adjusted according to demand.
[0183] In one embodiment, the present application provides an electrode assembly. In some embodiments, the positive electrode sheet, the negative electrode sheet and the separator can be made into an electrode assembly by a winding process or a lamination process. The outer packaging can be used to package the above electrode assembly and the electrolyte.
[0184] In some embodiments, the outer packaging of the secondary battery may be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc. In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The present application has no particular restrictions on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, Figure 2 The battery cell 5 is a square structure as an example.
[0185] In some embodiments, reference Figure 3 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0186] In some embodiments, battery cells may be assembled into a battery module. The number of battery cells contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.
[0187] Figure 4 4 is an example of a battery module. Figure 4 In the battery module 4, the plurality of battery cells 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of battery cells 5 may be fixed by fasteners.
[0188] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of battery cells 5 are received in the receiving space.
[0189] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.
[0190] Figure 5 and Figure 6 1 is a battery pack 1 as an example. Figure 5 and Figure 6 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.
[0191] In addition, the present application also provides an electric device, which includes a secondary battery provided in the present application. The secondary battery can be used as a power source for the electric device, or as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.
[0192] As the electrical device, a battery cell, a battery module or a battery pack can be selected according to its usage requirements.
[0193] Figure 7 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.
[0194] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.
[0195] Example
[0196] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0197] 1. Preparation method
[0198] Example 1
[0199] 1) Preparation of positive electrode active materials
[0200] Step S0: nickel sulfate, cobalt sulfate and manganese sulfate are prepared into a mixed salt solution with a concentration of 2 mol / L according to a molar ratio of Ni:Co:Mn = 92:7:1, 4 mol / L NaOH solution is used as an alkaline solution precipitant, and 2 mol / L ammonia water is used as a complexing agent;
[0201] Add 20 L of deionized water to a 100 L reactor, and add a certain amount of NaOH solution to make the pH in the reactor 11 to obtain a reaction bottom solution;
[0202] Under a nitrogen protective atmosphere, the reaction base liquid is heated to 55°C, and at a stirring speed of 600 rpm, a mixed salt solution, an alkali solution and an ammonia solution are added to the reaction base liquid in parallel, and the flow rates of the mixed salt solution, the alkali solution and the ammonia solution are adjusted so that the pH of the reaction solution is 11. After the reaction reaches the target particle size Dv50 (9.5 μm), the pumping is stopped, and the reaction solution is allowed to stand for 24 hours to obtain an aged slurry containing a precursor material, and the precursor material is obtained by washing and drying;
[0203] Step S1: LiOH•H 2 O and the above precursor materials are mixed uniformly at a molar ratio of 1.05:1, and then sintered at 750°C for 15 h in a box furnace under a pure oxygen atmosphere, and the initial product can be obtained by crushing and sieving;
[0204] Step S2: mixing the initial product obtained above with cobalt hydroxide, wherein the ratio of the molar amount of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.02:0.98, and sintering is performed in an oxygen atmosphere at a sintering temperature of 600° C. and a sintering time of 8 hours to obtain a secondary product;
[0205] Step S3: dissolve a certain amount of malic acid in 5L pure water and stir to obtain a 0.1mol / L acidic solution, add 5kg of the intermediate product obtained above into the acidic solution and stir for 2min, then filter and dry to obtain the intermediate product, and sinter at 400°C in an oxygen atmosphere for 6h to obtain the positive electrode active material.
[0206] 2) Positive electrode
[0207] The positive electrode active material, polyvinylidene fluoride and conductive carbon black were mixed in a mass ratio of 94:3:3, and then N-methylpyrrolidone (NMP) was added and stirred for 2 hours. Then, it was stirred in a homogenizer at 1200 r / min until it was evenly mixed, and then evenly coated on the double-side surface of a 13-micron thick aluminum foil current collector. After coating, it was dried in a drying oven at 120°C, cold pressed, and cut to obtain positive electrode sheets.
