One-dimensional SnSe screw dislocation nanowire and its preparation method and application

By using the preparation method of one-dimensional SnSe helical dislocation nanowires in tin selenide, the problem of low structural pollution and success rate of tin selenide is solved, and the controllable growth and excellent performance of one-dimensional SnSe helical dislocation nanowires are achieved. , suitable for the field of thermoelectric materials.

CN118343684BActive Publication Date: 2024-11-01CHINA UNIV OF MINING & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410561684.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-08
Publication Date
2024-11-01
Estimated Expiration
2044-05-08

AI Technical Summary

Technical Problem

In the prior art, the structure of tin selenide is mainly based on two-dimensional transfer mechanical stacking, with problems of structural pollution, sample damage and low success rates, which limits the research on the rotational structure stacking of layered van der Waals materials.

Method used

A method of preparing one-dimensional SnSe spiral dislocation nanowires is adopted. By using Au nanoparticles as catalyst in a tube furnace, the concentration and airflow conditions of the precursor SnSe powder are adjusted to achieve the growth of one-dimensional SnSe spiral dislocation nanowires , avoid secondary mechanical stacking interference, and use Burton-Cabrera-Frank theory to promote crystal growth.

Benefits of technology

Achieve controllable growth of one-dimensional SnSe spiral dislocation nanowires, with superior electrical, optical properties and thermal properties. They are suitable for infrared photoelectric instruments, memory switching switches and thermoelectric cooling materials. They have simple process, easy operation and environmental protection etc.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118343684B_ABST
    Figure CN118343684B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of semiconductor phase change storage materials, and specifically relates to a one-dimensional SnSe screw dislocation nanowire and its preparation method and application. The preparation method adopts the following steps: placing SnSe powder in the central area of ​​a tube furnace, placing a substrate material at the downstream low-temperature end, adjusting c / c0 to 1.2-1.4, using Au nanoparticles as a catalyst, and performing a heating reaction to obtain the one-dimensional SnSe screw dislocation nanowire. The present invention realizes the controllable growth of the morphology, structure, size and angle of one-dimensional van der Waals SnSe screw dislocation nanowires by chemical vapor deposition; the preparation method has the advantages of simple process, easy control of operation, relatively cheap reagents used and green environmental protection; the SnSe screw dislocation nanowire has superior electrical and optical properties, and also has the characteristics of excellent thermal performance, environmental friendliness, stable chemical properties and low cost, and has great application value in the fields of infrared optoelectronic instruments, memory switching switches and thermoelectric cooling materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of semiconductor phase change storage materials, and in particular relates to a one-dimensional SnSe screw dislocation nanowire and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background section is intended to enhance understanding of the overall background of the invention and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Crystal electronic structure and related phenomena (such as superconductivity and insulation) are determined by the superlattice potential generated in the atomic lattice and interlayer moiré fringes. Since the report of the dramatic transition from superconductivity to insulator in double-layer graphene stacking at different angles ("magic angle" graphene), van der Waals heterostructures with angled stacking between adjacent layers (interlayer distortion) have attracted great interest from researchers. The rich tunability of the electronic band structure brought about by the variable angle stacking of layered materials, and the resulting novel physical properties, have quickly become a research hotspot in condensed matter physics and materials science.

[0004] Tin selenide (SnSe) is an important IV-VI semiconductor and a typical layered metal chalcogenide (LMCs). It has excellent electrical and optical properties, excellent thermal properties, abundant earth resources, environmental friendliness, stable chemical properties and low cost. It has great application value in infrared optoelectronic instruments, memory switches and thermoelectric cooling materials. At present, the structure of tin selenide is mainly based on the mechanical stacking method of two-dimensional transfer, which usually requires polymers as auxiliary materials. It may be accompanied by structural contamination, sample damage and low success rate, which restricts the research on the corner structure stacking of layered van der Waals materials. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing one-dimensional SnSe screw dislocation nanowires; the preparation method has the advantages of simple method, easy operation and control, relatively cheap reagents used and green environmental protection.

[0006] The second object of the present invention is to provide a one-dimensional SnSe screw dislocation nanowire prepared by the above method.

[0007] The third object of the present invention is to provide applications of the one-dimensional SnSe screw dislocation nanowires.