[0208] 3) Negative electrode
[0209] Artificial graphite, hard carbon, conductive agent acetylene black, binder styrene butadiene rubber (SBR), and thickener sodium carbon methyl cellulose (CMC) are mixed in a weight ratio of 90:5:2:2:1, deionized water is added, and the mixture is stirred evenly in a blender. The slurry is then coated on both sides of an 8-micron thick copper foil, dried in an oven at 120°C, cold pressed, and cut to obtain negative electrode sheets.
[0210] 4) Electrolyte
[0211] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then LiPF 6 Dissolve in the above organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0212] 5) Isolation film
[0213] A polyethylene film with a thickness of 13 μm was used as the separator.
[0214] 6) Preparation of secondary batteries
[0215] The positive electrode sheet, the isolation film, and the negative electrode sheet are stacked in order, so that the isolation film is placed between the positive and negative electrode sheets to play an isolating role, and then wound to obtain a bare battery cell, the tabs are welded to the bare battery cell, and the bare battery cell is placed in an aluminum shell, and the electrolyte is injected. The steps of standing, formation, and capacity are carried out to prepare a secondary battery.
[0216] Example 2
[0217] Compared with Example 1, Example 2 adjusts the preparation method of the positive electrode active material, which is as follows:
[0218] Step S0: nickel sulfate, cobalt sulfate and manganese sulfate are prepared into a mixed salt solution with a concentration of 2 mol / L according to a molar ratio of Ni:Co:Mn = 92:7:1, 4 mol / L NaOH solution is used as an alkaline solution precipitant, and 2 mol / L ammonia water is used as a complexing agent;
[0219] Add 20 L of deionized water to a 100 L reactor, and add a certain amount of NaOH solution to make the pH in the reactor 11 to obtain a reaction bottom solution;
[0220] Under a nitrogen protective atmosphere, the reaction base liquid is heated to 55°C, and at a stirring speed of 600 rpm, a mixed salt solution, an alkali solution and an ammonia solution are added to the reaction base liquid in parallel, and the flow rates of the mixed salt solution, the alkali solution and the ammonia solution are adjusted so that the pH of the reaction solution is 11. After the reaction reaches the target particle size Dv50 (9.5 μm), the pumping is stopped, and the reaction solution is allowed to stand for 24 hours to obtain an aged slurry containing a precursor material, and the precursor material is obtained by washing and drying;
[0221] Step S1: LiOH•H 2 O and the above-mentioned precursor materials, Nb 2 O 5 (calculated as the molar number of Nb element) are mixed uniformly according to the molar ratio of 1.05:1:0.002, and then sintered at 750°C for 15 h in a box furnace under a pure oxygen atmosphere, and the initial product can be obtained by crushing and sieving;
[0222] Step S2: mixing the initial product obtained above with cobalt hydroxide, wherein the ratio of the molar number of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.02:0.98, and sintering is performed in an oxygen atmosphere at a sintering temperature of 600° C. and a sintering time of 8 hours to obtain a secondary product;
[0223] Step S3: dissolve a certain amount of malic acid in 5L pure water and stir to obtain a 0.1mol / L acidic solution, add 5kg of the intermediate product obtained above into the acidic solution and stir for 2min, then filter and dry to obtain the intermediate product, and sinter at 400°C in an oxygen atmosphere for 6h to obtain the positive electrode active material.