[0008] To achieve the above object, the present invention adopts the following technical solution:

[0009] A method for preparing one-dimensional SnSe screw dislocation nanowires, the preparation method comprising the following steps:

[0010] The precursor SnSe powder is placed in the central area of ​​the tube furnace, the base material is placed at the downstream low-temperature end, the catalyst is spin-coated on the bottom of the base material, the catalyst is Au nanoparticles, and a heating reaction is performed. The c / c0 is adjusted to 1.2-1.4 to obtain the one-dimensional SnSe screw dislocation nanowire; wherein c is the concentration of the precursor SnSe powder and c0 is the equilibrium concentration.

[0011] Furthermore, the substrate material is a single-sided polished Si wafer having a SiO2 layer with a thickness of 300 nm.

[0012] Furthermore, the size of the base material is 1 cm*1 cm.

[0013] Furthermore, the diameter of the Au nanoparticles is 25-50 nm.

[0014] Furthermore, the gas flow source for the heating reaction is a mixture of Ar and H2.

[0015] Furthermore, the mixed gas of Ar and H2 contains H2 with a volume fraction of 10%.

[0016] Furthermore, the gas flow rate of the gas flow source is set to 100 sccm.

[0017] Furthermore, the gas pressure of the heating reaction is -0.09 Mpa.

[0018] Furthermore, the heating reaction temperature is 800°C, the time is 2 h, and the heating rate is 10°C / min.

[0019] One-dimensional SnSe screw dislocation nanowires prepared by the above method.

[0020] Application of the one-dimensional SnSe screw dislocation nanowires: The one-dimensional SnSe screw dislocation nanowires can be used in the field of thermoelectric materials.

[0021] Application of the above one-dimensional SnSe screw dislocation nanowires: the one-dimensional SnSe screw dislocation nanowires can be used in the field of thermoelectric conversion of micro devices.

[0022] Application of the above one-dimensional SnSe screw dislocation nanowires: the one-dimensional SnSe screw dislocation nanowires can be used in the field of chip heat dissipation.

[0023] The supersaturation (σ) of the system is the driving force for crystal growth: σ=ln(c / c0), where c is the precursor concentration and c0 is the equilibrium concentration. During the growth process of the precursor maintaining a low supersaturation concentration, the screw dislocation line intersects with the crystal surface to produce a step edge, and atoms are continuously injected into the step edge. There is no need to overcome the energy barrier to form a new crystal step. Therefore, under low supersaturation conditions, screw dislocation defects can promote crystal growth, thereby obtaining a one-dimensional screw dislocation nanowire. This model is called the Burton-Cabrera-Frank (BCF) theory. Compared with the traditional two-dimensional van der Waals structure, the difference of this one-dimensional twisted van der Waals structure is that: 1) the chiral nanowires spontaneously produce interlayer moiré fringes through the Eshelby twist associated with the axial screw dislocation, avoiding secondary mechanical stacking interference; 2) by adjusting the size of the catalyst in the chemical vapor deposition growth, the diameter of the nanowire can be changed, thereby regulating the axial rotation and twist angle, bringing rich adjustability; 3) the moiré fringes change systematically along the spiral path, and the material has strong uniformity, which is conducive to subsequent physical property analysis and regulation.

[0024] In this system, c / c0 is controlled between 1.2-1.4.

[0025] Starting from the dislocation-driven growth mechanism, the present invention designs a fine reactor device based on a multi-temperature zone high vacuum CVD growth platform. By selecting gold (Au) nanoparticles of different sizes (diameter 20-50 nm) as catalysts and placing 300 nm covered Si / SiO2 as substrate in a low-temperature deposition zone, appropriate supersaturated growth conditions with low precursor concentration / vapor pressure are created to grow SnSe spiral dislocation nanowires.

[0026] Beneficial effects: (1) The present invention realizes the controllable growth of the size of the screw dislocation nanowire structure by controlling the factors such as the temperature, pressure and air flow velocity of the furnace and the settling zone; realizes the controllable growth of the morphology by controlling the supersaturation degree of the raw materials; realizes the controllable growth of the nanostructure size and rotation angle by selecting the size of the catalyst Au nanoparticles; and finally realizes the preparation of one-dimensional van der Waals SnSe monomer nanostructures of different sizes and interlayer stacking angles.

[0027] (2) The present invention adopts a direct and controllable chemical vapor deposition (CVD) growth method, which has the characteristics of no external pollution and is simple and easy to operate. In addition, the preparation method of the present invention also has the advantages of simple process, easy operation control, relatively cheap reagents used, and green environmental protection.