[0224] Example 3
[0225] Compared with Example 1, Example 3 adjusts the preparation method of the positive electrode active material, which is as follows:
[0226] Step S0: nickel sulfate, cobalt sulfate and manganese sulfate are prepared into a mixed salt solution with a concentration of 2 mol / L according to a molar ratio of Ni:Co:Mn = 80:10:10, 4 mol / L NaOH solution is used as an alkaline solution precipitant, and 2 mol / L ammonia water is used as a complexing agent;
[0227] Add 20 L of deionized water to a 100 L reactor, and add a certain amount of NaOH solution to make the pH in the reactor 11 to obtain a reaction bottom solution;
[0228] Under a nitrogen protective atmosphere, the reaction base liquid is heated to 55°C, and at a stirring speed of 600 rpm, a mixed salt solution, an alkali solution and an ammonia solution are added to the reaction base liquid in parallel, and the flow rates of the mixed salt solution, the alkali solution and the ammonia solution are adjusted so that the pH of the reaction solution is 11. After the reaction reaches the target particle size Dv50 (9.5 μm), the pumping is stopped, and the reaction solution is allowed to stand for 24 hours to obtain an aged slurry containing a precursor material, and the precursor material is obtained by washing and drying;
[0229] Step S1: LiOH•H 2 O and the above precursor materials are mixed uniformly at a molar ratio of 1.05:1, and then sintered at 780°C for 15 h in a box furnace under a pure oxygen atmosphere, and the initial product can be obtained by crushing and sieving;
[0230] Step S2: mixing the initial product obtained above with cobalt hydroxide, wherein the ratio of the molar amount of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.02:0.98, and sintering is performed in an oxygen atmosphere at a sintering temperature of 600° C. and a sintering time of 8 hours to obtain a secondary product;
[0231] Step S3: dissolve a certain amount of malic acid in 5L pure water and stir to obtain a 0.1mol / L acidic solution, add 5kg of the intermediate product obtained above into the acidic solution and stir for 2min, filter and dry to obtain the intermediate product, and sinter at 400°C for 6h in an oxygen atmosphere to obtain the positive electrode active material.
[0232] Embodiment 4-7
[0233] Compared with Example 1, Examples 4-7 adjust the area ratio of the rock salt phase structure in the first surface region by adjusting step S3 in the method for preparing the positive electrode active material, as follows:
[0234] Example 4: A certain amount of malic acid was dissolved in 5 L of pure water and stirred to obtain a 0.1 mol / L acidic solution. 5 kg of the intermediate product obtained above was added to the acidic solution and stirred for 1.5 min, then filtered and dried to obtain the intermediate product, which was sintered at 400°C for 6 h in an oxygen atmosphere to obtain the positive electrode active material.
[0235] Example 5: A certain amount of malic acid was dissolved in 5 L of pure water and stirred to obtain a 0.1 mol / L acidic solution. 5 kg of the intermediate product obtained above was added to the acidic solution and stirred for 2.5 min, then filtered and dried to obtain the intermediate product, which was sintered at 400 °C in an oxygen atmosphere for 6 h to obtain the positive electrode active material.
[0236] Example 6: A certain amount of malic acid was dissolved in 5 L of pure water and stirred to obtain a 0.1 mol / L acidic solution. 5 kg of the intermediate product obtained above was added to the acidic solution and stirred for 2 min, then filtered and dried to obtain the intermediate product, which was sintered at 450° C. for 6 h in an oxygen atmosphere to obtain the positive electrode active material.
[0237] Example 7: A certain amount of malic acid was dissolved in 5 L of pure water and stirred to obtain a 0.1 mol / L acidic solution. 5 kg of the intermediate product obtained above was added to the acidic solution and stirred for 2.5 min, then filtered and dried to obtain the intermediate product, which was sintered at 450°C for 6 h in an oxygen atmosphere to obtain the positive electrode active material.
[0238] Embodiment 8-11
[0239] Compared with Example 1, Examples 8-11 adjust the area ratio of the spinel phase structure in the second surface layer region by adjusting step S2 in the method for preparing the positive electrode active material, as follows:
[0240] Example 8: The initial product obtained above is mixed with cobalt hydroxide, wherein the ratio of the molar amount of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.01:0.99, and sintering is carried out in an oxygen atmosphere at a sintering temperature of 600°C and a sintering time of 8 hours to obtain a secondary product.