[0028] (3) The SnSe screw dislocation nanowires prepared by the present invention have excellent electrical and optical properties, as well as excellent thermal properties, environmental friendliness, stable chemical properties and low cost. They have great application value in the fields of infrared optoelectronic instruments, memory switching switches and thermoelectric cooling materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein:

[0030] Figure 1 This is a structural diagram of the SnSe screw dislocation nanowire prepared in Example 1;

[0031] Figure 2 This is a structural diagram of the SnSe screw dislocation nanowire prepared in Example 2;

[0032] Figure 3 A simplified device diagram for the growth process of SnSe screw dislocation nanowires;

[0033] Figure 4 This is the SEM image of SnSe nanowires prepared in Comparative Example 1;

[0034] Figure 5 is the SEM image of SnSe particles prepared in Comparative Example 2;

[0035] Figure 6 This is the SEM image of the SnSe block prepared in Comparative Example 3;

[0036] Figure 7 TEM-EDS image of SnSe screw dislocation nanowires prepared in Example 1;

[0037] Figure 8 TEM 4D-STEM pattern image of SnSe screw dislocation nanowires prepared in Example 1;

[0038] Fig. 9 The thermal conductivity test schematic diagram and statistical diagram of the screw dislocation nanowire prepared in Example 1 are shown in FIG. Fig. 9 a is a schematic diagram of thermal conductivity test. Fig. 9 b is the thermal conductivity statistics diagram. Specific embodiments

[0040] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0041] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions.

[0042] In addition, any method and material similar or equivalent to the content described herein can be applied to the method of the present invention. The preferred implementation methods and materials described in the present invention are for demonstration purposes only. The present invention is further described based on the accompanying drawings and specific embodiments of the present invention.

[0043] Example 1

[0044] 20 mg of SnSe powder was placed in the center area of ​​the tube furnace, and the substrate material was placed at the downstream low-temperature end. The substrate material was a single-sided polished Si wafer substrate with a SiO2 layer of 300 nm thickness and a size of 1 cm*1 cm. Au nanoparticles with a diameter of about 25 nm were selected as catalysts and were evenly spin-coated on the Si wafer substrate at a speed of 1000 r / min. A mixture of Ar and H2 containing 10% H2 was used as the gas flow source. The gas flow rate was set to 100 sccm, and the gas pressure in the tube was maintained at -0.09 MPa. The center temperature of the tube furnace was set to 800℃, the heating rate was 10℃ / min, and it was maintained for 2 h. The c / c0 ratio was adjusted between 1.2-1.4, and then the heating system was turned off and the temperature was naturally cooled to obtain one-dimensional SnSe screw dislocation nanowires.

[0045] Figure 1 This is a picture of the SnSe screw dislocation nanowire prepared in Example 1. The results show that when the diameter of the Au catalyst is between 20nm and 30nm, the c / c0 ratio is adjusted between 1.2-1.4, and the SnSe screw dislocation nanowire can be grown in a spiral upward angle.

[0046] Example 2

[0047] 20 mg of SnSe powder was placed in the center area of ​​the tube furnace, and the substrate material was placed at the downstream low-temperature end. The substrate material was a single-sided polished Si wafer substrate with a SiO2 layer of 300 nm thickness and a size of 1 cm*1 cm. Au nanoparticles with a diameter of about 50 nm were selected as catalysts and were evenly spin-coated on the Si wafer substrate at a speed of 1000 r / min. A mixture of Ar and H2 containing 10% H2 was used as the gas flow source. The gas flow rate was set to 100 sccm, and the gas pressure in the tube was maintained at -0.09 MPa. The center temperature of the tube furnace was set to 800℃, the heating rate was 10℃ / min, and it was maintained for 2 h. The c / c0 ratio was adjusted between 1.2-1.4, and then the heating system was turned off and the temperature was naturally cooled to obtain one-dimensional SnSe screw dislocation nanowires.

[0048] Figure 2 This is a picture of the SnSe screw dislocation nanowire prepared in Example 2. The results show that when the diameter of the Au catalyst is between 50nm and 60nm, by adjusting the c / c0 ratio between 1.2-1.4, a SnSe screw dislocation nanowire with a spiral upward morphology can be grown, with a dislocation line in the center.

[0049] Example 3

[0050] 20 mg of SnSe powder was placed in the center area of ​​the tube furnace, and the substrate material was placed at the downstream low-temperature end. The substrate material was a single-sided polished Si wafer substrate with a SiO2 layer of 300 nm thickness and a size of 1 cm*1 cm. Au nanoparticles with a diameter of about 50 nm were selected as catalysts and were evenly spin-coated on the Si wafer substrate at a speed of 1000 r / min. A mixture of Ar and H2 containing 10% H2 was used as the gas flow source. The gas flow rate was set to 100 sccm, and the gas pressure in the tube was maintained at -0.09 MPa. The center temperature of the tube furnace was set to 800℃, the heating rate was 10℃ / min, and it was maintained for 2 h. The c / c0 ratio was adjusted between 1.2-1.4, and then the heating system was turned off and the temperature was naturally cooled to obtain one-dimensional SnSe screw dislocation nanowires.

[0051] Figure 3 A simplified diagram of the SnSe screw dislocation nanowire growth process.

[0052] Comparative Example 1

[0053] 20 mg of SnSe powder was placed in the central area of ​​the tube furnace, and the substrate material was placed at the downstream low-temperature end. The substrate material was a single-sided polished Si wafer substrate with a SiO2 layer of 300 nm thickness and a size of 1 cm*1 cm. Au nanoparticles with a diameter of about 50 nm were selected as catalysts and were evenly spin-coated on the Si wafer substrate at a speed of 1000 r / min. A mixture of Ar and H2 containing 10% H2 was used as the gas flow source. The gas flow rate was set to 10 sccm, and the gas pressure in the tube was maintained at -0.09 MPa. The center temperature of the tube furnace was set to 900℃, the heating rate was 10℃ / min, and it was maintained for 2 h, so that the c / c0 was between 1.5-2.0, and then the heating system was turned off and the temperature was naturally cooled to obtain messy one-dimensional SnSe nanowires, but no screw dislocation nanowires were obtained.

[0054] Figure 4 This is a SEM image of the SnSe nanowires prepared in Comparative Example 1. The results show that the one-dimensional SnSe nanowires prepared in Comparative Example 1 are in a disordered state, and no screw dislocations are observed.

[0055] Comparative Example 2

[0056] 20 mg of SnSe powder was placed in the center area of ​​the tube furnace, and the substrate material was placed at the downstream low-temperature end. The substrate material was a single-sided polished Si wafer substrate with a SiO2 layer of 300 nm thickness and a size of 1cm*1cm. Au nanoparticles with a diameter of about 50 nm were selected as catalysts and were evenly spin-coated on the Si wafer substrate at a speed of 1000 r / min. A mixture of Ar and H2 containing 10% H2 was used as the gas flow source. The gas flow rate was set to 10 sccm, and the gas pressure in the tube was maintained at -0.09 MPa. The center temperature of the tube furnace was set to 600℃, the heating rate was 10℃ / min, and it was maintained for 2 h to make c / c0<1, and then the heating system was turned off and the temperature was naturally cooled to obtain messy SnSe particles, but no screw dislocation nanowires were obtained.

[0057] Figure 5 This is a SEM image of the SnSe particles prepared in Comparative Example 2. The results show that the SnSe particles are in a disordered state and no screw dislocation is observed.

[0058] Comparative Example 3

[0059] 20 mg SnSe powder was placed in the center of the tube furnace, and the substrate material was placed at the downstream low-temperature end. The substrate material was a single-sided polished Si wafer substrate with a SiO2 layer of 300 nm thickness and a size of 1 cm*1 cm. Au nanoparticles with a diameter of about 50 nm were selected as catalysts and were evenly spin-coated on the Si wafer substrate at a speed of 1000 r / min. A mixture of Ar and H2 containing 10% H2 was used as the gas flow source. The gas flow rate was set to 10 sccm, and the gas pressure in the tube was maintained at -0.08 MPa. The center temperature of the tube furnace was set to 800℃, and the heating rate was 10℃ / min. The temperature was maintained for 2 h, so that c / c0<1, and then the heating system was turned off and the temperature was naturally lowered to obtain the following: Figure 6 The block shown does not produce screw dislocation nanowires.

[0060] Figure 6 This is the SEM image of the SnSe block prepared in Comparative Example 3, and no screw dislocation nanowires were obtained.

[0061] Performance Testing

[0062] 1. Figure 7 This is a transmission electron microscope energy dispersive spectroscopic analysis (TEM-EDS) image of the SnSe screw dislocation nanowire prepared in Example 1. Through TEM EDS, it can be determined that the nanowire is a SnSe nanowire. Figure 1 , it can be determined that the screw dislocation rotation angle is 31°.