[0241] Example 9: The initial product obtained above is mixed with cobalt hydroxide, wherein the ratio of the molar amount of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.02:0.98, and sintering is carried out in an oxygen atmosphere at a sintering temperature of 620°C and a sintering time of 8 hours to obtain a secondary product.
[0242] Example 10: The initial product obtained above is mixed with cobalt hydroxide, wherein the ratio of the molar amount of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.025:0.975, and sintering is carried out in an oxygen atmosphere at a sintering temperature of 600°C and a sintering time of 8 hours to obtain a secondary product.
[0243] Example 11: The initial product obtained above is mixed with cobalt hydroxide, wherein the ratio of the molar amount of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.025:0.975, and sintering is carried out in an oxygen atmosphere at a sintering temperature of 650°C and a sintering time of 8 hours to obtain a secondary product.
[0244] Example 12
[0245] Compared with Example 1, Example 12 adjusts the preparation method of the positive electrode active material, which is as follows:
[0246] Step S1: LiOH•H 2 O and the precursor material in Example 1 are mixed uniformly at a molar ratio of 1.05:1, and then sintered at 750° C. for 15 h in a box furnace under a pure oxygen atmosphere, and the initial product can be obtained by crushing and sieving;
[0247] Step S2: mixing the initial product obtained above with cobalt hydroxide, wherein the ratio of the molar amount of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.02:0.98, and sintering is performed in an oxygen atmosphere at a sintering temperature of 600° C. and a sintering time of 12 h to obtain an intermediate product;
[0248] Step S3: dissolve a certain amount of malic acid in 5L pure water and stir to obtain a 0.1mol / L acidic solution, add 5kg of the intermediate product obtained above into the acidic solution and stir for 5min, filter and dry, and sinter at 400°C in an oxygen atmosphere for 8h to obtain a positive electrode active material.
[0249] Example 13
[0250] Compared with Example 1, Example 13 adjusts the preparation method of the positive electrode active material, which is as follows:
[0251] Step S1: LiOH•H 2 O and the precursor material in Example 1 are mixed uniformly at a molar ratio of 1.05:1, and then sintered at 750° C. for 15 h in a box furnace under a pure oxygen atmosphere, and the initial product can be obtained by crushing and sieving;
[0252] Step S2: mixing the initial product obtained above with cobalt hydroxide, wherein the ratio of the molar amount of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.02:0.98, and sintering is performed in an oxygen atmosphere at a sintering temperature of 580° C. and a sintering time of 7 hours to obtain a secondary product;
[0253] Step S3: dissolve a certain amount of malic acid in 5L pure water and stir to obtain a 0.1mol / L acidic solution, add 5kg of the intermediate product obtained above into the acidic solution and stir for 2min, then filter and dry to obtain the intermediate product, and sinter at 400°C in an oxygen atmosphere for 6h to obtain the positive electrode active material.
[0254] Comparative Example 1
[0255] Compared with Example 1, the preparation method of the positive electrode active material in Comparative Example 1 is adjusted as follows:
[0256] Step S0: nickel sulfate, cobalt sulfate and manganese sulfate are prepared into a mixed salt solution with a concentration of 2 mol / L according to a molar ratio of Ni:Co:Mn = 92:7:1, 4 mol / L NaOH solution is used as an alkaline solution precipitant, and 2 mol / L ammonia water is used as a complexing agent;
[0257] Add 20 L of deionized water to a 100 L reactor, and add a certain amount of NaOH solution to make the pH in the reactor 11 to obtain a reaction bottom solution;
[0258] Under a nitrogen protective atmosphere, the reaction base liquid is heated to 55°C, and at a stirring speed of 600 rpm, a mixed salt solution, an alkali solution and an ammonia solution are added to the reaction base liquid in parallel, and the flow rates of the mixed salt solution, the alkali solution and the ammonia solution are adjusted so that the pH of the reaction solution is 11. After the reaction reaches the target particle size Dv50 (9.5 μm), the pumping is stopped, and the reaction solution is allowed to stand for 24 hours to obtain an aged slurry containing a precursor material, and the precursor material is obtained by washing and drying;
[0259] Step S1: LiOH•H 2 O and the above-mentioned precursor materials are uniformly mixed in a molar ratio of 1.05:1, and then sintered at 750° C. for 15 h in a box furnace under a pure oxygen atmosphere, and the positive electrode active material can be obtained by crushing and sieving.