[0063] 2. Figure 8 This is a four-dimensional scanning transmission electron microscopy (TEM4D-STEM) pattern of the SnSe screw dislocation nanowire prepared in Example 1. Combined with the TEM 4D STEM pattern, it is determined that the lattice distribution of different regions of the SnSe nanowire with a screw dislocation line at the center is different.

[0064] 3. The SnSe screw dislocation nanowires and the existing one-dimensional nanowires prepared in Example 1 were transferred to the test system using a needle transfer platform. -4 mba) to conduct thermal conductivity test, the results are as follows Fig. 9 As shown, the black dots are the thermal conductivity of the screw dislocation nanowires prepared in Example 1, and the green dots are the thermal conductivity of the existing one-dimensional SnSe nanomaterials. By comparison, it is found that the thermal conductivity is reduced by more than 80%. Since the energy conversion efficiency of thermoelectric materials is evaluated by the "thermoelectric figure of merit" - ZT, its physical formula is: ZT = S 2 σT / κ, where α: Seebeck coefficient (μV·K -1 ), T: temperature (K), σ: electrical conductivity (S·cm -1 ), κ: thermal conductivity (W·m -1 ·K-1 ), so reducing the thermal conductivity of materials plays an important role in improving thermoelectric performance.

[0065] The present invention uses molecular dynamics, classical crystal growth theory and other means to construct different supersaturations (σ): σ=ln(c / c0), and analyzes and determines that when c / c0 is in the range of 1.2 to 1.4, SnSe screw dislocation nanowires can be grown.

[0066] And based on the above-mentioned excellent thermoelectric properties of SnSe, the SnSe screw dislocation one-dimensional van der Waals nanostructure has rich electron energy band tunability and phonon scattering enhancement sites, which can achieve electric-acoustic decoupling and then synergistically optimize the thermoelectric properties of the material, and can be applied to the field of thermoelectric materials, such as thermoelectric conversion of micro-devices and chip heat dissipation.

[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing one-dimensional SnSe screw dislocation nanowires, characterized in that: The preparation method adopts the following steps: The precursor SnSe powder is placed in the central area of ​​the tube furnace, the base material is placed at the downstream low-temperature end, Au nanoparticles are spin-coated on the bottom of the base material, and a heating reaction is performed, and c / c0 is adjusted to 1.2-1.4 to obtain the one-dimensional SnSe screw dislocation nanowire; Where c is the concentration of precursor SnSe powder, c0 is the equilibrium concentration; The gas pressure of the heating reaction is -0.09 Mpa, the gas flow rate is 100 sccm; the temperature of the heating reaction is 800°C, the time is 2 h, and the heating rate is 10°C / min.

2. The preparation method according to claim 1, characterized in that: The diameter of the Au nanoparticles is 25-50 nm.

3. The preparation method according to claim 1, characterized in that: The substrate material is a single-sided polished Si wafer with a SiO2 layer with a thickness of 300 nm.

4. The preparation method according to claim 3, characterized in that: The size of the base material is 1 cm*1 cm.

5. The preparation method according to claim 1, characterized in that: The gas flow source for the heating reaction is a mixture of Ar and H2.

6. The preparation method according to claim 5, characterized in that: The mixed gas of Ar and H2 contains H2 with a volume fraction of 10%.

7. One-dimensional SnSe screw dislocation nanowire prepared by the method according to any one of claims 1 to 6.

8. Use of the one-dimensional SnSe screw dislocation nanowire prepared by the method according to any one of claims 1 to 6 and / or use of the one-dimensional SnSe screw dislocation nanowire according to claim 7, characterized in that: The one-dimensional SnSe screw dislocation nanowire is used in the field of thermoelectric materials.

Citation Information

Patent Citations

  • Method for preparing coiled carbon nano material under nickel nano catalytic actions

    CN104386668A

  • Novel spiral GaN monocrystal nanowire and preparation method thereof

    CN105040096A

  • Growth method of tellurium nanowire vertical array

    CN114032510A

  • Method for producing inorganic fine particle powder, organic-inorganic composite material and optical element

    JP2009013009A

  • Methods for the synthesis of arrays of thin crystal grains of layered semiconductors SNS 2 and SNS at designed locations

    WO2014182697A1