[0260] Comparative Example 2
[0261] Compared with Example 1, Comparative Example 2 adjusted the preparation method of the positive electrode active material, as follows:
[0262] Step S1: LiOH•H 2 O and the precursor material prepared in Example 1 are mixed uniformly at a molar ratio of 1.05:1, and then sintered at 750° C. for 15 h in a box furnace under a pure oxygen atmosphere, and the initial product is obtained by crushing and sieving;
[0263] Step S2: dissolve a certain amount of malic acid in 5L pure water and stir to obtain a 0.1mol / L acidic solution, add 5kg of the intermediate product obtained above into the acidic solution and stir for 12min, filter and dry, and sinter at 400°C in an oxygen atmosphere for 6h to obtain a positive electrode active material.
[0264] Comparative Example 3
[0265] Compared with Example 1, Comparative Example 3 adjusted the preparation method of the positive electrode active material, as follows:
[0266] Step S1: LiOH•H 2O and the precursor material prepared in Example 1 are mixed uniformly at a molar ratio of 1.05:1, and then sintered at 750° C. for 15 h in a box furnace under a pure oxygen atmosphere, and the initial product is obtained by crushing and sieving;
[0267] Step S2: Mix the initial product obtained above with cobalt hydroxide, wherein the ratio of the molar amount of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.02:0.98, and sinter under an oxygen atmosphere at a sintering temperature of 660° C. for 12 hours to obtain a positive electrode active material.
[0268] Comparative Example 4
[0269] Compared with Example 1, Comparative Example 4 adjusted the preparation method of the positive electrode active material, as follows:
[0270] Step S1: LiOH•H 2 O and the precursor material prepared in Example 1 are mixed uniformly at a molar ratio of 1.05:1, and then sintered at 750° C. for 15 h in a box furnace under a pure oxygen atmosphere, and the initial product is obtained by crushing and sieving;
[0271] Step S2: mixing the initial product obtained above with cobalt hydroxide, wherein the ratio of the molar amount of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.03:0.97, and sintering is performed in an oxygen atmosphere at a sintering temperature of 600° C. and a sintering time of 12 h to obtain a secondary product;
[0272] Step S3: dissolve a certain amount of malic acid in 5L pure water and stir to obtain a 0.2mol / L acidic solution, add 5kg of the intermediate product obtained above into the acidic solution and stir for 10min, filter and dry to obtain the intermediate product, and sinter at 450°C for 10h in an oxygen atmosphere to obtain the positive electrode active material.
[0273] Comparative Example 5
[0274] Compared with Example 1, the preparation method of the positive electrode active material in Comparative Example 5 is adjusted as follows:
[0275] Step S1: LiOH•H 2 O and the precursor material prepared in Example 1 are mixed uniformly at a molar ratio of 1.05:1, and then sintered at 750° C. for 15 h in a box furnace under a pure oxygen atmosphere, and the initial product is obtained by crushing and sieving;
[0276] Step S2: dissolve a certain amount of malic acid in 5L pure water and stir to obtain a 0.1mol / L acidic solution, add 5kg of the intermediate product obtained above into the acidic solution and stir for 10min, filter and dry, and sinter at 500°C in an oxygen atmosphere for 6h to obtain a positive electrode active material.
[0277] Comparative Example 6
[0278] Compared with Example 1, Comparative Example 6 adjusted the preparation method of the positive electrode active material, as follows:
[0279] Step S1: LiOH•H 2 O and the precursor material prepared in Example 1 are mixed uniformly at a molar ratio of 1.05:1, and then sintered at 750° C. for 15 h in a box furnace under a pure oxygen atmosphere, and the initial product is obtained by crushing and sieving;
[0280] Step S2: Mix the initial product obtained above with cobalt hydroxide, wherein the ratio of the molar amount of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.02:0.98, and sinter under an oxygen atmosphere at a sintering temperature of 650° C. for 8 hours to obtain a positive electrode active material.
[0281] Comparative Example 7
[0282] Compared with Example 1, Comparative Example 7 adjusts the preparation method of the positive electrode active material, which is as follows:
[0283] Step S1: LiOH•H 2 O and the precursor material in Example 1 are mixed uniformly at a molar ratio of 1.05:1, and then sintered at 750° C. for 15 h in a box furnace under a pure oxygen atmosphere, and the initial product can be obtained by crushing and sieving;
[0284] Step S2: dissolving a certain amount of malic acid in 5L of pure water and stirring to obtain a 0.1mol / L acidic solution, adding 5kg of the initial product obtained above into the acidic solution and stirring for 10min, filtering and drying, and sintering at 500°C for 6h in an oxygen atmosphere to obtain an intermediate product;
[0285] Step S3: Mix the intermediate product obtained above with cobalt hydroxide, wherein the ratio of the molar amount of cobalt in the added cobalt hydroxide to the total molar amount of Ni, Co, and Mn elements in the precursor is 0.005:0.995, and sinter under an oxygen atmosphere at a sintering temperature of 550° C. for 8 hours to obtain a positive electrode active material.
[0286] 2. Test Method
[0287] 1. Cycle capacity retention rate of secondary batteries
[0288] At 25°C, charge the secondary battery at a constant current of 1C to a voltage of 4.25V, then charge at a constant voltage of 4.25V to a current ≤0.05mA. After standing for 5 minutes, discharge the battery at a constant current of 1C to a voltage of 2.8V. This is the first charge / discharge cycle of the battery. The discharge capacity is recorded as the discharge capacity of the first cycle of the battery (C0). Repeat the above steps for the same battery. The discharge capacity of the battery after the 500th cycle (C1) is the capacity retention rate after 500 cycles = C1 / C0×100%.
[0289] III. Analysis of test results of various embodiments and comparative examples
[0290] The positive electrode active materials and secondary batteries of the embodiments and comparative examples were prepared according to the above methods, and various parameters were measured. The results are shown in the following table.
[0291] Table 1
[0292]
[0293] Table 2
[0294]
[0295] It can be seen from the above table that the secondary batteries in Examples 1-13 of the present application include: a positive electrode plate, a negative electrode plate and an electrolyte, the positive electrode plate includes a positive electrode collector and a positive electrode active material layer arranged on at least one side of the positive electrode collector, the positive electrode active material layer includes a positive electrode active material, the positive electrode active material includes a lithium-containing transition metal oxide, the particles of the lithium-containing transition metal oxide include an internal region and a surface region that at least partially surrounds the internal region, the surface region includes a first surface region and a second surface region, the second surface region is located between the first surface region and the internal region, the first surface region and the second surface region both contain a first phase structure and a second phase structure, wherein the first phase structure includes a layered phase structure, and the second phase structure includes at least one of a spinel phase structure and a rock salt phase structure, wherein the first surface region includes a rock salt phase structure and a layered phase structure, and the second surface region includes a spinel phase structure and a layered phase structure.
[0296] From the comparison between Examples 1-13 and Comparative Example 1, it can be seen that the first surface region and the second surface region include a second phase structure of a spinel phase structure or a rock salt phase structure, which can improve the cycle capacity retention rate of the battery and improve the cycle performance of the battery.
[0297] From the comparison between Examples 1-13 and Comparative Examples 2-4, it can be seen that the first surface region and the second surface region contain a layered phase structure, which can increase the cycle capacity retention rate of the battery and improve the cycle performance of the battery.
[0298] From the comparison between Examples 1-13 and Comparative Examples 6-7, it can be seen that the first surface region includes a rock salt phase structure and a layered phase structure, which can further improve the cycle capacity retention rate of the battery and improve the cycle performance of the battery.
[0299] From the comparison between Examples 1-13 and Examples 5 and 7, it can be seen that the second surface region includes a spinel phase structure and a layered phase structure, which can further improve the cycle capacity retention rate of the battery and improve the cycle performance of the battery.
[0300] From the comparison between Example 1-11 and Example 12, it can be seen that the first surface region refers to the region extending 10 nm from the particle surface of the positive electrode active material to the inside of the particle, which can further improve the cycle capacity retention rate of the battery and improve the cycle performance of the battery.
[0301] From the comparison between Examples 1-11 and Example 13, it can be seen that the second surface region refers to the region extending from 10 nm to 60 nm from the particle surface of the positive electrode active material to the interior of the particle, which can further improve the battery's cycle capacity retention rate and improve the battery's cycle performance.
[0302] As can be seen from Examples 1, 4-7, based on the total area of the rock salt phase structure and the layered phase structure in the first surface region, the area of the rock salt phase structure accounts for 60%-80%, and the area of the layered phase structure in the first surface region accounts for 20%-40%. The battery has a high cycle capacity retention rate and the battery has excellent cycle performance. As can be seen from the comparison of Examples 1, 5-6 with Examples 4 and 7, based on the total area of the rock salt phase structure and the layered phase structure in the first surface region, the area of the rock salt phase structure accounts for 65%-75%, and the area of the layered phase structure in the first surface region accounts for 25%-35%, which can further improve the cycle capacity retention rate of the battery and improve the cycle performance of the battery.
[0303] From Examples 1, 8-11, it can be seen that based on the total area of the spinel phase structure and the layered phase structure in the second surface region, the area of the spinel phase structure accounts for 50%-90%, and the layered phase structure in the second surface region accounts for 10%-50%. The battery has a high cycle capacity retention rate and the battery has excellent cycle performance. From the comparison of Examples 1, 9-10 with Examples 8 and 11, it can be seen that based on the total area of the spinel phase structure and the layered phase structure in the second surface region, the area of the spinel phase structure accounts for 60%-80%, and the layered phase structure in the second surface region accounts for 20%-40%, which can further improve the cycle capacity retention rate of the battery and improve the cycle performance of the battery.
[0304] From the comparison between Example 2 and Example 1, it can be seen that the positive electrode active material also includes any one or more modifying elements of Zr, Al, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K, which can further improve the cycle capacity retention rate of the battery and improve the cycle performance of the battery.
[0305] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A secondary battery, characterized in that: include: Positive electrode sheet, negative electrode sheet and electrolyte, The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes a lithium-containing transition metal oxide. The lithium-transition metal oxide-containing particles include an inner region and a surface region at least partially surrounding the inner region. The surface region includes a first surface region and a second surface region, the second surface region is located between the first surface region and the inner region, and the first surface region and the second surface region both include a first phase structure and a second phase structure, The first phase structure includes a layered phase structure, and the second phase structure includes at least one of a spinel phase structure and a rock salt phase structure. The first surface region includes a rock salt phase structure and a layered phase structure, the second surface region includes a spinel phase structure and a layered phase structure, and the first surface region refers to a region extending from the surface of the lithium-containing transition metal oxide particle to the inside of the particle by a distance of 10 nm. The second surface region refers to a region extending from 10 nm to 60 nm from the surface of the lithium-containing transition metal oxide particle to the interior of the particle. The inner region comprises a lamellar phase structure, The lithium-containing transition metal oxide includes Li a1 Ni x1 Co y1 Mn 1-x1-y1 M1 w1 O 2-b1 , Li a2 Ni x2 Co y2 Al 1-x2- y2 M2 w2 O 2-b2 Any of the following: Among them, 0.8≤a1≤1.2, 0.6≤x1≤1, 0≤y1≤0.4, -0.1≤b1≤0.1, 0≤w1≤0.1; 0.8≤a2≤1.2,0.6≤x2≤1,0≤y2≤0.4,-0.1≤b2≤0.1, 0≤w2≤0.1, M1 includes at least one element selected from Zr, Al, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K. M2 includes at least one element of Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, K, The space group of the rock salt phase structure is Fm-3m, the space group of the layered phase structure is R-3m, and the space group of the spinel phase structure is Fd-3m.
2. The secondary battery according to claim 1, characterized in that: Based on the total area of the rock salt phase structure and the layered phase structure in the first surface region, the area of the rock salt phase structure accounts for 60%-80%, and / or the area of the layered phase structure in the first surface region accounts for 20%-40%.
3. The secondary battery according to claim 1, characterized in that: Based on the total area of the rock salt phase structure and the layered phase structure in the first surface region, the area of the rock salt phase structure accounts for 65%-75%, and / or the area of the layered phase structure in the first surface region accounts for 25%-35%.
4. The secondary battery according to claim 1, characterized in that: Based on the total molar number of metal elements except Li in the first surface layer region, the molar content of nickel element is 50%-80%.
5. The secondary battery according to claim 1, characterized in that: Based on the total area of the spinel phase structure and the layered phase structure in the second surface region, the area of the spinel phase structure accounts for 50%-90%, and / or, the area of the layered phase structure in the second surface region accounts for 10%-50%.
6. The secondary battery according to claim 1, characterized in that: Based on the total area of the spinel phase structure and the layered phase structure in the second surface region, the area of the spinel phase structure accounts for 60%-80%, and / or, the area of the layered phase structure in the second surface region accounts for 20%-40%.
7. The secondary battery according to claim 1, characterized in that: Based on the total molar number of metal elements except Li in the second surface layer region, the molar content of the cobalt element is 60%-90%.
8. The secondary battery according to claim 1, characterized in that: Based on the molar amount of metal elements other than Li in the lithium-containing transition metal oxide, the molar content of nickel element in the lithium-containing transition metal oxide is greater than or equal to 60%.
9. The secondary battery according to claim 1, characterized in that: Based on the molar amount of metal elements other than Li in the lithium-containing transition metal oxide, the molar content of nickel element in the lithium-containing transition metal oxide is greater than or equal to 80%.
10. The secondary battery according to claim 1, characterized in that: Based on the molar amount of metal elements other than Li in the lithium-containing transition metal oxide, the molar content of nickel element in the lithium-containing transition metal oxide is greater than or equal to 90%.
11. The secondary battery according to claim 1, characterized in that: The lithium-containing transition metal oxide also includes a modifying element, and the modifying element includes one or more of Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K.
12. The secondary battery according to claim 11, characterized in that: Based on the mass of the lithium-containing transition metal oxide, the mass content of the modifying element is less than or equal to 3000 ppm.
13. The secondary battery according to claim 1, characterized in that: The lithium-containing transition metal oxide includes Li a1 Ni x1 Co y1 Mn 1-x1-y1 M1 w1 O 2-b1 , Li a2 Ni x2 Co y2 Al 1-x2-y2 M2 w2 O 2-b2 Any of the following: Among them, 0.8≤a1≤1.2, 0.8≤x1≤1, 0≤y1≤0.2, -0.1≤b1≤0.1, 0≤w1≤0.1; 0.8≤a2≤1.2,0.8≤x2≤1,0≤y2≤0.2,-0.1≤b2≤0.1, 0≤w2≤0.1, M1 includes at least one element selected from Zr, Al, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K. M2 includes at least one element of Zr, B, Mg, Ti, W, Mo, Nb, Ta, Sr, Sb, and K.
14. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to any one of claims 1 to 13.